Computer-aided design method for synthesis process of Al-added copper-nickel alloy

By establishing a thermodynamic database and phase diagram of the Cu-Ni-Al system, we calculated and verified the phase fraction changes under the added amount of Al, optimized the casting process, solved the problem of unstable copper-nickel alloy properties, and improved the mechanical properties and performance of copper-nickel alloys. Production efficiency.

CN118737336AInactive Publication Date: 2024-10-01GUILIN UNIV OF ELECTRONIC TECH +2

Patent Information

Application Number
CN202410898114.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When adding Al element to traditional copper-nickel alloys, there is a lack of accurate and quantitative design methods, resulting in unstable performance, long development cycles, high costs, and casting defects affecting mechanical properties. The existing literature mainly relies on guesswork and experiments, which is inefficient.

Method used

A computer-aided design method was used to establish a thermodynamic database for the Cu-Ni-Al system. The phase fraction changes under different Al addition amounts were calculated through the equilibrium relationship phase diagram and Thermo-calc software. Combined with experimental verification, the Cu and Al contents in the alloy were determined. Optimize the casting process to reduce casting defects.

Benefits of technology

It has achieved a stable improvement in the mechanical properties of copper-nickel alloys, especially the tensile strength and yield strength, reduced the research and development cycle and cost, and improved the efficiency of process design and the overall performance of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737336A_ABST
    Figure CN118737336A_ABST
Patent Text Reader

Abstract

The invention discloses a computer-aided design method for a synthesis process of Al-added copper-nickel alloy. The method comprises the following steps: S1, establishing a thermodynamic database of a Cu-Ni-Al system; s2, an equilibrium relation phase diagram is obtained, and the content of Cu and the content of Al in the alloy are determined; s3, calculating the phase fraction change conditions of different phases of the alloy under different Al addition amounts; verifying the content of each element in the alloy; s4, performing experimental verification; and S5, guiding alloy production according to the content of each element in the alloy and the smelting process after experimental verification. According to the method, an Al element interval can be accurately and quantitatively determined by combining a thermodynamic database and a phase diagram of a Cu-Ni-Al system, the performance improvement performance is determined firstly, then the phase fraction change conditions of different phases of the alloy under different Al addition amounts are calculated, a stable interval is obtained, it is determined that precipitation of the ordered phase is effective, and then experimental verification shows that the precipitation of the ordered phase is effective. Finally, a stable improvement scheme is obtained, waste is reduced, and cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of computer-aided design, and in particular relates to a computer-aided design method for a synthesis process of a copper-nickel alloy with Al added. Background Art

[0002] High-strength and high-conductivity copper alloys are a high-tech field that my country focuses on developing. The national grade B10 type Cu-Ni alloy has the characteristics of high elasticity and high conductivity and is widely used in offshore operating environments. However, its overall hardness and strength are insufficient, and a single Cu-Ni alloy cannot cope with complex and changing environmental requirements. The solid solubility of Al in copper is very large, reaching 9.4wt%, forming a continuous solid solution with copper, with a wide single-phase region, which can significantly improve the mechanical properties of copper to adapt to increasingly changing environmental requirements.

[0003] Traditional copper-nickel alloys consider adding Be to improve their mechanical properties, but because Be is highly toxic and expensive, Al, which is relatively cheap and non-toxic, is selected as an additive element to form a continuous solid solution with copper, with a wide single-phase region to improve the mechanical properties of copper alloys. At present, the traditional design method cannot accurately quantify the amount of Al added. Past experience has been based on the ratio obtained by doping and random addition, and its performance is unstable. At the same time, in industrial production, the prices of copper and nickel are relatively high, and unstable performance will cause a lot of waste. The current public literature is mainly based on speculation on the amount of aluminum added, and then added. After the finished product comes out, performance testing and judgment are carried out. This process requires a lot of trial and error and testing, and its cost is relatively high.

