Semiconductor element and manufacturing method thereof
Wet etching technology is used to process the recessed sides of semiconductor components, which solves the problems of dry etching damage and thinning of the AlGaN layer thickness, achieves efficient electrode coverage and low contact resistance, and improves the performance of semiconductor components.
Patent Information
- Application Number
- CN202410284549.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-01
AI Technical Summary
In existing semiconductor components, the recessed structure is prone to etching damage when formed by dry etching, and the inclination of the recessed side leads to thinner AlGaN layer thickness and reduced 2DEG concentration. High-precision step coverage is required during electrode formation, but sputtering may damage the semiconductor.
Wet etching technology is used to process the concave sides after dry etching to form sides and platforms with smaller tilt angles to improve electrode coverage and prevent electrode breakage. It is also etched with alkaline solutions such as TMAH aqueous solution to form no etching damage. electrode contact surface.
It effectively reduces the contact resistance of the electrode, prevents electrode disconnection, avoids the decrease in 2DEG layer concentration, and improves the coating of the electrode and the on-resistance performance of the component.
Smart Images

Figure CN118738112A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a semiconductor element and a method for manufacturing the same. Background Art
[0002] A semiconductor device is known which has a heterojunction structure in which a channel layer composed of GaN and a barrier layer composed of AlGaN are sequentially stacked and operates using a two-dimensional electron gas (2DEG) layer formed at a heterojunction interface as a channel.
[0003] In such semiconductor elements, there is a case where a recessed structure is provided so that the electrode can make good contact with the 2DEG layer (for example, Patent Document 1). The recessed structure is a structure in which a groove (recess) having a depth reaching the channel layer is provided in a part of the surface of the barrier layer, so that the heterojunction interface is exposed on the side of the groove, and the electrode is provided along the upper surface, side surface, and bottom surface of the recess. According to such a structure, the electrode is in contact with the 2DEG layer, so that the contact resistance can be reduced.
[0004] Patent Documents 2 and 3 describe HFETs in which two levels of inclination are provided on the side of the recess, and show the following structure: the inclination angle of the recess side changes at the position where the barrier layer is exposed, so that the inclination of the upper side is gentler than the inclination of the lower side. Patent Document 4 also shows a structure in which the inclination angle of the recess side is changed.
[0005] Patent Document 1: Japanese Patent No. 5329606
[0006] Patent Document 2: Japanese Patent Application Publication No. 2012-99542
[0007] Patent Document 3: Japanese Patent No. 5625314
[0008] Patent Document 4: Japanese Patent No. 7057473
[0009] However, since the recess is formed by dry etching, etching damage of the recess is caused, and the etching damage cannot be removed.
[0010] Furthermore, since the side surfaces of the recess are inclined, the substantial thickness of the AlGaN layer becomes thinner, resulting in a decrease in the 2DEG concentration near the recess.
[0011] In addition, when forming an electrode in a recess, in order to prevent the electrode from being disconnected or to prevent the electrode from contacting the 2DEG layer, the electrode needs to be spread over the steps of the recess with high precision. Therefore, as a method for forming the electrode, sputtering with excellent step coverage needs to be selected. However, sputtering may damage the semiconductor. Summary of the invention
[0012] The present invention has been made in view of the above background, and aims to provide a semiconductor device capable of making good contact with a 2DEG layer and a method for manufacturing the same.
[0013] One embodiment of the present invention is a semiconductor element, comprising: a substrate, a channel layer arranged on the above substrate and composed of a group III nitride semiconductor, and a barrier layer arranged on the above channel layer and in contact with the above channel layer and composed of a group III nitride semiconductor with a higher Al composition than the above channel layer, in the above semiconductor element, there are: a recess, which is arranged in a partial area of the surface of the above barrier layer and has a depth reaching the above channel layer; and an electrode, which is arranged to cover along the above recess, and the above recess has: a first side surface, which is a surface that exposes the above barrier layer and is a surface that has an angle with respect to the main surface of the above substrate; a platform, which is a surface connected to the above first side surface and exposes the surface of the above channel layer; and a second side surface, which is a surface connected to the above platform and on which the above channel layer is exposed, and is a surface inclined relative to the main surface of the substrate and whose inclination angle is smaller than that of the above first side surface.
[0014] In addition, another embodiment of the present invention is a method for manufacturing a semiconductor element, the semiconductor element comprising: a substrate, a channel layer disposed on the substrate and composed of a group III nitride semiconductor, and a barrier layer disposed on the channel layer and in contact with the channel layer and composed of a group III nitride semiconductor having a higher Al composition than the channel layer, wherein the method for manufacturing the semiconductor element comprises: a first recess forming step, in which a predetermined area on the surface of the barrier layer is dry-etched to form a first recess having a side surface inclined relative to a main surface of the substrate and a bottom surface deeper than the surface of the channel layer; and a second recess forming step. A process, in which the side of the above-mentioned first recess is wet-etched by an alkaline solution to form a second recess; and an electrode forming process, in which an electrode is formed on the above-mentioned barrier layer in a manner covering the above-mentioned second recess. In the manufacturing method, in the above-mentioned second recess forming process, the above-mentioned barrier layer is wet-etched to form a surface having an angle with respect to the main surface of the above-mentioned substrate, that is, the first side surface, and the surface of the above-mentioned channel layer is exposed to form a platform, and the above-mentioned channel layer is wet-etched to form a surface inclined with respect to the main surface of the above-mentioned substrate and having a smaller inclination angle than the above-mentioned first side surface, that is, the second side surface.
[0015] According to the present invention, the coverage of the electrode with respect to the recess is high, and the electrode can be prevented from being broken. As a result, the contact resistance of the electrode can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a cross-sectional view showing the structure of the semiconductor element in the first embodiment, and is a view showing a cross section perpendicular to the main surface of the substrate.
