Semiconductor preparation method and semiconductor device
By controlling the etching time and etching rate of HCD-SIN, combined with temperature sensitivity and position correlation, the problem of morphological differences in Spacer HCD-SIN is solved, achieving a more uniform film thickness and stable device structure, improving the electrical properties of the transistor.
Patent Information
- Application Number
- CN202410716198.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, there are differences in the morphology of Spacer HCD-SIN from the same batch, which affects the electrical properties of the transistors and the stability of the process structure. Especially after wet cleaning, the morphology of the device sidewalls changes vertically with the inside of the furnace tube. The position in the direction is related, resulting in uneven thickness.
By controlling the thickness uniformity of HCD-SIN at different positions in the vertical direction of the same furnace tube, a combination of dry etching and wet cleaning is used to set the etching time of HCD-SIN, taking into account its vertical position in the furnace tube. Position and temperature sensitivity in the direction, adjust the etch rate to reduce morphology differences. Specific steps include: controlling U% <0.4%, performing dry etching, limiting the etching time according to the thickness to be etched, position and etching rate during wet cleaning, and introducing a correlation curve between temperature sensitivity and etching rate to Optimize the etching process.
It effectively reduces the difference in morphology of HCD-SIN at different locations in the same furnace tube after wet cleaning, improves the uniformity and stability of the film thickness, ensures the structural stability of Spacer HCD-SIN as a spacer layer, and improves the electrical properties of the transistor.
Smart Images

Figure CN118737830A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a transistor device, and in particular to a method for preparing a semiconductor and a semiconductor device. Background Art
[0002] Using hexachlorodisilane (HCD) as raw material, through the following chemical reaction: 3Si2Cl6(g)+26NH3(g)→2Si3N4(s)+18NH4Cl(g)+3H2(g), the formed silicon nitride (SiN) can form HCD-SIN at a relatively low temperature of 580°C. This type of silicon nitride can be effectively used in the spacer layer, making silicon nitride widely used in the manufacture of transistors due to its excellent physical and chemical properties.
[0003] At present, the preparation process of Spacer HCD-SIN mainly includes the following steps (such as Figure 1 As shown in the figure): first, prepare an oxide spacer layer (Spacer ox layer); then, prepare a silicon nitride spacer layer (SpacerHCD-SIN layer); then, by etching the spacer layer (Spacer ET) dry etching, effectively etch the Spacer HCD-SINlayer on the horizontal surface of the device, and at the same time, combine with the wet etching of diluted hydrofluoric acid (DHF) to remove the HCD-SIN on the source and drain ends of the transistor device and the top of the poly (gate). After wet cleaning, hydrofluoric acid will etch the HCD-SIN on the side wall, which will cause the morphology of the HCD-SIN protective film layer on the side wall of the device to change, and form a SpacerHCD-SIN with a certain morphology on the side wall; finally, you can choose whether to strip the spacer layer as needed. The stripping of the spacer layer can be carried out by sequentially using diluted hydrofluoric acid (Dilute HydroFluoric acid, referred to as DHF), sulfur peroxide mixture (Sulfuric Peroxide Mixture, referred to as SPM, also known as sulfuric acid peroxide mixture, mainly used for cleaning organic matter) and a mixture of ammonium hydroxide and hydrogen peroxide (SC1) for cleaning.
[0004] However, with the further increase in the demand for the computing power and storage capacity of integrated circuits, the size of the transistor is required to be further reduced in terms of its gate length and film thickness, resulting in a significant change in the thermal distribution of the dopant of the device. In order to make the device have consistent and reliable electrical properties, the thermal budget used to manufacture the integrated circuit also needs to be further reduced, which is generally achieved by making the thin layer of the manufacturing device have good uniformity and stability. However, the Spacer HCD-SIN of the same batch prepared by the existing process has differences in morphology, which in turn affects the process structure formed by the process, further affects the subsequent ion implantation, and ultimately affects the electrical properties of the device. Therefore, it is urgent to find a preparation process that can greatly reduce the difference in morphology of the Spacer HCD-SIN of the same batch to achieve the improvement of the electrical properties of transistor devices. Summary of the invention
[0005] In order to solve the problem of differences in morphology of the same batch of Spacer HCD-SIN, the inventors have repeatedly studied the process of Spacer HCD-SIN and found that even if the morphology of HCD-SIN from the same furnace is not much different when it is just out of the furnace, after wet cleaning, the morphology of Spacer HCD-SIN from the same furnace will be greatly different; at the same time, the inventors also found that after wet cleaning, the morphology change of HCD-SIN from the same furnace is correlated with its position in the vertical direction of the furnace tube, which is specifically reflected in the following: after wet cleaning of HCD-SIN from the same furnace and the same thickness, the thickness of the Spacer HCD-SIN located at the top of the furnace is significantly greater than the thickness of the Spacer HCD-SIN located at the bottom of the furnace. Based on this, the inventors proposed a semiconductor preparation method, which includes the following steps:
[0006] S20: Control the thickness U% of HCD-SIN prepared at different positions in the vertical direction of the same tube furnace to be less than 0.4%;
[0007] S30: dry etching the HCD-SIN prepared in the furnace tube;
[0008] S40: wet-clean the HCD-SIN that has been dry-etched, and, during the wet-cleaning process, set the etching time of HCD-SIN to be limited by the thickness of HCD-SIN to be etched, the position of HCD-SIN in the vertical direction in the furnace tube when preparing HCD-SIN, and the etching rate of HCD-SIN at different positions in the vertical direction in the furnace tube (the etching rate of HCD-SIN at different positions in the vertical direction in the furnace tube means that the HCD-SIN prepared in the furnace tube has different etching rates at different positions in the vertical direction). Among them, U% = Sigma / Mean, U represents the uniformity of the film thickness; Sigma is a statistical parameter that characterizes the degree of fluctuation in a set of data; mean represents the average value. In general, the process requirement of the furnace tube process is to control the uniformity of the film thickness of HCD-SIN grown at different positions in the same furnace tube U% < 0.4%.
