Semiconductor structure and manufacturing method thereof, and conductive structure and manufacturing method thereof
By forming microparticles between the conductive matrix and the auxiliary layer, the problem of interface peeling caused by the mismatch in thermal expansion coefficients between the conductive pillar and the auxiliary layer is solved, and the product yield and process efficiency of the semiconductor device are improved.
Patent Information
- Application Number
- CN202410857504.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
During the heat treatment process of semiconductor devices, the thermal expansion coefficient mismatch between the conductive pillar and the auxiliary layer causes the contact interface to peel off, affecting product yield.
By depositing a second initial auxiliary layer between the conductive matrix and the auxiliary layer, and allowing its elements to migrate into the conductive matrix to form microparticles during the heat treatment process, the grain growth of the conductive pillars is restricted and the contact interface between the conductive pillars and the auxiliary layer is improved. Matching degree.
It effectively reduces the interface peeling problem between the conductive pillar and the auxiliary layer, improves the product yield, and reduces verification cost and time.
Smart Images

Figure CN118738017A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of semiconductor technology, and in particular to a semiconductor structure and a manufacturing method thereof, and a conductive structure and a manufacturing method thereof. Background Art
[0002] As an important material, metal materials play an important role in the manufacture of semiconductor devices. Metal materials can be used to manufacture the conductor layer of semiconductor chips. For example, the collector of an insulated gate bipolar transistor (IGBT) includes multiple metal layers stacked in layers. Metal materials can also be used for packaging and connection of semiconductor devices. For example, in the silicon adapter board that realizes the interconnection between chips, TSV (Through Silicon Via) is filled with metal materials. The organizational properties of metal materials directly affect the performance of semiconductor chips or semiconductor devices, so they have always attracted much attention. Summary of the invention
[0003] According to a first aspect of the present disclosure, there is provided a semiconductor structure, comprising:
[0004] a first substrate;
[0005] A first conductive structure is located in the first substrate; the first conductive structure includes a conductive column and a first auxiliary layer arranged around the side wall of the conductive column, wherein the conductive column includes a first conductive matrix and first microparticles distributed in the first conductive matrix, and at least some elements of the first microparticles are different from elements of the first conductive matrix.
[0006] In some embodiments, the first conductive structure further includes:
[0007] The second auxiliary layer is located between the conductive column and the first auxiliary layer, wherein the second auxiliary layer is used to provide at least part of the elements forming the first microparticles.
[0008] In some embodiments, the composition of the second auxiliary layer includes: a metal boride;
[0009] Wherein, the first microparticles include boron element.
[0010] In some embodiments, the composition of the first conductive matrix includes at least one of the following: copper, tungsten.
[0011] In some embodiments, the first auxiliary layer comprises:
[0012] A barrier layer and an adhesion layer are stacked along the radial direction of the conductive column, and the adhesion layer is located between the conductive column and the barrier layer; wherein,
[0013] The adhesive layer includes an adhesive matrix and second fine particles distributed in the adhesive matrix, wherein at least part of elements of the second fine particles are different from elements of the adhesive matrix.
[0014] In some embodiments, the first substrate is a silicon substrate having a first surface and a second surface opposite to each other, and the first conductive structure extends along a direction perpendicular to the first surface and penetrates the silicon substrate;
[0015] The semiconductor structure further comprises:
[0016] a redistribution layer, located on the first surface of the silicon substrate and connected to the first conductive structure;
[0017] The bump is located on the second surface of the silicon substrate and connected to the first conductive structure.
[0018] According to a second aspect of the present disclosure, a method for manufacturing a semiconductor structure is provided, the method comprising:
[0019] providing a first substrate;
[0020] etching the first substrate to form a hole in the first substrate;
[0021] forming a first initial auxiliary layer on the sidewalls of the hole;
[0022] forming a second initial auxiliary layer on a sidewall of the first initial auxiliary layer;
[0023] After forming the second initial auxiliary layer, filling the hole to form a first conductive matrix;
[0024] The second initial auxiliary layer and the conductive substrate are subjected to a heat treatment, wherein at least part of the elements in the second initial auxiliary layer migrate to the first conductive substrate to form first microparticles.
[0025] In some embodiments, the heat treatment of the second initial auxiliary layer and the conductive substrate comprises:
[0026] The first substrate formed with the first initial auxiliary layer, the second initial auxiliary layer and the first conductive base is annealed; wherein the first initial auxiliary layer after annealing forms a first auxiliary layer.
[0027] According to a third aspect of the present disclosure, there is provided another semiconductor structure, the semiconductor structure comprising:
[0028] A second substrate having a P region and an N region formed therein;
[0029] A second conductive structure is in contact with the P region or the N region, the second conductive structure includes a plurality of conductive layers, at least one of the conductive layers includes a second conductive matrix, and third microparticles distributed in the second conductive matrix, at least some elements of the third microparticles are different from elements of the second conductive matrix.
[0030] In some embodiments, the second conductive structure further includes: a third auxiliary layer, the third auxiliary layer being disposed between two adjacent conductive layers or on a side of the conductive layer farthest from the second substrate away from the second substrate;
[0031] The third auxiliary layer is used to provide an element for forming the third fine particles to the conductive layer in contact with the third auxiliary layer.
[0032] In some embodiments, the third auxiliary layer is disposed between every two adjacent conductive layers.
[0033] In some embodiments, the composition of the third auxiliary layer includes: a metal boride;
[0034] Wherein, the third microparticles include boron element.
[0035] In some embodiments, the semiconductor structure includes an insulated gate bipolar transistor structure, wherein the second conductive structure is a collector of the insulated gate bipolar transistor structure.
[0036] According to a fourth aspect of the present disclosure, there is provided a conductive structure, the conductive structure comprising: a conductive layer and an auxiliary layer stacked;
[0037] The conductive layer includes a conductive matrix and microparticles distributed in the conductive matrix; the auxiliary layer is used to provide at least part of the elements forming the microparticles.
[0038] In some embodiments, the auxiliary layer comprises: a metal boride;
[0039] Wherein, the microparticles include boron element.
[0040] According to a fifth aspect of the present disclosure, a method for manufacturing a conductive structure is provided, the manufacturing method comprising:
[0041] forming a conductive substrate and an initial auxiliary layer arranged in a stacked manner;
[0042] The conductive substrate and the initial auxiliary layer are subjected to a heat treatment, wherein at least part of the elements in the initial auxiliary layer migrate to the conductive substrate to form microparticles.
[0043] In some embodiments, the thickness of the auxiliary layer is less than 100 nm.
[0044] In the semiconductor structure provided by the embodiment of the present disclosure, the semiconductor structure includes a first substrate and a first conductive structure located in the first substrate, the first conductive structure includes a conductive column and a first auxiliary layer surrounding the conductive column, and the conductive column includes a first conductive matrix and first microparticles distributed in the first conductive matrix. The first microparticles are second phase particles formed during the heat treatment of the semiconductor structure, and the second phase particles are relative to the matrix phase of the first conductive matrix. The first microparticles can be pinned at the grain boundaries of the grains in the first conductive matrix, hindering the growth of the grains of the first conductive matrix during the heat treatment, thereby limiting the change in the thermal expansion coefficient of the first conductive matrix, improving the problem of contact interface peeling caused by the poor matching of the thermal expansion coefficients between the conductive column and the first auxiliary layer after heat treatment, and reducing the product yield loss.