[0004] At the same time, since the melting points of copper and nickel are relatively high, while the melting point of aluminum is relatively low, it is not easy to melt Al added to Cu-Ni alloys. Casting defects during the melting process will significantly affect the performance of the final product, resulting in the development method of using Al to improve Cu-Ni alloys, which has the problems of low efficiency, high cost, and low accuracy. Therefore, there are currently few research papers on Al addition to improve Cu-Ni alloys. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for computer-aided design of a synthesis process of a copper-nickel alloy with added Al, which can effectively and quickly determine the proportion of the copper-nickel alloy with added Al, reduce the research and development cycle and cost, and improve the mechanical properties of the copper-nickel alloy with added Al.

[0006] The technical solution adopted by the present invention to solve the technical problem is a method for computer-aided design of a synthesis process of a copper-nickel alloy with Al added, comprising the following steps:

[0007] Step S1, establishing a thermodynamic database for the Cu-Ni-Al system;

[0008] Step S2, after the database is established, the equilibrium relationship under a certain nickel content is described, the equilibrium relationship phase diagram under a certain nickel content is obtained, the composition design is performed according to the requirements of the two ordered phases existing in the alloy, and the content of Cu and Al in the alloy is determined;

[0009] Step S3, using the Cu-Ni-Al system thermodynamic database established in step S1 and the alloy equilibrium relationship phase diagram constructed in step S2, calculate the phase fraction changes of different phases of the alloy under different Al addition amounts; and verify the content of each element in the alloy;

[0010] Step S4, experimental verification: according to the content of each element in the alloy obtained in step S3, the alloy is melted and cast, and the performance of the cast alloy is tested and analyzed, and the obtained results are verified by experiments;

[0011] Step S5, alloy production: alloy production is guided by the content of each element in the alloy and the smelting process verified by experiments.

[0012] Furthermore, in step S1, the phase equilibrium relationship of each component of Cu-Ni-Al is evaluated based on historical Cu-Ni-Al phase equilibrium experiments, and a thermodynamic database of the Cu-Ni-Al system is established using the Calphad method.

[0013] Furthermore, in step S2, the nickel content is 9-11 wt %. Furthermore, the nickel content is 10 wt %.

[0014] Further, in step S2, the addition amounts of Cu and Al in the alloy are determined to be (85-88) wt% and (2-5) wt% of the total mass of the alloy, respectively.

[0015] Further, in step S3, the important ordered phases of the alloy are Ni3Al and β-NiAl phases.

[0016] Further, in step S3, the Cu-Ni-Al system thermodynamic database established in step S1 and the alloy equilibrium relationship phase diagram constructed in step S2 are used to establish a Cu-0.1Ni-ωAl (0<ω<10%) alloy solidification phase diagram, and Thermo-calc software is used to calculate the change in the content of the ordered phase generated during the alloy solidification process under different Al addition amounts, and the content of each element in the alloy is verified.

[0017] Further, in step S4, the alloy is melted in an induction melting furnace and poured into a graphite mold. Furthermore, the current change during the melting process of the induction melting furnace is controlled, the temperature is raised to 1180-1220°C (preferably 1200°C), the current is 320A as the peak value, and after melting for 2-3 minutes, it is quickly cooled down to 270-280A (preferably 275A) (preferably cooled down to 275A within 1 minute), and then poured into the mold. By controlling these parameters, the occurrence of casting defects in the melting process can be reduced.

[0018] Furthermore, in step S4, when determining the added weight of each element, each element is added 5% to 10% more based on the weight of each element obtained in step S3. Studies have shown that adding more of each element, combined with the control of the smelting process of the induction melting furnace, can reduce the occurrence of casting defects. It will not cause unnecessary waste, nor will casting defects cause the entire product to be scrapped.

[0019] The present invention combines the thermodynamic database and phase diagram of the Cu-Ni-Al system to accurately and quantitatively determine the Al element interval, first determine the performance improvement, then calculate the phase fraction changes of different phases of the alloy under different Al addition amounts to obtain a stable interval, determine that the precipitation of the ordered phase is indeed effective, and then verify it through experiments, and finally obtain a stable improvement plan, which reduces waste and saves costs.