[0009] Therefore, the etching time of HCD-SIN obtained by the above method can reduce the difference in the etching amount of HCD-SIN located at different positions in the vertical direction in the furnace tube during the wet cleaning process, and greatly reduce the morphology difference of HCD-SIN in the same furnace after wet cleaning; since the method of the present invention can reduce the morphology difference of Spacer HCD-SIN of the same batch, it is of certain significance to maintain the stability of the device structure of the spacer loop (Spacer loop) using SpacerHCD-SIN as the spacer layer.
[0010] As the inventors further studied the process of Spacer HCD-SIN, they found that the main reason why the morphology of the same batch of Spacer HCD-SIN in the wet process shows regular changes with the change of its position in the vertical direction of the furnace tube is that the HCD-SIN at different positions in the vertical direction of the same vertical tube furnace tube has different sensitivities to temperature, that is, there is a correlation between the temperature sensitivity of HCD-SIN and the position of HCD-SIN in the vertical direction of the furnace tube. This is because when HCD-SIN is prepared in the same furnace tube, different positions in the vertical direction of the furnace tube will be affected by the temperature and the flow of reaction gas, resulting in different thicknesses of the prepared HCD-SIN. However, in order to ensure the stability and uniformity of the HCD-SIN growth process, it is necessary to try to ensure that the HCD-SIN grown in the same furnace tube at different positions in the vertical direction of the furnace tube In order to improve the thickness uniformity of HCD-SIN, and because the gas flow at different positions is difficult to adjust, it is necessary to collect the relationship between the growth thickness and temperature of HCD-SIN grown at different positions in the vertical direction of the furnace tube, and then improve the uniformity of the film thickness of HCD-SIN prepared in the same furnace tube by adjusting the temperature of each area. Based on the relationship between the growth thickness and temperature of HCD-SIN grown at different positions in the vertical direction of the furnace tube collected above, the inventor obtains the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, and finds that the temperature sensitivity of HCD-SIN is correlated with the position of HCD-SIN in the vertical direction of the furnace tube. As a result, HCD-SIN produced from the same furnace tube will have morphological differences after wet cleaning. At the same time, because the inventor further studied the process of Spacer HCD-SIN, it was found that the etching rates corresponding to HCD-SIN with different temperature sensitivities were also different. Based on the correlation of temperature sensitivity of different positions in the vertical direction of HCD-SIN grown under certain conditions in the furnace tube, when collecting the etching rates of HDC-SIN at different positions in the vertical direction of the furnace tube, the correlation of temperature sensitivity and etching rate at different positions in the vertical direction of the furnace tube was also established. Therefore, when the inventors defined the etching time of HCD-SIN by the thickness to be etched of HCD-SIN and its position in the vertical direction of the furnace tube when preparing HCD-SIN, and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, HCD-SIN temperature sensitivity was introduced, and the position in the vertical direction of the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube were correlated by temperature sensitivity.Specifically, the inventors first correlated the position of HCD-SIN in the vertical direction in the furnace tube when it was prepared with the temperature sensitivity of HCD-SIN at different positions in the vertical direction in the furnace tube, and then correlated the temperature sensitivity of HCD-SIN at different positions in the vertical direction in the furnace tube with the etching rate of HCD-SIN at different positions in the vertical direction in the furnace tube. Finally, the thickness to be etched of HCD-SIN at different positions in the vertical direction in the furnace tube was correlated with the etching rate of HCD-SIN at different positions in the vertical direction in the furnace tube, so as to obtain the etching time of HCD-SIN at different positions in the vertical direction in the furnace tube.