[0045] In addition, at least some elements of the first microparticles are different from the elements of the first conductive matrix. In other words, the first microparticles can be formed by elements in the first conductive matrix and other foreign elements. In the embodiment of the present disclosure, the composition and formation process of the existing first conductive matrix are not changed. Instead, after the first conductive matrix is formed, elements are provided from the outside so that the elements of the first conductive matrix and the foreign elements are combined to form the first microparticles, which has little impact on the existing formation process of the first conductive structure, can reduce verification costs and time, and reduce product yield loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1a A schematic diagram of a semiconductor structure including TSV before heat treatment provided in an embodiment of the present disclosure;
[0047] Figure 1b A schematic diagram of a semiconductor structure including TSV after heat treatment provided in an embodiment of the present disclosure;
[0048] Figure 2 A schematic diagram of a process for manufacturing a semiconductor structure provided by an embodiment of the present disclosure;
[0049] Figure 3a to Figure 3h A schematic diagram of the structure of a semiconductor structure during the manufacturing process provided by an embodiment of the present disclosure;
[0050] Figure 4 A schematic diagram of a semiconductor structure provided by an embodiment of the present disclosure;
[0051] Figure 5 A schematic diagram of another semiconductor structure provided by an embodiment of the present disclosure;
[0052] Figure 6 A schematic diagram of another semiconductor structure provided by an embodiment of the present disclosure;
[0053] Figure 7 A schematic diagram of another semiconductor structure provided by an embodiment of the present disclosure;
[0054] Figure 8 A schematic diagram of another semiconductor structure provided by an embodiment of the present disclosure;
[0055] Fig. 9 A schematic flow chart of another method for manufacturing a semiconductor structure provided by an embodiment of the present disclosure;
[0056] Figures 10a to 10c A schematic diagram of the structure of another semiconductor structure during the manufacturing process provided by an embodiment of the present disclosure;
[0057] Fig.11 A schematic diagram of a semiconductor structure provided by an embodiment of the present disclosure;
[0058] Fig.12 A schematic diagram of a conductive structure provided in an embodiment of the present disclosure;
[0059] Fig.13 A schematic flow chart of a method for manufacturing a conductive structure provided in an embodiment of the present disclosure. DETAILED DESCRIPTION
[0060] The technical solution of the present disclosure is described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0061] In the description of the present disclosure, it is necessary to understand that the terms "length", "width", "depth", "up", "down", "outside", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present disclosure.
[0062] 2.5D silicon adapter board refers to the technology that uses silicon as an adapter board and TSV as a line interconnection tool to interconnect memory chips and CPU (Central Processing Unit), GPU (Graphics Processing Unit), SOC (System on Chip) and other chips. The silicon adapter board can shorten the routing length, reduce parasitic capacitance and inductance, thereby reducing signal delay and loss, achieving high-speed computing and data exchange, and can reduce power consumption and improve efficiency. Silicon adapter boards are widely used in CPU, GPU, 5G (5th Generation Mobile Communication Technology, referred to as 5G, the fifth generation of mobile communication technology) and other chip fields.
[0063] Figure 1a A schematic diagram of a semiconductor structure including TSV before heat treatment provided by an embodiment of the present disclosure. Figure 1a As shown, the semiconductor structure is a silicon transfer board, which includes a silicon substrate 10 and a TSV 20 located in the silicon substrate 10, wherein the TSV 20 includes a filling body 21 and a functional layer 22, wherein the functional layer 22 surrounds the sidewall of the filling body 21. The material of the filling body 21 is a metal, such as copper (Cu), tungsten (W), etc., which plays an interconnection role and is used to realize the interconnection between the chips on both sides of the silicon transfer board. One of the functions of the material of the functional layer 22 is to prevent the metal of the filling body 21 from entering the silicon substrate to avoid a negative impact on the isolation performance of the silicon substrate 10.
[0064] In some embodiments, the silicon adapter plate needs to be heat treated, and the heat treatment step is after the step of forming the filling body 21. Since the functional layer 22 and the filling body 21 are made of different materials, during the heat treatment process, the material of the filling body 21 and / or the material of the functional layer 22 may undergo structural changes, such as changes in grain size and crystal orientation, resulting in different thermal expansion coefficients of the materials of the filling body 21 and the functional layer 22. After the heat treatment, the contact interface between the filling body 21 and the functional layer 22 is prone to peeling, resulting in yield loss.
[0065] Figure 1a The enlarged view in FIG. 1 shows a schematic diagram of the structure of the filling body before heat treatment. This embodiment is described by taking the filling body 21 as an example of copper. Figure 1a As shown, the copper just deposited has a small grain size and a uniform size, so that the filling body 21 is isotropic as a whole. The interface contact between the filling body 21 and the functional layer 22 is good.
[0066] Figure 1b A schematic diagram of a semiconductor structure including TSV after heat treatment provided by an embodiment of the present disclosure. Figure 1b As shown, after heat treatment, the grains aggregate and grow, and the amount of grain boundary migration increases, so that the filling body 21 extends in the extension direction (for example Figure 1b The deformation in the Z direction (in the middle) becomes larger, resulting in tearing between the filling body 21 and the functional layer 22, causing the interface between the two to peel off, such as Figure 1b As shown at A in FIG. 1 , the interface between the filling body 21 and the functional layer 22 is partially separated.
[0067] In view of this, an embodiment of the present disclosure provides a method for manufacturing a semiconductor structure, which is used to improve the interface between the filling body and the functional layer. Figure 2 A schematic diagram of a method for manufacturing a semiconductor structure provided by an embodiment of the present disclosure. Figure 2As shown, the manufacturing method includes:
[0068] S110: providing a first substrate;
[0069] S210: etching the first substrate to form a hole in the first substrate;
[0070] S310: forming a first initial auxiliary layer on the sidewall of the hole;
[0071] S410: forming a second initial auxiliary layer on the sidewall of the first initial auxiliary layer;
[0072] S510: After forming the second initial auxiliary layer, filling the holes to form a first conductive matrix;
[0073] S610: heat-treating the second initial auxiliary layer and the first conductive substrate; wherein at least part of the elements in the second initial auxiliary layer migrate to the first conductive substrate to form first microparticles, and the heat-treated second initial auxiliary layer forms a second auxiliary layer.
[0074] Figure 3a to Figure 3h A schematic diagram of a semiconductor structure in the manufacturing process provided by an embodiment of the present disclosure. Figure 3a to Figure 3h The method for manufacturing the semiconductor structure provided by the embodiment of the present disclosure is described in detail. Figure 3a As shown, steps S110 and S210 are performed to provide a first substrate 100 , and to etch the first substrate 100 to form a hole 110 in the first substrate 100 .
[0075] The first substrate 100 may be a semiconductor substrate. For example, the material of the semiconductor substrate may be silicon, germanium, silicon germanium semiconductor, or silicon carbide, or may be silicon on insulator (SOI), germanium on insulator (GOI), silicon germanium on insulator (SGOI), or may be other materials, such as III-V compounds such as gallium arsenide.
[0076] The first substrate 100 has a first surface 101 and a second surface 102 that are arranged opposite to each other. For example, the first surface 101 and the second surface 102 are both perpendicular to the Z direction. Figure 3a As shown, the first substrate 100 is etched from the first surface 101 of the first substrate 100 to form a hole 110 in the first substrate 100. The extension direction of the hole 110 may be perpendicular to the first surface 101. Figure 3a As shown, the hole 110 extends along the Z direction.
[0077] In some embodiments, the hole 110 may extend into the first substrate 100 along a direction perpendicular to the first surface (such as the Z direction), that is, the hole 110 does not penetrate the first substrate 100. In other embodiments, the hole 110 may extend along a direction perpendicular to the first surface to penetrate the first substrate 100. It should be understood that the present disclosure does not limit the extension direction and extension depth of the hole in the first substrate. In different embodiments, it can be set as needed.
[0078] In some embodiments, the process of etching the first substrate 100 may be a wet etching process or a dry etching process. For example, a mask layer may be formed on the first substrate, and the mask layer may be etched to form a pattern corresponding to the hole. Based on the mask layer having the pattern formed, the first substrate may be etched using a wet etching process or a dry etching process to form a hole in the first substrate.
[0079] like Figure 3b and Figure 3c As shown, step S310 is performed to form a first initial auxiliary layer 210 on the sidewall of the hole 110 .
[0080] For example, a deposition process may be used to form the first initial auxiliary layer 210 on the sidewall of the hole 110. The deposition process includes but is not limited to physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), and the like.
[0081] In some embodiments, the first preliminary auxiliary layer 210 may be deposited simultaneously on the sidewall and the bottom of the hole 110 using a deposition process.
[0082] In some embodiments, Figure 3c As shown, the first initial auxiliary layer 210 includes an initial barrier layer 211 and an initial adhesion layer 212 . Step S310 forms the first initial auxiliary layer 210 on the sidewall of the hole 110 , specifically including: forming the initial barrier layer 211 on the sidewall of the hole 110 ; forming the initial adhesion layer 212 on the sidewall of the initial barrier layer 211 .
[0083] For example, Figure 3b As shown, a deposition process may be used to form an initial barrier layer 211 on the sidewall and bottom of the hole 110. Figure 3c As shown, the initial adhesion layer 212 is formed on the surface of the initial barrier layer 211 in the hole 110. That is, the initial adhesion layer 212 is formed on the sidewall and bottom of the hole 110 where the initial barrier layer 211 is formed.