[0020] The copper-nickel alloy with Al added determined by the present invention can improve the mechanical properties of the copper-nickel alloy, especially the existing B10 alloy grade, which are mainly manifested in tensile strength, yield strength, and elastic modulus. The present invention assists the optimization design of the ordered phase through computational simulation, accurately quantifies the Al addition range, and ensures stable performance.

[0021] Research shows that in step S4, when the sample is actually weighed, 5wt% to 10wt% of each element is added, and the current change during the smelting process in the induction melting furnace is controlled. The temperature is raised to 1200°C, and the current is 320A as the peak value. After smelting for 2-3 minutes, it is quickly cooled and reduced to 275A before pouring into the mold to reduce the occurrence of casting defects.

[0022] The computer-aided design method for the synthesis process of copper-nickel alloy with Al added provided by the present invention establishes a thermodynamic database of the Cu-Ni-Al system, calculates the equilibrium phase relationship of the Cu-Ni-Al system under a certain nickel content, simulates the relationship between the phase fraction of different phases of the Cu-Ni-Al alloy and the amount of Al added during the casting process, and quickly obtains the optimal addition range of Al in the Cu-Ni alloy. This can not only effectively meet the requirements of product performance and structure, but also greatly improve the mechanical properties of the alloy, and optimize the comprehensive performance of existing copper-nickel alloys, especially B10 alloy products. The method can effectively and quickly determine the proportion of copper-nickel alloys with Al added, reduce the research and development cycle and cost, and improve the mechanical properties of copper-nickel alloys with Al added. It can meet the requirements of alloy performance and structure, greatly reduce the research and development cycle and cost of alloy process design, improve work efficiency, and has important guiding value for the design and production of new high-performance alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 It is a schematic diagram of the vertical cross-section thermodynamic calculation verification results of the equilibrium relationship under 10wt% nickel content in the present invention (mass fraction, %);

[0025] Figure 2 Schematic diagram of the change of the phase fraction of the ordered phase of the Cu-Ni alloy under different Al addition amounts in the present invention (there are many, only one of them is shown here);

[0026] Figure 3 Schematic diagram of tensile strength mechanical properties of Cu-Ni alloy with different Al addition amounts in the embodiment of the present invention;

[0027] Figure 4 Schematic diagram of yield strength mechanical properties of Cu-Ni alloy with different Al addition amounts in the embodiment of the present invention;

[0028] Figure 5 Schematic diagram of the elongation mechanical properties of Cu-Ni alloy at different Al addition amounts in an embodiment of the present invention. DETAILED DESCRIPTION

[0029] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments and drawings. The contents mentioned in the implementation modes are not intended to limit the present invention.

[0030] Example

[0031] The computer-aided design method for the synthesis process of the copper-nickel alloy with Al added in this embodiment includes the following steps:

[0032] Step S1, establishing a thermodynamic database for the Cu-Ni-Al system:

[0033] A literature survey was conducted on the Cu-Ni-Al system, historical phase equilibrium experiments of the Cu-Ni-Al system were collected, the phase equilibrium relationship of each component of the Cu-Ni-Al system was evaluated, and the thermodynamic database of the Cu-Ni-Al system was established using Calphad. The full name of the Calphad method is the computational thermodynamic phase diagram method (CALculation of PHAse Diagrams), which is a calculation method based on the principle of thermodynamic equilibrium. It can predict the phase change behavior of materials under different temperatures, pressures and compositions. The Cu-Ni-Al system is a ternary system, which has four binary systems and one ternary system. In order to ensure the compatibility and rationality of the thermodynamic parameters and thermodynamic models of the ternary system, it is necessary to investigate the Cu-Ni-Al phase equilibrium experiments and thermodynamic descriptions of previous researchers.

[0034] Step S2, composition design: calculate the equilibrium phase relationship of Cu-Ni-Al alloy under 10wt% Ni, and calculate the phase diagram as follows Figure 1 As shown, the addition amount of Cu and Al in the alloy is determined. The addition amount of Cu and Al in the alloy is determined to be (85-88) wt% and (2-5) wt% of the total mass of the alloy, respectively.