[0011] Specifically, when the inventor associates the position of HCD-SIN in the vertical direction of the furnace tube with the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, it is thought of associating the different positions of HCD-SIN in the vertical direction of the furnace tube with the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube to obtain a first correlation relationship. More specifically, by acquiring the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, curve fitting is performed (the acquisition method and curve fitting method of the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube can be adopted in the conventional manner of the prior art, and the present invention is not limited thereto) to obtain a first correlation curve. For example, by detecting the sensitivity of HCD-SIN to temperature at the top position of the furnace tube (the third position for placing wafers from top to bottom in the furnace tube, there are 70 positions from top to bottom in a furnace tube, and each position is 0.6 cm apart) is (Angstroms / degrees Celsius, where the temperature is the growth temperature of HCD-SIN); the temperature sensitivity of HCD-SIN near the top of the furnace tube (the 16th wafer placement position in the furnace tube from the top to the bottom) is The temperature sensitivity of the HCD-SIN located in the middle of the furnace tube (the 29th wafer placement position from the top of the furnace tube) is The temperature sensitivity of the HCD-SIN near the bottom of the furnace tube (the 42nd wafer placement position from the top of the furnace tube) is The temperature sensitivity of HCD-SIN at the bottom of the furnace tube (the 55th wafer placement position from the top of the furnace tube) is The first correlation curve is: Ya = 0.0415Xa + 8.2354, R1 2 =0.9878, Ya is the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, the unit is Xa is the vertical position of HCD-SIN in the furnace tube (the position of the wafer placed from top to bottom in the furnace tube), R1 2Refers to the accuracy of the fitting curve. The closer the value is to 1, the stronger the correlation is. In general, the temperature sensitivity of HCD-SIN decreases with the increase of its vertical height in the furnace tube, that is, the temperature sensitivity of HCD-SIN at different vertical positions in the furnace tube is linearly negatively correlated with its vertical position from bottom to top in the furnace tube when preparing HCD-SIN.
[0012] When the inventor associates the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube with the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, he also thinks of associating the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube with the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube to obtain a second correlation relationship. More specifically, by obtaining the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, the two are curve-fitted (the acquisition method of the temperature sensitivity at different positions in the vertical direction of the furnace tube, the acquisition method of the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube and the curve fitting method adopt the commonly used methods of the prior art, and the present invention is not limited to this) to obtain a second correlation curve. The second correlation curve obtained is: Yb=-1.3532Xb 2 +27.882Xb-102.83, that is, the second correlation is defined by the second-order polynomial of the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, where Yb is the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, and the unit is Xb is the HCD-SIN temperature sensitivity at different positions in the vertical direction of the furnace tube, in units of And Xb=Ya. Thus, when it is necessary to specifically determine the etching time of HCD-SIN at different positions in the vertical direction of the furnace tube, the etching time of HCD-SIN at different positions in the vertical direction of the furnace tube can be obtained by the thickness of HCD-SIN to be etched at different positions in the vertical direction of the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube in the second correlation curve. Thus, etching HCD-SIN according to the etching time obtained by this method can make the actual etching amount of HCD-SIN prepared at different positions in the vertical direction of the same furnace tube closer to the thickness of HCD-SIN to be etched than that not using this method, thereby reducing the morphological difference of HCD-SIN prepared at different positions in the vertical direction of the same furnace tube after etching.
[0013] That is, as the inventors further study the process of Spacer HCD-SIN, the etching rates of HCD-SIN at different positions in the vertical direction of the furnace tube are set to be defined by the first correlation formed between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and its position in the vertical direction of the furnace tube when preparing HCD-SIN, and the second correlation formed between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and the etching rates of HCD-SIN at different positions in the vertical direction of the furnace tube. In addition, the first correlation is defined by the first correlation curve, wherein the first correlation curve is: Ya = 0.0415Xa + 8.2354, R1 2 =0.9878, Ya is the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, and Xa is the position of HCD-SIN in the vertical direction of the furnace tube. The second correlation relationship is defined by the second correlation curve, where the second correlation curve is: Yb=-1.3532Xb 2 +27.882Xb-102.83, Yb is the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, the unit is Xb is the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, and Xb=Ya.