[0084] For example, the initial barrier layer 211 may be made of a metal nitride, which may include at least one of tantalum nitride (TaN) and titanium nitride (TiN). The initial adhesion layer 212 may be made of a metal, which may include at least one of tantalum (Ta), titanium (Ti), nickel (Ni), and cobalt (Co). In some embodiments, the metal in the initial barrier layer 211 is the same as the metal in the initial adhesion layer 212. For example, Figure 3b and Figure 3c In the illustrated embodiment, the composition of the initial barrier layer 211 is tantalum nitride, and the composition of the initial adhesion layer 212 is tantalum.
[0085] It should be understood that in other embodiments, the first initial auxiliary layer 210 may only include the initial barrier layer 211. Figure 3c The step of forming the initial adhesion layer 212 shown may be omitted.
[0086] See also Figure 3d , performing step S410 to form a second initial auxiliary layer 220 on the sidewall of the first initial auxiliary layer 210 .
[0087] For example, a deposition process may be used to form the second initial auxiliary layer 220 on the sidewall of the first initial auxiliary layer 210. The deposition process includes but is not limited to physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), and the like.
[0088] In some embodiments, the second initial auxiliary layer 220 may be formed on the surface of the first initial auxiliary layer 210 exposed in the hole 110 by a deposition process, that is, the second initial auxiliary layer 220 may be formed on the sidewall and bottom of the hole 110 where the first initial auxiliary layer 210 is formed.
[0089] The second initial auxiliary layer includes metal boride. The metal in the metal boride is a transition metal. The transition metal includes at least one of titanium (Ti), aluminum (Al), vanadium (V), and silver (Ag). That is, the second auxiliary layer includes but is not limited to titanium boride, aluminum boride, vanadium boride, and silver boride.
[0090] Next, step S510 is performed to fill the holes 110 to form a first conductive matrix after forming the second initial auxiliary layer 220 .
[0091] See also Figure 3e After forming the second initial auxiliary layer 220 in the hole 110, the remaining space of the hole 110 is filled with a conductive material to form a first conductive matrix 230. For example, Figure 3eAs shown, the conductive material fills the remaining space within the hole 110 .
[0092] For example, a deposition process may be used to form the first conductive matrix 230 in the hole 110. The deposition process includes, but is not limited to, physical vapor deposition (PVD), chemical vapor deposition (CVD), and the like.
[0093] In some embodiments, the composition of the first conductive matrix 230 includes metal, and the metal includes at least one of copper (Cu), tungsten (W), and the like.
[0094] Then, if Figure 3f As shown, step S610 is performed to heat-treat the second initial auxiliary layer 220 and the first conductive substrate 230; wherein at least part of the elements in the second initial auxiliary layer 220 migrate to the first conductive substrate 230 to form the first microparticles 331, and the second initial auxiliary layer 220 after heat treatment forms the second auxiliary layer 320. The conductive pillar 330 includes the first conductive substrate 230 and the first microparticles 331.
[0095] In some embodiments, the step of heat treating the second initial auxiliary layer 220 and the first conductive substrate 230 specifically includes: annealing the first substrate 100 formed with the first initial auxiliary layer 210 , the second initial auxiliary layer 220 and the first conductive substrate.
[0096] When the first substrate 100 is annealed, the elements in the second initial auxiliary layer 220 migrate into the first conductive matrix 230 and combine with the elements in the first conductive matrix 230 to form the first microparticles 331. The interaction between the first microparticles and the dislocations and grain boundaries in the matrix phase of the first conductive matrix limits the aggregation and growth of the grains in the matrix phase, thereby reducing the deformation of the conductive pillar 330, so as to improve the performance of the contact interface between the conductive pillar 330 and the first auxiliary layer 310.
[0097] By way of example, the boron element in the second initial auxiliary layer is combined with the metal element in the first conductive matrix to form the first microparticles. The composition of the first microparticles may be copper boride, tungsten boride, etc. By way of example, part of the boron element in the second initial auxiliary layer may also be recombined with the metal element in the second auxiliary layer in the first conductive matrix to form the first microparticles. At this time, the composition of the first microparticles may be titanium boride, aluminum boride, vanadium boride, silver boride, etc. By way of example, part of the boron element in the second initial auxiliary layer may also be combined with the metal element in the first conductive matrix and the metal element in the second auxiliary layer to form the first microparticles. At this time, the composition of the first microparticles may be a composite boride, such as copper titanium boride, tungsten vanadium boride, etc. It should be understood that the composition of the first microparticles in the first conductive matrix may be any one, any two, or all three as described in the above embodiments.
[0098] The annealed first initial auxiliary layer 210 forms a first auxiliary layer 310. In some embodiments, the elements in the second initial auxiliary layer 220 also migrate to the initial adhesion layer 212. For example, the elements that migrate from the second initial auxiliary layer 220 to the initial adhesion layer 212 combine with the elements of the initial adhesion layer 212 to form second microparticles. The initial adhesion layer 212 after heat treatment forms an adhesion layer 312. The adhesion layer 312 may include an adhesion matrix and second microparticles distributed in the adhesion matrix. The composition of the adhesion matrix is the same as that of the initial adhesion layer 212. The second microparticles in the adhesion layer can limit the aggregation and growth of grains in the adhesion matrix, thereby limiting the deformation of the adhesion layer to improve the performance of the contact interface between the conductive pillar and the adhesion layer.
[0099] For example, the boron element in the second initial auxiliary layer combines with the metal element in the initial adhesion layer to form the second microparticles. The composition of the second microparticles can be tantalum boride, etc. Since the composition of the initial adhesion layer 212 and the first conductive substrate 230 is different, the composition of the second microparticles in the adhesion layer is different from that of the first microparticles in the conductive column.
[0100] In some embodiments, Figure 3e and Figure 3f As shown, part of the boron element and part of the metal element in the second initial auxiliary layer 220 migrate to the first conductive substrate 230 and / or the initial adhesion layer 212, then the semiconductor structure after heat treatment includes a second auxiliary layer 320, and part of the elements of the second auxiliary layer 320 are the same as the elements of the first microparticles. For example, the second auxiliary layer is composed of titanium nitride, and the first microparticles are composed of copper nitride, and they both include boron elements. At this time, the first conductive structure 300 includes a first auxiliary layer 310, a second auxiliary layer 320 and a conductive column 330. Among them, the first auxiliary layer 310 includes a barrier layer 311 and an adhesion layer 312.
[0101] In other embodiments, the boron element in the second initial auxiliary layer 220 can be substantially completely migrated to the first conductive substrate and / or the initial adhesion layer, while the atomic size of the metal element is relatively large and the diffusion rate is relatively slow, resulting in some metal elements being retained after the heat treatment, so that the second auxiliary layer 320 after the heat treatment basically includes the metal element. In this case, the second auxiliary layer 320 can be used as an adhesion layer, and the first initial auxiliary layer 210 can only include the initial barrier layer 211. The first conductive structure 300 obtained by the heat treatment includes the first auxiliary layer 310, the second auxiliary layer 320 and the conductive pillar 330. Among them, the first auxiliary layer 310 includes the barrier layer 311.
[0102] In some other embodiments, during the annealing process, the elements in the second initial auxiliary layer 220 can be substantially completely migrated to the first conductive substrate and / or the initial adhesion layer, so that the semiconductor structure after the heat treatment does not include the second auxiliary layer. The first conductive structure 300 obtained by the heat treatment includes a first auxiliary layer 310 and a conductive column 330. The first auxiliary layer 310 includes a barrier layer 311 and an adhesion layer 312.
[0103] For example, the thickness range of the second initial auxiliary layer 220 is: less than 100nm. In one embodiment, the thickness range of the second initial auxiliary layer 220 is: less than 1nm. The second initial auxiliary layer 220 is set to be thin, so that in the subsequent heat treatment, the elements in the second initial auxiliary layer 220 can be completely diffused into the first conductive substrate and / or the first initial auxiliary layer, and the second auxiliary layer disappears so that the adhesion layer and the first conductive substrate are in direct contact to ensure that the contact interface has good performance. Alternatively, the boron element in the second initial auxiliary layer 220 is basically completely diffused into the first conductive substrate and / or the first initial auxiliary layer, and only the metal element is retained in the second auxiliary layer 320 to form a second auxiliary layer. The second auxiliary layer that roughly only includes metal elements can be used as an adhesion layer to ensure that the contact interface between the barrier layer and the second auxiliary layer, and the second auxiliary layer and the conductive column has good performance. And at this time, the composition and organization of the second auxiliary layer are more uniform and the performance is better.