[0035] For Al-added Cu-Ni alloys, different amounts of Cu and Al added will form different ordered phases, and there is a qualitative relationship between the process-composition-structure-performance of the alloy. The present invention intends to start from the source of the alloy and consider obtaining the best mechanical properties of the cast lightweight alloy by changing the alloy composition, so as to provide a basis for the subsequent staged control (such as different heat treatment processes, different solidification fine grain technologies, additive manufacturing, powder metallurgy and other processes) to positively affect the alloy performance.

[0036] Step S3, thermodynamic design: calculating the change in the phase fraction of the ordered phase of the alloy under different Al addition amounts.

[0037] The Cu-Ni-Al system thermodynamic database established in step S1 and the alloy equilibrium relationship phase diagram constructed in step S2 are used to establish the Cu-0.1Ni-ωAl (0<ω<10%) alloy solidification phase diagram. Thermo-calc software is used to calculate the content change of the ordered phase generated during the alloy solidification process under different Al addition amounts, and the content of each element in the alloy is verified; the calculation results are as follows: Figure 2As shown, the important ordered phases of the alloy are Ni3Al and β-NiAl phases.

[0038] Step S4, experimental verification: according to the content of each element in the alloy obtained in step S3, the alloy is melted and cast, and the performance of the cast alloy is tested and analyzed, and the obtained results are verified by experiments;

[0039] The alloy is melted in an induction melting furnace and poured into a graphite mold. The current change during the melting process of the induction melting furnace is controlled, the temperature is raised to 1200°C, the current is 320A as the peak value, and after melting for 2-3 minutes, it is quickly cooled down to 275A and poured into the mold. By controlling these parameters, the occurrence of casting defects in the melting process can be reduced.

[0040] When determining the added weight of each element, on the basis of the weight of each element obtained in step S3, each element is added 5% to 10% more. Studies have shown that adding more of each element, combined with the control of the smelting process of the induction melting furnace, can reduce the occurrence of casting defects. It will not cause unnecessary waste, nor will casting defects cause the entire product to be scrapped.

[0041] In order to verify the reliability and accuracy of the present invention, the composition and mechanical properties of Cu-Ni alloys with different Al addition amounts were tested and analyzed in this embodiment.

[0042] The experimental composition points of the alloy are shown in Table 1:

[0043] Table 1 Experimental verification of Cu-Ni-Al alloy composition (mass fraction, wt%)

[0044] Serial number Alloy composition 1 Cu-10Ni 2 Cu-10Ni-2Al 3 Cu-10Ni-3Al 4 Cu-10Ni-4Al 5 Cu-10Ni-5Al

[0045] In Table 1, Cu-10Ni represents a copper-nickel alloy having a nickel content of 10% by mass, and Cu-10Ni-2Al represents a copper-nickel alloy having a nickel content of 10% by mass and an aluminum content of 2% by mass.

[0046] The Cu-Ni alloys with different Al addition amounts in Table 1 were melted in an induction melting furnace and cast into a graphite mold. The tensile properties and other mechanical properties of the resulting cast alloys were tested. The results are shown in Table 1. Figure 3-5 Performance testing equipment: universal tensile testing machine (produced by Shanghai Lishi Scientific Instrument Co., Ltd.), testing method standard: GB / T 5234-1985.

[0047] from Figure 3 , Figure 4 , Figure 5It can be seen that with the increase of Al content, the mechanical properties of the cast Cu-Ni-Al alloy are greatly improved, and the specific addition range is mainly concentrated in (2-5)% Al (mass fraction, %) when the mechanical properties reach the optimal level.

[0048] Therefore, the optimal addition amount of Al obtained by experimental verification is consistent with the result predicted by computer. The changes in the phase fractions of different phases of the alloy under different Al addition amounts calculated by S4 verify that the optimal addition amount of Al in Cu-Ni alloy is in the range of (2-5) (wt%).

[0049] Step S5, alloy production: alloy production is guided by the content of each element in the alloy and the smelting process verified by experiments.