[0014] In some embodiments, the etching time of HCD-SIN at different positions in the vertical direction of the furnace tube is set to Time(HCD-SIN)=Thinkness(HCD-SIN) / Yb, where Thinkness(HCD-SIN) is the thickness of the HCD-SIN to be etched. Thus, different etching times can be used for the HCD-SIN prepared at different positions in the vertical direction of the furnace tube, so that the actual etching amount of the HCD-SIN prepared at different positions in the vertical direction of the furnace tube is closer to the thickness of the HCD-SIN to be etched compared to not using this method, thereby reducing the morphological differences of the HCD-SIN prepared at different positions in the vertical direction of the furnace tube after etching; and, for different furnace tubes for growing HCD-SIN, since different furnace tubes need to be adjusted according to the temperature sensitivity of different positions in order to stabilize the uniformity of the thickness of the grown HCD-SIN film layer, thus, the vertical direction of each furnace tube can be obtained. The actual temperature sensitivity at different positions on the vertical direction of the furnace tube, that is, by adopting the method of the present invention, the temperature sensitivity at different positions in the vertical direction of the furnace tube when preparing HCD-SIN can be directly used without obtaining the temperature sensitivity separately, and the operation is faster; and, because the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube can be obtained when HCD-SIN is prepared in different furnaces, the formula Time (HCD-SIN) = Thinkness (HCD-SIN) / Yb, which is jointly defined by the first correlation curve, the second correlation curve and the etching time of HCD-SIN at different positions in the vertical direction of the furnace tube of the present invention, can be applied to different furnace tubes.
[0015] In some embodiments, the etching time of HCD-SIN at different positions in the vertical direction of the furnace tube is set to Time(HCD-SIN)=Thinkness(HCD-SIN) / Yc, wherein Thinkness(HCD-SIN) is the thickness of HCD-SIN to be etched, and Yc is the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, which is defined by a second-order polynomial of the position of HCD-SIN in the vertical direction of the furnace tube. Specifically, by obtaining the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, the two are curve-fitted (the acquisition method and curve-fitting method of the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube can be adopted in the conventional manner of the prior art, and the present invention is not limited thereto), to obtain the third correlation curve Yc=-0.0027Xc 2 +0.2609Xc+34.631, in units of Xc is the vertical position of HCD-SIN in the furnace tube.
[0016] In some embodiments, in step S20, the preparation conditions of HCD-SIN are as follows: controlling the flow range of HCD to be 40-50 sccm (sccm is a unit of volume flow rate, and gas volume flow rate refers to the volume of gas flowing through the delivery pipeline per unit time), controlling the flow range of NH3 to be 1800-1900 sccm, and controlling the temperature range in the furnace tube to be 560-580°C.
[0017] In some embodiments, the uniformity of the film thickness of the Spacer HCD-SIN is adjusted based on the Spacer morphology at the position with the highest temperature sensitivity at the furnace tube growth position. Since the bottom of the furnace tube is the position with the highest temperature sensitivity of the Spacer HCD-SIN and the highest etching rate, the morphology of the Spacer HCD-SIN at this position is used as a reference, and the etching time can be adjusted by the correlation (correlation curve) provided by the present invention, and the wet cleaning time of the wafer at other positions is increased to achieve the purpose of stabilizing the morphology of the Spacer HCD-SIN.
[0018] In some embodiments, the etching solution used for wet cleaning is DHF (dilute hydrofluoric acid).
[0019] According to another aspect of the present invention, a semiconductor device is provided, wherein the Spacer HCD-SIN in the transistor is manufactured by the aforementioned semiconductor manufacturing method. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the process for preparing Spacer HCD-SIN in the prior art;
[0021] Figure 2 This is a transmission electron microscope (TEM) slice image of the Spacer HCD-SIN at the top of the furnace tube etched using the existing process;
[0022] Figure 3 This is a TEM slice image of the Spacer HCD-SIN located at the bottom of the furnace tube etched using the existing process;
[0023] Figure 4 A schematic flow chart of a semiconductor manufacturing method according to an embodiment of the present invention;
[0024] Figure 5 It is a schematic diagram of the fitting line of the growth temperature and thickness of HCD-SIN at different positions in the vertical direction of the furnace tube;
[0025] Figure 6It is a correlation curve diagram of the temperature sensitivity of HCD-SIN at different positions in the vertical direction in the furnace tube and its position in the vertical direction in the furnace tube when preparing HCD-SIN;
[0026] Figure 7 Correlation curve between the temperature sensitivity of HCD-SIN at different positions in the vertical direction in the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction in the furnace tube;
[0027] Figure 8 This is a TEM slice image of the Spacer HCD-SIN located at the bottom of the furnace tube etched by the method of the present invention;
[0028] Fig. 9 is a correlation curve diagram of the etching rate of HCD-SIN at different positions in the vertical direction in the furnace tube and the position of HCD-SIN in the vertical direction in the furnace tube when preparing HCD-SIN;
[0029] Fig.10 The actual etching rate diagram of HCD-SIN located at the top and bottom of the furnace tube;
[0030] Fig.11 The etching amount distribution diagram obtained after etching HCD-SIN at the top and bottom of the furnace tube for 9.8 minutes;
[0031] Fig.12 This is the etching amount distribution diagram obtained after etching the HCD-SIN at the top of the furnace tube for 9.8 minutes and etching the HCD-SIN at the bottom of the furnace tube for 8.6 minutes. DETAILED DESCRIPTION
[0032] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.