[0104] It should be understood that during the heat treatment, the metal elements in the second initial auxiliary layer can also diffuse into the first conductive substrate and / or the initial adhesion layer. The metal elements provided by the second initial auxiliary layer can be dissolved in the first conductive substrate and / or the initial adhesion layer (i.e., the adhesion substrate), or a portion of the metal elements can participate in the formation of the first microparticles and / or the second microparticles. For example, the first microparticles are composed of copper titanium boride, and the second microparticles are composed of tantalum titanium boride.
[0105] The initial barrier layer after heat treatment serves as a barrier layer. The barrier layer can effectively block metal elements from entering the first substrate 100, so that the first substrate 100 maintains good isolation performance. The barrier layer substantially does not include boron elements.
[0106] The following is an example in which the first initial auxiliary layer 210 includes an initial barrier layer 211 and an initial adhesion layer 212, the initial barrier layer 211 is composed of tantalum nitride, the initial adhesion layer 212 is composed of tantalum, the second initial auxiliary layer 220 is composed of titanium boride, and the first conductive substrate is composed of copper. It should be noted that this embodiment does not constitute a limitation on the present disclosure.
[0107] During the annealing process of the first substrate 100, the boron element in the titanium boride diffuses into the copper and combines with the copper to precipitate the boron copper compound. The boron copper compound is the second phase particle in the copper matrix phase. The second phase particle interacts with the grain boundary of the copper grain to limit the growth of the copper grain. During the annealing process, the titanium element will also diffuse into the copper and at least partially dissolve in the copper, and a part of the titanium element may also exist in the second phase particles. The boron copper compound is generated during high temperature annealing and migrates to the copper grain boundary. The boron copper compound at the grain boundary has a limiting effect on the growth of the grains and can limit the aggregation of the grains to reduce the probability of peeling at the copper-tantalum interface.
[0108] In addition, the boron element in titanium boride will also diffuse into tantalum and combine with tantalum to precipitate boron tantalum compounds. The boron tantalum compounds are second-phase particles in the tantalum matrix phase, and the second-phase particles will also limit the growth of tantalum grains. Titanium may also diffuse into tantalum and partially dissolve in tantalum. After high-temperature annealing, boron tantalum compounds are pinned to the tantalum grain boundaries to limit grain growth and reduce the probability of peeling at the copper-tantalum interface. During the annealing process, boron and titanium elements basically do not diffuse into tantalum nitride. Tantalum carbide can effectively block metal elements from entering the first substrate 100, so that the first substrate 100 maintains good isolation performance.
[0109] In some embodiments, Figure 3g and Figure 3h As shown, before heat treating the first substrate 100, the manufacturing method further includes:
[0110] A redistribution layer (RDL) 410 is formed on the first surface 101 of the first substrate 100 , and a conductive line 412 in the redistribution layer 410 is in contact with the first conductive structure 300 ;
[0111] Bumps 420 are formed on the second surface 102 of the first substrate 100 , and the bumps 420 are in contact with the first conductive structure 300 .
[0112] The present disclosure does not limit the order of forming the redistribution layer, the bump, and the first conductive structure. For example, the order of forming the first conductive structure, the redistribution layer, and the bump can be followed; or the order of forming the bump, the first conductive structure, and the redistribution layer can be followed. The following embodiments of the present disclosure are described by taking the sequential formation of the first conductive structure, the redistribution layer, and the bump as an example. It should be understood that this embodiment does not constitute a limitation on the present disclosure.
[0113] See also Figure 3g A redistribution layer 410 is formed on the first surface 101 of the first substrate 100, the redistribution layer 410 includes a dielectric layer 411 and at least one conductive line layer located in the dielectric layer 411, the conductive line layer includes at least one conductive line 412, and the conductive line 412 is connected to the first conductive structure 300. Here, the conductive line is connected to the first conductive structure means that they are electrically connected, and current can flow between the conductive line and the first conductive structure.
[0114] In addition, the redistribution layer may further include a conductive via 413, which contacts the conductive wire of the adjacent conductive wire layer to connect the conductive wires in the adjacent conductive wire layer. The conductive via 413 may also contact the conductive wire 412 and the first conductive structure 300 to connect the conductive wire and the first conductive structure.
[0115] like Figure 3h As shown, in some embodiments, the hole 110 in the first substrate 100 does not penetrate the first substrate 100. The bump 420 is formed on the second surface 102 of the first substrate 100, specifically including:
[0116] Thinning the first substrate 100 from the second surface 102 of the first substrate 100 until the first conductive structure 300 is exposed;
[0117] The bumps 420 are formed on the second surface 102 of the thinned first substrate 100 , wherein the bumps 420 are connected to the first conductive structure 300 .
[0118] For example, the first substrate 100 may be thinned to expose the first auxiliary layer 310, or the first substrate 100 may be thinned to expose the conductive pillar 330. Figure 3h As shown. Afterwards, a bump 420 is formed on the second surface 102 of the thinned first substrate 100. By way of example, the bump 420 may contact the first conductive structure 300 to achieve connection.
[0119] In some embodiments, heat treatment is performed on the first substrate 100, including heat treatment of the redistribution layer 410 and the first substrate 100. The heat treatment can increase the density of the conductive lines in the redistribution layer to improve the electrical properties of the conductive lines.
[0120] In some other embodiments, the first substrate 100 is subjected to a heat treatment, including: the redistribution layer 410 , the first substrate 100 , and the bump 420 are subjected to a heat treatment.
[0121] The semiconductor structure provided in this embodiment can be a silicon adapter, and the heat treatment step of the silicon adapter is performed after the TSV (i.e., the first conductive structure 300) and the redistribution layer are formed. Heat treatment of the silicon adapter can increase the density of the conductive wires in the redistribution layer to improve the electrical properties of the conductive wires, such as reducing the resistance of the conductive wires. In the embodiment of the present disclosure, based on the heat treatment step that already exists in the original process, a second initial auxiliary layer is deposited between the conductive substrate and the first initial auxiliary layer. During the heat treatment process, the elements in the second initial auxiliary layer enter the conductive substrate and / or the first initial auxiliary layer, so that microparticles are formed in the conductive substrate and / or the first initial auxiliary layer, reducing the deformation of the conductive column and / or the first auxiliary layer during the heat treatment, thereby improving the problem of peeling of the conductive column and the first auxiliary layer after heat treatment, and improving the product yield. Furthermore, in the embodiment of the present disclosure, the elements for forming the microparticles are provided by depositing a second initial auxiliary layer, and the microparticles are not formed by changing the deposition process of the first initial auxiliary layer or the conductive substrate. This can reduce the impact on the deposition steps of the first initial auxiliary layer and the conductive substrate in the original process, shorten the verification time and cost, and ensure product yield.
[0122] Figure 4 A schematic diagram of a semiconductor structure provided by an embodiment of the present disclosure, such as Figure 4 As shown, the semiconductor structure includes: a first substrate 100 and a first conductive structure 300, the first conductive structure 300 is located in the first substrate 100; the first conductive structure 300 includes a conductive column 330, and a first auxiliary layer 310 arranged around the side wall of the conductive column 330, wherein the conductive column 330 includes a first conductive matrix 230, and first microparticles 331 distributed in the first conductive matrix 230, and at least some elements of the first microparticles 331 are different from the elements of the first conductive matrix 230.
[0123] Here, the essence of the first microparticles 331 is the second phase particles, which are relative to the matrix phase of the first conductive substrate 230. The essence of grain growth is the migration of grain boundaries. The interaction between the second phase particles and the dislocations and grain boundaries in the matrix phase can significantly hinder the migration of the grain boundaries of the matrix phase. This effect is called the "pinning" effect of the insoluble second phase particles. During the heat treatment process, the pinning effect of the first microparticles can be used to limit the growth of the grains of the first conductive substrate at high temperatures to reduce the overall deformation of the first conductive substrate, that is, to reduce the deformation of the conductive column, thereby reducing the probability of peeling at the interface between the conductive column and the first auxiliary layer and improving the yield of the product.
[0124] In some embodiments, Figure 4 As shown, in the conductive column after heat treatment, the first microparticles 331 are relatively evenly distributed in the first conductive matrix 230 , wherein at least a portion of the first microparticles 331 are pinned at the grain boundaries of the first conductive matrix 230 to limit the grain growth of the first conductive matrix 230 .
[0125] At least part of the elements of the first microparticles 331 in the conductive column are different from the elements of the first conductive matrix 230. In other words, the first microparticles 331 are formed by the elements in the first conductive matrix 230 and other foreign elements. It should be understood that the elements of the first conductive matrix refer to the elements of the matrix phase, excluding the solid solution elements dissolved in the matrix phase.