[0050] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present technical solution is within the protection scope of the present invention.

[0051] In order to make it easier for ordinary technicians in the field to understand the improvements of the present invention over the prior art, some drawings and descriptions of the present invention have been simplified, and for the sake of clarity, some other elements are omitted in this application document. Ordinary technicians in the field should realize that these omitted elements may also constitute the content of the present invention.

Claims

1. A method for computer-aided design of a copper-nickel alloy synthesis process with Al addition, characterized in that: The following steps are involved: Step S1, establishing a thermodynamic database for the Cu-Ni-Al system; Step S2, after the database is established, the equilibrium relationship under a certain nickel content is described, the equilibrium relationship phase diagram under a certain nickel content is obtained, the composition design is performed according to the requirements of the two ordered phases existing in the alloy, and the content of Cu and Al in the alloy is determined; Step S3, using the Cu-Ni-Al system thermodynamic database established in step S1 and the alloy equilibrium relationship phase diagram constructed in step S2, calculate the phase fraction changes of different phases of the alloy under different Al addition amounts; and verify the content of each element in the alloy; Step S4, experimental verification: according to the content of each element in the alloy obtained in step S3, the alloy is melted and cast, and the performance of the cast alloy is tested and analyzed, and the obtained results are verified by experiments; Step S5, alloy production: alloy production is guided by the content of each element in the alloy and the smelting process verified by experiments.

2. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al added according to claim 1, characterized in that: In step S1, the phase equilibrium relationship of each component of Cu-Ni-Al is evaluated based on historical Cu-Ni-Al phase equilibrium experiments, and a thermodynamic database of the Cu-Ni-Al system is established using the Calphad method.

3. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al addition according to claim 1 or 2, characterized in that: In step S2, the nickel content is 9-11 wt%.

4. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al added according to claim 3, characterized in that: The nickel content is 10 wt%.

5. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al addition according to claim 1 or 2, characterized in that: In step S2, the addition amounts of Cu and Al in the alloy are determined to be (85-88) wt% and (2-5) wt% of the total mass of the alloy, respectively.

6. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al added according to claim 1 or 2, characterized in that: In step S3, the important ordered phases of the alloy are Ni3Al and β-NiAl phases.

7. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al addition according to claim 1 or 2, characterized in that: In step S3, the Cu-Ni-Al system thermodynamic database established in step S1 and the alloy equilibrium relationship phase diagram constructed in step S2 are used to establish a Cu-0.1Ni-ωAl alloy solidification phase diagram, 0<ω<10%, and Thermo-calc software is used to calculate the change in the content of the ordered phase generated during the alloy solidification process under different Al addition amounts, and the content of each element in the alloy is verified.

8. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al addition according to claim 1 or 2, characterized in that: In step S4, the alloy is melted in an induction melting furnace and poured into a graphite mold.

9. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al added according to claim 8, characterized in that: Control the current change during the smelting process of the induction melting furnace, raise the temperature to 1180-1220℃, and set the current to 320A as the peak value. After smelting for 2-3 minutes, quickly cool it down to 270-280A and pour it into the mold.

10. The method for computer-aided design of a synthesis process of a copper-nickel alloy with Al addition according to claim 1 or 2, characterized in that: In step S4, when determining the added weight of each element, each element is added 5% to 10% more based on the weight of each element obtained in step S3.

Citation Information

Patent Citations

  • Method of designing and optimizing Al-Si-Cu-Mg system phase change heat storage alloy materials

    CN103136418A

  • Component optimization design method of 617 nickel-based superalloy

    CN111681716A

  • Computer-aided method for determining Al-Si-Y ternary alloy phase diagram

    CN115422618A

  • Computer-aided design method for Sc modified Al-Cu-Mg alloy

    CN117037970A

  • Computer-aided method for predicting castability of Al-Cu-Mg-Sc alloy

    CN117174210A

Cited By

  • Preparation process of high-performance Cu-Ni-Fe alloy calculated and designed based on first principle

    CN121674758A