[0033] It should also be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include" and "comprise" include not only those elements, but also other elements that are not explicitly listed, or also include elements inherent to such processes, methods, articles or equipment. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the existence of other identical elements in the process, method, article or equipment that includes the elements. The terms used in this article are generally commonly used terms by those skilled in the art. If they are inconsistent with commonly used terms, the terms in this article shall prevail.
[0034] In the present application, the term "Spacer HCD-SIN of the same batch" refers to all Spacer HCD-SIN obtained after HCD-SIN prepared in the same furnace tube is dry-etched and wet-cleaned.
[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0036] Figure 4 A semiconductor preparation method of an embodiment of the present invention is schematically shown. The method is based on the inventor's repeated research on the process of Spacer HCD-SIN to solve the problem of differences in morphology of HCD-SIN in the same furnace after wet cleaning. It is found that even if the morphology of HCD-SIN in the same furnace is not much different when it is just out of the furnace, after wet cleaning, the morphology of Spacer HCD-SIN in the same batch will also be greatly different, and the morphology change is correlated with its position in the vertical direction of the furnace tube (after wet cleaning of HCD-SIN in the same furnace and with the same thickness, the thickness of Spacer HCD-SIN at the top of the furnace is significantly greater than the thickness of Spacer HCD-SIN at the bottom of the furnace. For example, the Spacer HCD-SIN at the top of the furnace tube (the third position from the top of the furnace tube where the wafer is placed) and the Spacer HCD-SIN at the bottom of the furnace tube (the 60th position from the top of the furnace tube where the wafer is placed) are cleaned by DHF. HCD-SIN etching was performed for 9.8 min. After etching, the thickness of the SpacerHCD-SIN31 at the periphery of the gate 32 at the top of the furnace tube was in the range of 33.3-33.6 nm, and the height was in the range of 73.3-73.6 nm (e.g. Figure 2 After etching, the thickness of the SpacerHCD-SIN31 at the outer periphery of the gate 32 at the bottom of the furnace tube is 29.8nm, and the height range is 68.2-69nm (as shown); Figure 3 As shown in the figure, the thickness difference between the two after etching can reach 3.5nm) and the thickness difference of SpacerHCD-SIN31 on the periphery of the gate electrode 32 will lead to differences in wafer electrical properties and yield. Specifically, as Figure 4 As shown, the method comprises the following steps:
[0037] S20: Control the thickness U% of HCD-SIN prepared at different positions in the vertical direction of the same tube furnace to be less than 0.4%;
[0038] S30: dry etching the HCD-SIN prepared in the furnace tube;
[0039] S40: wet cleaning the HCD-SIN after dry etching, and, during the wet cleaning process, the etching time of the HCD-SIN is set to be defined by the thickness of the HCD-SIN to be etched, the position of the HCD-SIN in the vertical direction in the furnace tube when the HCD-SIN is prepared, and the etching rate of the HCD-SIN at different positions in the vertical direction in the furnace tube. Wherein, U% = Sigma / Mean.
[0040] The etching time of HCD-SIN obtained by the above method can reduce the difference in etching amount of HCD-SIN prepared at different positions in the furnace tube during the wet cleaning process, and greatly reduce the morphological difference of HCD-SIN in the same furnace after wet cleaning.