[0126] The elements of the first microparticles 331 are different from the elements of the matrix phase of the first auxiliary layer. It can be understood that the elements forming the first microparticles 331 are not provided by the matrix phase of the first auxiliary layer. That is, the matrix phase of the first auxiliary layer does not provide the elements used to form the first microparticles 331 to the first conductive matrix 230.
[0127] In some embodiments, the source of other foreign elements is the second initial auxiliary layer 220. The second initial auxiliary layer is located between the first initial auxiliary layer and the first conductive matrix 230. During the heat treatment process, the elements in the second initial auxiliary layer diffuse into the first conductive matrix. Among them, some elements provided by the second initial auxiliary layer can be combined with elements in the first conductive matrix to form first microparticles.
[0128] In some embodiments, the first conductive substrate comprises metal, including but not limited to copper and tungsten. The second initial auxiliary layer comprises metal boride, including but not limited to titanium boride, aluminum boride, vanadium boride, and silver boride.
[0129] For example, the boron element provided by the second initial auxiliary layer combines with the metal in the first conductive matrix to form first microparticles. The first microparticles include the boron element and the metal element in the first conductive matrix.
[0130] It should be understood that during the heat treatment process, the metal elements and boron elements in the second initial auxiliary layer will diffuse into the first conductive matrix, wherein the metal elements provided by the second initial auxiliary layer may be partially dissolved in the conductive matrix, or may be precipitated together with the boron element and the metal elements in the conductive matrix to form the first microparticles. The composition of the first conductive matrix mentioned above in the present disclosure refers to the composition of the matrix phase of the first conductive matrix, and does not include the metal elements provided by the second initial auxiliary layer fixed in the matrix phase.
[0131] In some embodiments, the first auxiliary layer includes second particles, wherein at least some elements of the second particles are different from elements of the first auxiliary layer. In other words, the second particles are formed by elements in the matrix phase of the first auxiliary layer and other foreign elements.
[0132] For example, the second microparticles have some of the same elements as the first microparticles. The same elements included in the second microparticles and the first microparticles are derived from the second initial auxiliary layer. During the heat treatment process, the second initial auxiliary layer can diffuse elements into the first conductive matrix or diffuse elements into the matrix phase of the first auxiliary layer. The elements diffused into the first auxiliary layer can combine with the elements of the matrix phase of the first auxiliary layer to form the second microparticles.
[0133] The second particles can hinder the growth of the matrix phase grains of the first auxiliary layer to reduce the deformation of the first auxiliary layer during heat treatment, further reduce the probability of peeling at the contact interface between the first auxiliary layer and the conductive column, and thus further improve the product yield.
[0134] In some embodiments, Figure 5 As shown, the first auxiliary layer 310 may include: a blocking layer 311 and an adhesion layer 312 stacked along the radial direction of the conductive column 330, and the adhesion layer 312 is located between the conductive column 330 and the blocking layer 311; wherein the adhesion layer includes an adhesion matrix and second microparticles distributed in the adhesion matrix, and at least some elements of the second microparticles are different from the elements of the adhesion matrix.
[0135] The second microparticles are also second phase particles in essence, and the second phase particles here are relative to the matrix phase of the adhesion matrix. The matrix phase of the above-mentioned second auxiliary layer refers to the matrix phase of the adhesion matrix. It should be understood that the elements of the adhesion matrix here do not include the metal elements provided by the second initial auxiliary layer that are solid-dissolved in the adhesion matrix. The second microparticles in the adhesion layer can reduce the deformation of the adhesion matrix during heat treatment and improve the problem of peeling off at the contact interface between the adhesion layer and the conductive column.
[0136] The barrier layer is used to reduce the probability of metal in the conductive column and the adhesion layer diffusing into the first substrate. The barrier layer can also reduce the probability of metal in the second initial auxiliary layer diffusing into the first substrate, so that the first substrate maintains good isolation performance. For example, there are no microparticles in the barrier layer.
[0137] Illustratively, the composition of the barrier layer includes metal nitride, which includes but is not limited to tantalum nitride (TaN), titanium nitride (TiN), etc. Here, the metal of the barrier layer is different from the metal of the conductive pillar.
[0138] For example, the composition of the adhesion substrate includes metal, including but not limited to tantalum, titanium, cobalt, nickel, etc. For example, the metal of the adhesion substrate is the same as the metal of the barrier layer. For example, if the barrier layer is composed of tantalum nitride, then the metal of the adhesion substrate can be tantalum. The composition of the second microparticles includes boron element and the metal element in the adhesion substrate. The composition of the second microparticles is, for example, boron tantalum compound.
[0139] In some embodiments, if the thickness of the second initial auxiliary layer is relatively thin, the elements in the second initial auxiliary layer may all diffuse into the first conductive substrate and / or the adhesive substrate during the heat treatment process. Figure 5 As shown, after the heat treatment, the second initial auxiliary layer disappears, and the first conductive structure 300 includes a conductive column 330 and a first auxiliary layer 310, and the first auxiliary layer 310 includes a barrier layer 311 and an adhesion layer 312. The conductive column 330 is in direct contact with the adhesion layer 312. The adhesion layer has good adhesion to the conductive column and the barrier layer, so as to improve the interface performance between the adhesion layer and the conductive column, and between the adhesion layer and the barrier layer, and ensure the reliability of the product.
[0140] In some embodiments, Figure 6 As shown, the first conductive structure 300 may further include a conductive column 330, a first auxiliary layer 310 and a second auxiliary layer 320, wherein the first auxiliary layer 310 includes a barrier layer 311 and an adhesion layer 312. The second auxiliary layer 320 includes boron and metal elements. The adhesion layer 312 contacts the second auxiliary layer 320 and the conductive column 330 to improve the performance of multiple contact interfaces in the first conductive structure to ensure the reliability of the product.
[0141] In some embodiments, Figure 7 As shown, the first conductive structure 300 may further include a conductive column 330, a first auxiliary layer 310 and a second auxiliary layer 320, wherein the first auxiliary layer 310 includes a barrier layer 311. The second auxiliary layer 320 includes a metal element. The second auxiliary layer 320 is used as an adhesion layer. The second auxiliary layer is also used to improve the adhesion between the barrier layer and the conductive column, so that the contact interface between the barrier layer, the adhesion layer and the conductive column is closely contacted and free of peeling, so as to ensure the reliability of the product.
[0142] For example, in this setting, the barrier layer and the second auxiliary layer include the same metal element. For example, if the main component of the second initial auxiliary layer is a boron titanium compound (TiB), then the main component of the barrier layer can be titanium nitride (TiN). When the boron element in the second initial auxiliary layer is basically completely diffused into the first conductive substrate, the main component of the second auxiliary layer is titanium. Titanium has good adhesion to titanium nitride and titanium to copper, so that the contact interface performance in the first conductive structure is good to improve the product yield.
[0143] Figure 8 A schematic diagram of another semiconductor structure provided by an embodiment of the present disclosure. Figure 8 As shown, in some embodiments, the first auxiliary layer 310 may also be located on the bottom surface of the conductive pillar 330, wherein the first auxiliary layer 310 surrounds the portion of the side wall of the conductive pillar 330 and is connected to the portion of the first auxiliary layer 310 located on the bottom surface of the conductive pillar 330. By way of example, the first auxiliary layer 310 is integral. The second auxiliary layer 320 may also be located on the bottom surface of the conductive pillar 330, wherein the second auxiliary layer 320 surrounds the portion of the side wall of the conductive pillar 330 and is connected to the portion of the second auxiliary layer 320 located on the bottom surface of the conductive pillar 330. By way of example, the second auxiliary layer 320 is integral.
[0144] In some embodiments, the semiconductor structure is a silicon interposer. Figure 3h As shown, the first substrate 100 is a silicon base in a silicon adapter. The silicon base has a first surface 101 and a second surface 102 arranged opposite to each other, and the first conductive structure extends along a direction perpendicular to the first surface 101 and penetrates the silicon base. For example, the first surface 101 and the second surface 102 of the silicon base are both perpendicular to the Z direction, and the first conductive structure extends along the Z direction and penetrates the silicon base.
[0145] The silicon transfer board further includes: a redistribution layer 410 and a bump 420, the redistribution layer 410 is located on the first surface 101 of the silicon substrate and contacts the first conductive structure 300, and the bump 420 is located on the second surface 102 of the silicon substrate and contacts the first conductive structure 300. By way of example, the redistribution layer 410 includes a dielectric layer 411 and at least one conductive wire layer located in the dielectric layer 411, and the conductive wire layer includes at least one conductive wire 412.