[0041] In a preferred embodiment of the present invention, as the inventors further studied the process of Spacer HCD-SIN, they found that the main reason why the morphology of the same batch of HCD-SIN in the wet process shows regular changes with the change of its position in the vertical direction of the furnace tube is that the HCD-SIN at different positions in the vertical direction of the same furnace tube has different sensitivities to temperature. Therefore, the inventors introduced the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube in the process of jointly limiting the etching time of HCD-SIN by the thickness to be etched of HCD-SIN and its position in the vertical direction of the furnace tube when preparing HCD-SIN and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube. Based on this, the correlation curve between the growth temperature and growth thickness of HCD-SIN at different positions in the vertical direction of the furnace tube was obtained (such as Figure 5As shown, its slope is the HCD-SIN temperature sensitivity of different positions in the vertical direction of the furnace tube), and finally the HCD-SIN temperature sensitivity table of different positions in the furnace tube as shown in Table 1 is obtained. According to the experimental results, the HCD-SIN temperature sensitivity of different positions in the vertical direction of the furnace tube decreases with the increase of its position in the vertical direction of the furnace tube, that is, the HCD-SIN temperature sensitivity of different positions in the vertical direction of the furnace tube is linearly negatively correlated with its position in the vertical direction from bottom to top in the furnace tube when preparing HCD-SIN. Based on this discovery, the inventor has done further research and found that the HCD-SIN temperature sensitivity of different positions in the vertical direction of the furnace tube is correlated with its position in the vertical direction of the furnace tube when preparing HCD-SIN. Based on these findings, the inventors obtained the correlation between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and its position in the vertical direction of the furnace tube through multiple experiments (the correlation curve between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and its position in the vertical direction of the furnace tube is shown in FIG. Figure 6 Specifically, by obtaining the HCD-SIN temperature sensitivity at different positions in the vertical direction of the furnace tube, a curve fitting is performed, which is specifically reflected in the first correlation curve: Ya = 0.0415Xa + 8.2354, R1 2 =0.9878, Ya is the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the HCD-SIN furnace tube, unit is Xa is the position of HCD-SIN in the vertical direction of the furnace tube (the position of the wafer placed from top to bottom in the furnace tube); the inventors also obtained through multiple experiments that the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube are correlated (the correlation curve of the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube is as shown in Figure 7 Specifically, by obtaining the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, the two are curve-fitted, which is specifically reflected in the second correlation curve: Yb = -1.3532Xb 2 +27.882Xb-102.83, that is, the second correlation is defined by the second-order polynomial of the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, where Yb is the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, and the unit is Xb is the HCD-SIN temperature sensitivity at different positions in the vertical direction of the furnace tube, in units of And Xb=Ya. Therefore, the inventor further sets the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube to be defined by the first correlation formed between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and its position in the vertical direction of the furnace tube when preparing HCD-SIN, and the second correlation formed between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube; the inventor also combines the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube in the second correlation curve with the thickness to be etched of HCD-SIN, and obtains the etching time of HCD-SIN at different positions in the vertical direction of the furnace tube. For example, the etching time of HCD-SIN at different positions in the vertical direction of the furnace tube is set to Time(HCD-SIN)=Thinkness(HCD-SIN) / Yb.
[0042] Table 1:
[0043]
[0044] It is required to etch away HCD-SIN For example, the HCD-SIN is wet cleaned with diluted hydrofluoric acid of the same concentration (for example, the volume ratio of hydrofluoric acid to water is 1:100). When the HCD-SIN located at the top of the furnace (Xa=3) is required to be etched When the thickness is , first, the temperature sensitivity Ya = 8.3599 at the furnace top is calculated through the first correlation curve: Ya = 0.0415Xa + 8.2354, and then the second correlation curve: Yb = -1.3532Xb 2 +27.882Xb-102.83 to calculate the etching rate at the top of the furnace Yb = -94.5723 + 233.0907-102.83 = 35.6884 (the calculation process and results are retained to four decimal places, according to Fig.10 As shown in Figure (a), the actual average etching rate ER at the top of the furnace is Mean It can be seen that the theoretical etching rate calculated by the second correlation curve is not much different from the actual etching rate). Finally, by using the formula Time(HCD-SIN)=Thinkness(HCD-SIN) / Yb, Time(HCD-SIN)=350 / 35.6844min≈9.8min (the calculation result retains one decimal place); when the HCD-SIN at the bottom of the furnace (Xa=60) is required to etch When the thickness is , first, the temperature sensitivity Ya = 10.7254 at the furnace top is calculated through the first correlation curve: Ya = 0.0415Xa + 8.2354, and then the second correlation curve: Yb = -1.3532Xb 2 +27.882Xb-102.83 to calculate the etching rate at the top of the furnace Yb = -155.6643 + 299.0456 - 102.83 = 40.5513 (the calculation process and results are retained to four decimal places, according to Fig.10 As shown in Figure (b), the actual average etching rate ER at the bottom of the furnace is Mean It can be seen that the theoretical etching rate calculated by the third correlation curve is not much different from the actual etching rate). Finally, the formula Time(HCD-SIN)=Thinkness(HCD-SIN) / Yb is used to calculate that Time(HCD-SIN)=350 / 40.2213min≈8.7min (the calculation result retains one decimal place). The thickness range of HCD-SIN31 at the top of the furnace tube after etching is 33.3-33.6nm, and the height range is 73.3-73.6nm (such as Figure 2 After etching, the thickness of HCD-SIN31 at the bottom of the furnace tube is 32.6-32.9nm, and the height range is 76.0-76.3nm (as shown in FIG. Figure 8 As shown in the figure, the thickness difference between the two after etching is only 1 nm at most, thereby reducing the morphological difference after HCD-SIN etching at different positions in the vertical direction in the same batch of furnace tubes.
[0045] At the same time, since the etching rate of the HCD-SIN at the top of the furnace is different from that at the bottom of the furnace tube, if the same etching time is used, the etching amount of the HCD-SIN at the top of the furnace and the etching amount of the HCD-SIN at the bottom of the furnace tube will be greatly different, for example, Fig.11 As shown, the HCD-SIN at the top of the furnace tube and the HCD-SIN at the bottom of the furnace tube were wet cleaned for 9.8 minutes, and the etching amount distribution diagram of the HCD-SIN at the top of the furnace tube was obtained as shown in FIG. Fig.11 As shown in Figure (a), the average etching amount is The etching amount distribution diagram of HCD-SIN at the bottom of the furnace tube is as follows: Fig.11 As shown in Figure (b), the average etching amount is It can be seen that the same etching time will result in a difference in the etching amount between the HCD-SIN at the top of the furnace tube and the HCD-SIN at the bottom of the furnace tube. By adopting the method of the present invention, according to the formula, different etching times are used for HCD-SIN at different heights of the furnace tube, which can greatly reduce the difference in the etching amount of HCD-SIN at different heights of the furnace tube. For example, Fig.12 As shown, the HCD-SIN at the top of the furnace tube was wet cleaned for 9.8 minutes, and the HCD-SIN at the bottom of the furnace tube was wet cleaned for 8.6 minutes. The etching amount distribution diagram of the HCD-SIN at the top of the furnace tube is as shown in FIG. Fig.12 As shown in Figure (a), the average etching amount is The etching amount distribution diagram of HCD-SIN at the bottom of the furnace tube is as follows: Fig.12 As shown in Figure (b), the average etching amount is It can be seen that by reducing the etching time of the HCD-SIN at the bottom of the furnace tube, the difference in etching amount between the HCD-SIN at the top of the furnace tube and the HCD-SIN at the bottom of the furnace tube can be reduced to
[0046] In some embodiments, in step S20, the preparation conditions of HCD-SIN are as follows: controlling the flow range of HCD to be 40-50 sccm (sccm is a unit of volume flow rate, and gas volume flow rate refers to the volume of gas flowing through the delivery pipeline per unit time), controlling the flow range of NH3 to be 1800-1900 sccm, and controlling the temperature range in the furnace tube to be 560-580°C.
[0047] In some embodiments, the uniformity of the film thickness of the Spacer HCD-SIN is adjusted based on the morphology of the Spacer HCD-SIN at the position where the temperature sensitivity of the furnace tube growth position is the highest.
[0048] In other embodiments, the inventors also found in the process of studying the process of Spacer HCD-SIN that during the wet cleaning process, the morphology of the HCD-SIN of the same batch changes regularly with the change of its position in the vertical direction of the furnace. It is also manifested in that the etching rate of HCD-SIN at different positions in the vertical direction of the same furnace tube is different. For example, the etching rate of HCD-SIN at the top of the furnace tube (the third position from the top to the bottom of the furnace tube where the wafer is placed, that is, the "upper" position in the vertical direction of the furnace tube) is (angstroms / minute); The etching rate of HCD-SIN located in the middle of the furnace tube near the top (the 16th wafer placement position from the top to the bottom of the furnace tube, that is, the "upper middle" position in the vertical direction of the furnace tube) is (angstroms / minute); The etching rate of HCD-SIN located in the middle of the furnace tube (the 29th wafer placement position from the top to the bottom of the furnace tube, that is, the "middle" position in the vertical direction of the furnace tube) is (angstroms / minute); The etching rate of HCD-SIN located in the middle of the furnace tube near the bottom (the 42nd wafer placement position from the top to the bottom of the furnace tube, that is, the "lower middle" position in the vertical direction of the furnace tube) is (angstroms / minute); The etching rate of HCD-SIN at the top of the furnace tube (the 55th wafer placement position from the top to the bottom of the furnace tube, that is, the "bottom" position in the vertical direction of the furnace tube) is (Angstroms / minute). That is, the etching rate of HCD-SIN decreases as its vertical position in the furnace tube increases (the correlation curve between the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube and its vertical position in the furnace tube is shown in Fig. 9 Specifically, by obtaining the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, the two are curve-fitted, which is specifically reflected in the third correlation curve: Yc = -0.0027Xc 2 +0.2609Xc+34.631, that is, the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube is defined by the second-order polynomial of the position of HCD-SIN in the vertical direction of the furnace tube, where R3 2 =0.9998, Yc is the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, the unit is Xc is the position of HCD-SIN in the vertical direction of the furnace. In order to improve the fitting accuracy of the third correlation curve, a large amount of corresponding relationships between the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube and the position of HCD-SIN in the vertical direction of the furnace tube can be collected, and then the collected data can be determined by intelligent analysis and model training. Therefore, the inventor further found that the etching time of HCD-SIN is set to be limited by the thickness to be etched of HCD-SIN, the position of HCD-SIN in the vertical direction of the furnace tube when preparing HCD-SIN, and the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube. It can also be achieved by the following steps:
[0049] The etching time of HCD-SIN at different positions in the vertical direction of the furnace tube is set to Time(HCD-SIN)=Thinkness(HCD-SIN) / Yc, where Thinkness(HCD-SIN) is the thickness of HCD-SIN to be etched, and Yc=-0.0027Xc 2 +0.2609Xc+34.631.