[0146] The silicon adapter board can carry multiple chips and realize the interconnection between chips. Among them, the redistribution layer 410 can realize a high-density interconnection structure, reduce the delay and power consumption of signal transmission, and improve the working performance of the circuit. The silicon substrate and the chip both use silicon as the substrate material, and the mismatch of the thermal expansion coefficient between the two is small, the thermal stress borne by the chip is reduced, and the reliability is improved. The bump 420 can be connected to the packaging substrate. The chip is connected to the redistribution layer 410 on the silicon adapter board, and then connected to the packaging substrate through TSV (that is, the first conductive structure 300) and the bump 420 on the second surface 102.
[0147] In the silicon transfer board provided in this embodiment, the performance of multiple contact interfaces in the TSV is good, and the yield of the silicon transfer board can be improved.
[0148] In the semiconductor field, transistors are an important device with multiple functions such as amplification, switching, rectification, and voltage regulation. IGBT (Insulated Gate Bipolar Transistor) is a type of transistor and a voltage-controlled device. It is a composite power semiconductor device composed of BJT (Bipolar Junction Transistor, also known as triode) and MOSFET (Metal Oxide Semiconductor Field Effect Transistor), and is an important branch of discrete devices in the semiconductor field. In some embodiments, IGBT is manufactured based on wafers. Specifically, an N source region, a P emitter region, an N base region, an N buffer region, and a P collector region are formed on the front side of the wafer by doping, and a composite metal layer is deposited on the back side of the wafer as a collector.
[0149] In the process of depositing metal on the back of the wafer, after multiple layers of metal are stacked, in order to make the metal X closest to the wafer fully contact with silicon (the component of the wafer) to form SiX alloy (that is, metal silicide) and reduce contact resistance, heat treatment can be used to accelerate the mutual diffusion of metal X and silicon so that they can quickly and fully contact to form SiX alloy. However, during the heat treatment process, metal grains aggregate, which will make the color of the back of the IGBT device uneven, and different areas will show different colors, affecting the quality of shipment.
[0150] Based on this, the present disclosure provides another method for manufacturing a semiconductor structure. Fig. 9 A schematic diagram of a process flow of another method for manufacturing a semiconductor structure provided by an embodiment of the present disclosure is shown in FIG. Fig. 9 As shown, the method for manufacturing the semiconductor structure includes:
[0151] S120: providing a second substrate, and forming a P region and an N region in the second substrate;
[0152] S220: forming a second initial conductive structure on the surface of the second substrate; the second initial conductive structure comprises a plurality of initial conductive layers stacked along the thickness direction of the second substrate and at least one third initial auxiliary layer, wherein the third initial auxiliary layer is arranged between two adjacent conductive layers or arranged on a side of the initial conductive layer farthest from the second substrate away from the second substrate;
[0153] S320: performing heat treatment on the second substrate and the second conductive structure, wherein at least part of the elements in the third initial auxiliary layer migrate to the adjacent conductive layer to form third microparticles.
[0154] Figures 10a to 10c A schematic diagram of a structure of another semiconductor structure in a manufacturing process provided by an embodiment of the present disclosure is shown in FIG. Fig.10aAs shown, step S120 is performed to provide a second substrate 500 and form a P region and an N region in the second substrate.
[0155] The second substrate 500 may be a semiconductor substrate. For example, the material of the semiconductor substrate may be silicon, germanium, silicon germanium semiconductor, silicon carbide, etc., or may be silicon on insulator (SOI), germanium on insulator (GOI), silicon germanium on insulator (SGOI), etc.
[0156] The second substrate 500 has a third surface 501 and a fourth surface 502 that are arranged opposite to each other. For example, the third surface 501 and the fourth surface 502 are both perpendicular to the Z direction. Fig.10a As shown, the second substrate 500 is doped from the third surface 501 of the second substrate 500 to form a P region and / or an N region. The undoped second substrate 500 itself may also include a P region or an N region. These P region rings and N regions are used to form PN junctions, PNP transistors, NPN transistors, MOSFETs (Metal-Oxide-Semiconductor Field-EffectTransistors), GTRs (Giant Transistors), GTOs (Gate Turn-Offs), BJTs (Bipolar Junction Transistors), IGBTs and other devices.
[0157] Next, step S220 is performed to form a second initial conductive structure on the surface of the second substrate; the second initial conductive structure includes a plurality of initial conductive layers stacked along the thickness direction of the second substrate and at least one third initial auxiliary layer, and the third initial auxiliary layer is arranged between two adjacent initial conductive layers or on the side of the initial conductive layer farthest from the second substrate away from the second substrate.
[0158] For example, Fig.10b As shown, a second initial conductive structure 600 is formed on the fourth surface 502 of the second substrate 500. The second initial conductive structure 600 contacts the P region or the N region in the second substrate and serves as an electrode. The second initial conductive structure 600 includes a first conductive structure 600 extending in the thickness direction of the second substrate (i.e., Fig.10b The first embodiment of the present invention comprises a plurality of initial conductive layers 610 stacked in a stacked manner (in the Z direction) and a third initial auxiliary layer 620. The third initial auxiliary layer 620 is not disposed between the second substrate 500 and the initial conductive layer 610 closest to the second substrate, and the third initial auxiliary layer 620 may be disposed between two adjacent initial conductive layers 610, or on a side of the initial conductive layer 610 farthest from the second substrate away from the second substrate.
[0159] The initial conductive layer 610 includes metals, including but not limited to copper, tungsten, silver, tantalum, titanium, aluminum, nickel, cobalt, vanadium, etc. The components of two adjacent initial conductive layers 610 are different.
[0160] In some embodiments, the semiconductor structure may be an IGBT. By way of example, the number of initial conductive layers is 5, and the components of the multiple initial conductive layers are aluminum, titanium, nickel, vanadium, and silver (Al / Ti / Ni / V / Ag) in the direction away from the second substrate. It should be understood that the components of the back conductive layer may be different in different devices, and the present disclosure is not limited thereto.
[0161] The third initial auxiliary layer 620 includes metal boride, and the metal in the metal boride is a transition metal. The transition metal may include but is not limited to titanium (Ti), aluminum (Al), vanadium (V), and silver (Ag). That is, the third initial auxiliary layer 620 includes but is not limited to titanium boride, aluminum boride, vanadium boride, and silver boride.
[0162] Next, step S320 is performed to heat-treat the second substrate and the second initial conductive structure, wherein at least part of the elements in the third initial auxiliary layer 620 migrate to the adjacent initial conductive layer to form third particles, and the initial conductive layer 610 after heat treatment forms a conductive layer.
[0163] Illustratively, heat treating the second substrate and the second initial conductive structure includes: annealing the second substrate and the second initial conductive structure.
[0164] The purpose of heat treating the second substrate and the second initial conductive structure is to make the metal X closest to the second substrate fully contact with the second substrate (such as silicon Si) to form a SiX alloy and reduce the contact resistance. It is also beneficial to the metal densification of the initial conductive layer 610. However, during the heat treatment process, the metal grains may abnormally aggregate to form coarse columnar crystals. These coarse columnar crystals will cause obvious anisotropy of the metal, reduce the strength, toughness, damage tolerance and fatigue performance of the metal, and also cause the second conductive structure as a whole to have uneven color, affecting the quality of shipment.
[0165] The manufacturing method provided by the embodiment of the present disclosure utilizes the third initial auxiliary layer 620 to provide some elements, which are combined with the metal in the initial conductive layer 610 to form third microparticles, and the pinning effect is used to limit the grain growth of the metal, which can ensure the isotropy inside the metal to ensure that the conductive layer has good performance. And after the grains are refined by the third microparticles, the problem of uneven color on the back of the device caused by the aggregation of metal grains can be improved, and the quality of product shipment can be guaranteed. In addition, the embodiment of the present disclosure does not directly adjust the composition of the initial conductive layer 610, but uses the third initial auxiliary layer 620 to provide foreign elements to form third microparticles, which makes little change to the existing back gold process (the process of depositing metal on the back), can save verification costs and time, and ensure product quality.