[0050] The theoretical etching rate calculated by the third correlation curve is not much different from the actual etching rate, so the difference in the morphology of HCD-SIN after etching prepared at different vertical positions in the furnace tube can be reduced.
[0051] According to another aspect of the present invention, a semiconductor device is provided, wherein the Spacer HCD-SIN in the transistor is manufactured by the aforementioned semiconductor manufacturing method.
[0052] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A semiconductor manufacturing method, characterized in that: The following steps are involved: S20: Control the thickness U% of HCD-SIN prepared at different positions in the vertical direction of the same tube furnace to be less than 0.4%; S30: dry etching the HCD-SIN prepared in the furnace tube; S40: wet cleaning the dry-etched HCD-SIN, and, during the wet cleaning process, the etching time of the HCD-SIN is set to be limited by the thickness of the HCD-SIN to be etched, the position of the HCD-SIN in the vertical direction in the furnace tube when preparing the HCD-SIN, and the etching rate of the HCD-SIN at different positions in the vertical direction in the furnace tube.
2. The semiconductor manufacturing method according to claim 1, characterized in that: The etching rates of HCD-SIN at different positions in the vertical direction of the furnace tube are set to be defined by a first correlation formed between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and its position in the vertical direction of the furnace tube when preparing HCD-SIN, and a second correlation formed between the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube and the etching rates of HCD-SIN at different positions in the vertical direction of the furnace tube.
3. The semiconductor manufacturing method according to claim 2, characterized in that: The first correlation relationship is that the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube is linearly negatively correlated with its position in the vertical direction from bottom to top in the furnace tube when preparing HCD-SIN.
4. The semiconductor manufacturing method according to claim 3, characterized in that: The second correlation is defined by a second-order polynomial of the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube.
5. The semiconductor manufacturing method according to claim 4, characterized in that: The first association relationship is defined by a first correlation curve, wherein the first correlation curve is: Ya=0.0415Xa+8.2354,R1 2 =0.9878, Ya is the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, and Xa is the position of HCD-SIN in the vertical direction of the furnace tube; The second association relationship is defined by a second correlation curve, wherein the second correlation curve is: Yb=-1.3532Xb 2 +27.882Xb-102.83, Yb is the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, the unit is Xb is the temperature sensitivity of HCD-SIN at different positions in the vertical direction of the furnace tube, and Xb = Ya; The etching time of HCD-SIN at different positions in the vertical direction of the furnace tube is set to Time(HCD-SIN)=Thinkness(HCD-SIN) / Yb, where Thinkness(HCD-SIN) is the thickness of HCD-SIN to be etched.
6. The semiconductor manufacturing method according to claim 1, characterized in that: The etching time of HCD-SIN at different positions in the vertical direction of the furnace tube is set to Time(HCD-SIN)=Thinkness(HCD-SIN) / Yc, wherein Thinkness(HCD-SIN) is the thickness of HCD-SIN to be etched, and Yc is the etching rate of HCD-SIN at different positions in the vertical direction of the furnace tube, which is defined by a second-order polynomial of the position of HCD-SIN in the vertical direction of the furnace tube.
7. The semiconductor manufacturing method according to any one of claims 1 to 6, characterized in that: In step S20, the preparation conditions of HCD-SIN are as follows: controlling the flow range of HCD to 40-50 sccm, controlling the flow range of NH3 to 1800-1900 sccm, and controlling the temperature in the furnace tube to 560-580°C.
8. The semiconductor manufacturing method according to any one of claims 1 to 6, characterized in that: In step S40 , the uniformity of the film thickness of the Spacer HCD-SIN is adjusted based on the Spacer HCD-SIN morphology at the position where the temperature sensitivity of the furnace tube growth position is the highest.
9. The semiconductor manufacturing method according to any one of claims 1 to 6, characterized in that: The etching solution used for the wet cleaning is DHF.
10. A semiconductor device, characterized in that The Spacer HCD-SIN is prepared by the semiconductor preparation method described in any one of claims 1 to 9.