[0166] For example, when the second initial conductive structure is heat treated, the boron element in the third initial auxiliary layer 620 migrates to the adjacent initial conductive layer 610 and forms third microparticles with the metal in the initial conductive layer 610. The components of the third microparticles include: boron element and the metal in the initial conductive layer 610. The components of the third microparticles are, for example, boron copper compounds, boron tungsten compounds, boron cobalt compounds, etc. It should be understood that the metal elements in the third initial auxiliary layer 620 may also migrate to the initial conductive layer 610, some of the metal elements may be dissolved in the initial conductive layer 610, and some of the metal elements may participate in the formation of the third microparticles.
[0167] The initial conductive layer 610 after heat treatment forms a conductive layer 710. Fig.10c As shown, the conductive layer 710 includes a second conductive matrix 711 and third particles 712 distributed in the second conductive matrix. At least part of the elements of the third particles are different from those of the second conductive matrix. Here, the composition of the second conductive matrix is the same as that of the initial conductive layer.
[0168] In some embodiments, Fig.10b and Fig.10c As shown, part of the boron element and part of the metal element in the third initial auxiliary layer 620 migrate to the initial conductive layer 610, and then the semiconductor structure after heat treatment includes a third auxiliary layer 720, and part of the elements of the third auxiliary layer 720 are the same as the elements of the third microparticles. For example, the composition of the third auxiliary layer is titanium nitride, and the composition of the third microparticles is copper nitride, and they both include boron elements. At this time, the second conductive structure 700 includes multiple conductive layers 710 and a third auxiliary layer 720.
[0169] In other embodiments, the boron element in the third initial auxiliary layer 620 can be substantially completely migrated to the initial conductive layer, so that the third auxiliary layer 720 after heat treatment substantially includes metal elements. In this case, the third auxiliary layer 720 can be used as a conductive layer. The second conductive structure 700 obtained by heat treatment includes a plurality of conductive layers stacked.
[0170] In some other embodiments, during the heat treatment, the elements in the third initial auxiliary layer 620 can be substantially completely migrated to the initial conductive layer, so that the semiconductor structure after the heat treatment does not include the third auxiliary layer. The second conductive structure 700 obtained by the heat treatment includes a plurality of conductive layers stacked.
[0171] In some embodiments, in the second initial conductive structure, a third initial auxiliary layer is disposed between each two adjacent initial conductive layers so that each conductive layer includes third particles to hinder the grain growth of all conductive layers and better improve the problem of uneven color on the back of the device.
[0172] For example, the thickness of the third initial auxiliary layer 620 is in the range of less than 100 nm. In a specific embodiment, the thickness of the third initial auxiliary layer 620 is in the range of less than 1 nm. The third initial auxiliary layer 620 is set to be thin, so that in the subsequent heat treatment, the elements in the third initial auxiliary layer 620 can be completely diffused into the initial conductive layer, so that the third initial auxiliary layer disappears; or, the boron element in the third initial auxiliary layer is basically completely diffused into the initial conductive layer, and only the metal element is retained in the third initial auxiliary layer 620 to form a third auxiliary layer 720. In the second conductive structure at this time, the composition and organization of basically each conductive layer are relatively uniform, and the performance is better.
[0173] The present disclosure also provides a semiconductor structure, such as Fig.11 As shown, the semiconductor structure includes:
[0174] A second substrate 500, in which a P region and an N region are formed;
[0175] The second conductive structure is in contact with the P region or the N region. The second conductive structure includes multiple conductive layers. At least one conductive layer includes a second conductive matrix and third particles distributed in the second conductive matrix. At least some elements of the third particles are different from those of the second conductive matrix.
[0176] Here, the third particles are actually second-phase particles, which are relative to the matrix phase of the second conductive matrix. During the heat treatment process, the pinning effect of the third particles can limit the growth of the grains of the second conductive matrix at high temperatures, improve the uneven color of the back of the device caused by the aggregation of the matrix phase grains of the second conductive matrix, and thus ensure the shipment quality of the product.
[0177] In some embodiments, Fig.11As shown, in the conductive column after heat treatment, the third particles 712 are relatively evenly distributed in the second conductive matrix 711 , wherein at least a portion of the third particles 712 are pinned at the grain boundaries of the second conductive matrix 711 to limit the grain growth of the second conductive matrix 711 .
[0178] At least some of the elements of the third microparticles 712 in the conductive layer are different from the elements of the second conductive matrix 711. In other words, the third microparticles 712 are formed by the elements in the second conductive matrix 711 and other foreign elements. The composition of the third microparticles is different from that of the second conductive matrix, which means that at least some of the elements in the composition of the third microparticles are different from those of the second conductive matrix. That is, the third microparticles are not completely formed by the elements provided by the second conductive matrix, and at least some of the elements in the third microparticles may not come from the second conductive matrix, but may come from outside the second conductive matrix.
[0179] For example, the composition of the second conductive matrix includes metal, including but not limited to copper, tungsten, silver, tantalum, titanium, aluminum, nickel, cobalt, etc. The composition of two adjacent second conductive matrices is different. The composition of the third microparticles includes: boron element and the metal in the second conductive matrix. The composition of the third microparticles is, for example, boron copper compound, boron tungsten compound, boron cobalt compound, etc.
[0180] In some embodiments, Fig.10c As shown, the semiconductor structure further includes a third auxiliary layer 720, which is disposed between two adjacent conductive layers 710 or on a side of the conductive layer farthest from the second substrate away from the second substrate. The third auxiliary layer is used to provide elements for forming third particles to the conductive layer in contact with the third auxiliary layer.
[0181] In some embodiments, if the thickness of the third initial auxiliary layer is relatively thin, the elements in the third initial auxiliary layer may all diffuse into the initial conductive layer during the heat treatment process. Fig.11 As shown, after the heat treatment, the third initial auxiliary layer disappears, and the second conductive structure 700 includes a plurality of conductive layers stacked together.
[0182] In other embodiments, Fig.10c As shown, the third initial auxiliary layer does not disappear after the heat treatment and forms a third auxiliary layer 720. For example, the composition of the third auxiliary layer 720 may include metal borides, and the metal borides include but are not limited to: titanium boride, aluminum boride, vanadium boride, and silver boride. The second conductive structure 700 includes a plurality of conductive layers 710 and a third auxiliary layer 720 stacked.
[0183] As another example, the third auxiliary layer 720 may also only include metal. In this case, the third auxiliary layer may serve as a conductive layer.
[0184] In some embodiments, a third auxiliary layer may be disposed between every two adjacent conductive layers. It should be noted that the third auxiliary layer is not disposed between the second substrate and the conductive layer closest to the second substrate to prevent affecting the formation of metal silicide.
[0185] In the semiconductor structure provided by the embodiment of the present disclosure, the second conductive structure includes a second conductive substrate and third microparticles distributed in the second conductive substrate. The third microparticles can be pinned at the grain boundaries of the second conductive substrate to limit the grain growth of the second conductive substrate, so as to improve the performance of the conductive layer and improve the problem of uneven color on the back of the semiconductor device, thereby improving the shipment quality of the device.
[0186] In some embodiments, the semiconductor structure may be an insulated gate bipolar transistor, wherein the second conductive structure is a collector of the insulated gate bipolar transistor.
[0187] The embodiment of the present disclosure also provides a conductive structure, Fig.12 A schematic diagram of a conductive structure provided in an embodiment of the present disclosure, such as Fig.12 As shown, the conductive structure 800 includes a conductive layer 810 and an auxiliary layer 820 which are stacked;
[0188] The conductive layer 810 includes a conductive matrix and microparticles distributed in the conductive matrix; the auxiliary layer 820 is used to provide at least part of the elements forming the microparticles.
[0189] Here, the microparticles are actually second phase particles, which are relative to the matrix phase of the conductive matrix. The microparticles can be pinned at the grain boundaries of the grains in the conductive matrix, hindering the growth of the grains of the conductive matrix during the heat treatment process, thereby improving the performance of the conductive matrix.
[0190] In some embodiments, the composition of the conductive matrix includes a metal, including but not limited to copper, tungsten, silver, tantalum, titanium, aluminum, nickel, cobalt, vanadium, and the like.
[0191] In some embodiments, the auxiliary layer comprises: metal boride. The metal in the metal boride is a transition metal. The transition metal includes but is not limited to titanium (Ti), aluminum (Al), vanadium (V), and silver (Ag). That is, the auxiliary layer comprises but is not limited to: titanium boride, aluminum boride, vanadium boride, and silver boride.
[0192] The microparticles include boron element and metal elements in the conductive matrix. The components of the microparticles are, for example, boron copper compound, boron tungsten compound, boron cobalt compound, and the like.
[0193] In other embodiments, the boron element in the initial auxiliary layer is substantially completely diffused into the conductive substrate, and the auxiliary layer comprises metals, including but not limited to titanium, aluminum, vanadium, and silver.
[0194] One of the application scenarios of the conductive structure described in the embodiment of the present disclosure is the above-mentioned first conductive structure, wherein the conductive layer exists in the form of a conductive column. The second application scenario of the conductive structure described in the embodiment of the present disclosure is the second conductive structure. For more descriptions of the conductive structure described in the embodiment of the present disclosure, please refer to the above-mentioned first conductive structure and second conductive structure, which will not be repeated here. It should be understood that the conductive structure described in the embodiment of the present disclosure can also be applied to more devices, and the present disclosure does not limit this. In short, the conductive structure provided in the embodiment of the present disclosure can hinder the aggregation and growth of grains of the conductive layer, thereby improving the performance of the conductive layer.
[0195] The present disclosure also provides a method for manufacturing a conductive structure. Fig.13 A schematic diagram of a process for manufacturing a conductive structure provided in an embodiment of the present disclosure, such as Fig.13 As shown, the manufacturing method includes:
[0196] S130: forming a conductive substrate and an initial auxiliary layer stacked in layers;
[0197] S230: thermally treating the conductive substrate and the initial auxiliary layer, wherein at least part of the elements in the initial auxiliary layer migrate to the conductive substrate to form microparticles.
[0198] The conductive layer includes a conductive matrix and fine particles distributed in the conductive matrix.
[0199] In some embodiments, the composition of the conductive matrix includes a metal, including but not limited to copper, tungsten, silver, tantalum, titanium, aluminum, nickel, cobalt, vanadium, and the like.
[0200] The components of the initial auxiliary layer include: metal boride. The metal in the metal boride is a transition metal. The transition metal includes but is not limited to titanium (Ti), aluminum (Al), vanadium (V), and silver (Ag). That is, the components of the initial auxiliary layer include but are not limited to: titanium boride, aluminum boride, vanadium boride, and silver boride.
[0201] In some embodiments, the elements in the initial auxiliary layer may completely migrate into the conductive matrix during the heat treatment, so that the conductive structure after the heat treatment does not include the auxiliary layer. The conductive structure only includes the conductive layer.
[0202] In other embodiments, the boron element in the initial auxiliary layer migrates into the conductive matrix during the heat treatment and forms microparticles together with the metal element in the conductive matrix. The initial auxiliary layer after the heat treatment forms an auxiliary layer, and the auxiliary layer only includes the metal element. The conductive structure includes the conductive layer and the auxiliary layer.
[0203] In some other embodiments, part of the boron element and part of the metal element in the initial auxiliary layer migrate into the conductive matrix during the heat treatment. The initial auxiliary layer after the heat treatment forms an auxiliary layer, and the auxiliary layer includes boron element and metal element. The conductive structure includes a conductive layer and an auxiliary layer.
[0204] The application scenarios of the manufacturing method of the conductive structure described in the embodiment of the present disclosure include the manufacturing method of the first conductive structure and the manufacturing method of the second conductive structure mentioned above. For more descriptions of the manufacturing method of the conductive structure described in the embodiment of the present disclosure, please refer to the manufacturing method of the first conductive structure and the second conductive structure mentioned above, which will not be repeated here. It should be understood that the manufacturing method of the conductive structure described in the embodiment of the present disclosure can also be applied to more devices, and the present disclosure does not limit this. In short, the manufacturing method of the conductive structure provided in the embodiment of the present disclosure can hinder the aggregation and growth of grains of the conductive layer, thereby improving the performance of the conductive layer.
[0205] The above embodiments are merely illustrative of the principles and effects of the present disclosure, and are not intended to limit the present disclosure. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present disclosure. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present disclosure shall still be covered by the claims of the present disclosure.
Claims
1. A semiconductor structure, It is characterized in that The semiconductor structure comprises: a first substrate; A first conductive structure is located in the first substrate; the first conductive structure includes a conductive column and a first auxiliary layer arranged around the side wall of the conductive column, wherein the conductive column includes a first conductive matrix and first microparticles distributed in the first conductive matrix, and at least some elements of the first microparticles are different from elements of the first conductive matrix.
2. The semiconductor structure according to claim 1, It is characterized in that The first conductive structure further includes: The second auxiliary layer is located between the conductive column and the first auxiliary layer, wherein the second auxiliary layer is used to provide at least part of the elements forming the first microparticles.
3. The semiconductor structure according to claim 2, It is characterized in that The components of the second auxiliary layer include: metal boride; Wherein, the first microparticles include boron element.
4. The semiconductor structure according to claim 1, It is characterized in that The first conductive matrix comprises at least one of the following components: copper and tungsten.
5. The semiconductor structure according to claim 1, It is characterized in that The first auxiliary layer comprises: A barrier layer and an adhesion layer are stacked along the radial direction of the conductive column, and the adhesion layer is located between the conductive column and the barrier layer; wherein, The adhesive layer includes an adhesive matrix and second fine particles distributed in the adhesive matrix, wherein at least part of elements of the second fine particles are different from elements of the adhesive matrix.
6. The semiconductor structure according to claim 1, It is characterized in that The first substrate is a silicon substrate having a first surface and a second surface opposite to each other, and the first conductive structure extends along a direction perpendicular to the first surface and penetrates the silicon substrate; The semiconductor structure further comprises: a redistribution layer, located on the first surface of the silicon substrate and connected to the first conductive structure; The bump is located on the second surface of the silicon substrate and connected to the first conductive structure.
7. A method for manufacturing a semiconductor structure, It is characterized in that The manufacturing method comprises: providing a first substrate; etching the first substrate to form a hole in the first substrate; forming a first initial auxiliary layer on the sidewall of the hole; forming a second initial auxiliary layer on a sidewall of the first initial auxiliary layer; After forming the second initial auxiliary layer, filling the hole to form a first conductive matrix; The second initial auxiliary layer and the conductive substrate are subjected to a heat treatment, wherein at least part of the elements in the second initial auxiliary layer migrate to the first conductive substrate to form first microparticles.
8. The method for manufacturing a semiconductor structure according to claim 7, It is characterized in that The heat treatment of the second initial auxiliary layer and the conductive substrate comprises: The first substrate formed with the first initial auxiliary layer, the second initial auxiliary layer and the first conductive base is annealed; wherein the first initial auxiliary layer after annealing forms a first auxiliary layer.
9. A semiconductor structure, It is characterized in that The semiconductor structure comprises: A second substrate having a P region and an N region formed therein; A second conductive structure is in contact with the P region or the N region, the second conductive structure includes a plurality of conductive layers, at least one of the conductive layers includes a second conductive matrix, and third microparticles distributed in the second conductive matrix, at least some elements of the third microparticles are different from elements of the second conductive matrix.
10. The semiconductor structure according to claim 9, It is characterized in that The second conductive structure further includes: a third auxiliary layer, the third auxiliary layer being arranged between two adjacent conductive layers or on a side of the conductive layer farthest from the second substrate away from the second substrate; The third auxiliary layer is used to provide an element for forming the third fine particles to the conductive layer in contact with the third auxiliary layer.
11. The semiconductor structure according to claim 10, It is characterized in that The third auxiliary layer is disposed between every two adjacent conductive layers.
12. The semiconductor structure according to claim 10, It is characterized in that The composition of the third auxiliary layer includes: metal boride; Wherein, the third microparticles include boron element.
13. The semiconductor structure according to claim 9, It is characterized in that The semiconductor structure comprises an insulated gate bipolar transistor structure, wherein the second conductive structure is a collector of the insulated gate bipolar transistor structure.
14. A conductive structure, It is characterized in that The conductive structure comprises: a conductive layer and an auxiliary layer stacked in layers; The conductive layer includes a conductive matrix and microparticles distributed in the conductive matrix; The auxiliary layer is used to provide at least part of the elements forming the microparticles.
15. The conductive structure according to claim 14, It is characterized in that The components of the auxiliary layer include: metal boride; Wherein, the microparticles include boron element.
16. A method for manufacturing a conductive structure, It is characterized in that The manufacturing method comprises: forming a conductive substrate and an initial auxiliary layer arranged in a stacked manner; The conductive substrate and the initial auxiliary layer are subjected to a heat treatment, wherein at least part of the elements in the initial auxiliary layer migrate to the conductive substrate to form microparticles.
17. The method for manufacturing a conductive structure according to claim 16, It is characterized in that The thickness of the initial auxiliary layer is less than 100 nm.