[0017] Figure 2 This is a cross-sectional view showing an enlarged depressed portion of the semiconductor element in the first embodiment.
[0018] Figure 3 It is a diagram showing a planar pattern of an electrode.
[0019] Figure 4 It is a diagram showing the manufacturing process of the semiconductor element in the first embodiment.
[0020] Figure 5 It is a diagram showing the manufacturing process of the semiconductor element in the first embodiment.
[0021] Figure 6 It is a diagram showing the manufacturing process of the recessed portion of the semiconductor element in the first embodiment.
[0022] Figure 7 This is a graph comparing contact resistivity.
[0023] Figure 8 It is a graph showing the distribution of the on-resistance of each semiconductor element.
[0024] Fig. 9 This is a cross-sectional SEM image of the depression.
[0025] Description of Reference Numerals
[0026] 10...substrate; 11...buffer layer; 12...channel layer; 13...barrier layer; 14...undoped layer; 15...p layer; 16...gate electrode; 17...source electrode; 18...drain electrode; 19...2DEG layer; 20...recess. DETAILED DESCRIPTION
[0027] A semiconductor element comprises: a substrate, a channel layer arranged on the substrate and composed of a Group III nitride semiconductor, and a barrier layer arranged on the channel layer and in contact with the channel layer and composed of a Group III nitride semiconductor having a higher Al composition than the channel layer. In the semiconductor element, there is: a recess arranged in a partial area of the surface of the barrier layer and having a depth reaching the channel layer; and an electrode arranged to cover along the recess, the recess having: a first side surface, which is a surface that exposes the barrier layer and is a surface that has an angle relative to the main surface of the substrate; a platform, which is a surface connected to the first side surface and exposes the surface of the channel layer; and a second side surface, which is a surface connected to the platform and exposes the channel layer, and is a surface that is inclined relative to the main surface of the substrate and has a smaller inclination angle than the first side surface.
[0028] The width of the terrace may be 100 nm or more, which can improve the coverage of the electrode and better prevent the electrode from being broken.
[0029] Alternatively, the first side surface may be a surface having an angle of 80 degrees or more and 90 degrees or less relative to the main surface of the substrate. Alternatively, the first side surface may be an m-plane of the barrier layer. This can prevent the 2DEG concentration of the 2DEG layer from decreasing near the recessed side surface.
[0030] A method for manufacturing a semiconductor element, the semiconductor element comprising: a substrate, a channel layer disposed on the substrate and composed of a group III nitride semiconductor, and a barrier layer disposed on the channel layer and in contact with the channel layer and composed of a group III nitride semiconductor having a higher Al composition than the channel layer, wherein the method comprises: a first recess forming step, in which a predetermined area on the surface of the barrier layer is dry-etched to form a first recess having a side surface inclined relative to a main surface of the substrate and a bottom surface deeper than the surface of the channel layer; and a second recess forming step. A process, in which the side of the first recess is wet-etched by an alkaline solution to form a second recess; and an electrode forming process, in which an electrode is formed on the barrier layer in a manner covering the second recess, and further, in the second recess forming process, the barrier layer is wet-etched to form a surface having an angle with respect to the main surface of the substrate, i.e., the first side surface, and the surface of the channel layer is exposed to form a platform, and the channel layer is wet-etched to form a surface inclined with respect to the main surface of the substrate and having a smaller inclination angle than the first side surface, i.e., the second side surface.
[0031] In the second recess forming step, the terrace may be formed so that the terrace width becomes 100 nm or more. The coverage of the electrode can be improved, and the electrode can be prevented from being broken.
[0032] Alternatively, in the second recess forming step, the first side surface is formed to have an angle of 80 degrees or more and 90 degrees or less relative to the main surface of the substrate. In addition, in the second recess forming step, the first side surface is formed to be an m-plane. This can prevent the 2DEG concentration of the 2DEG layer from decreasing near the recess side surface. Alternatively, the alkaline solution is a TMAH aqueous solution.
[0033] (Implementation Method 1)
[0034] 1.Structure of semiconductor components
[0035] Figure 1 1 is a cross-sectional view showing the structure of the semiconductor element in the first embodiment, and is a view showing a cross section perpendicular to the main surface of the substrate. The semiconductor element in the first embodiment is a polarization super junction (PSJ) FET, such as Figure 1 As shown, it has a substrate 10, a buffer layer 11, a channel layer 12, a barrier layer 13, an undoped layer 14, a p-layer 15, a gate electrode 16, a source electrode 17, and a drain electrode 18. In addition, Figure 22 is a cross-sectional view showing an enlarged depressed portion of the semiconductor element in Embodiment 1. Figure 3 It is a top view showing an electrode pattern. Figure 3 The AA section in is Figure 1 .
[0036] The substrate 10 is made of sapphire having the c-plane or the a-plane as the main surface. The thickness of the substrate 10 is, for example, 50 μm to 500 μm.
[0037] The channel layer 12 is located on the substrate 10 via the buffer layer 11. The channel layer 12 is made of undoped GaN. The buffer layer 11 is, for example, AlN or GaN grown at a low temperature. The thickness of the channel layer 12 is, for example, 300 nm to 5000 nm.
[0038] The barrier layer 13 is located on the channel layer 12. The barrier layer 13 is composed of undoped AlGaN. The Al composition is 10% to 50%. The channel layer 12 and the barrier layer 13 are hybridized, and a two-dimensional electron gas (2DEG) layer 19 is generated near the interface and in the channel layer 12. The semiconductor element in the first embodiment operates using the 2DEG layer 19 as a channel. The thickness of the barrier layer 13 is, for example, 20nm to 150nm.
[0039] The undoped layer 14 is located in a part of the barrier layer 13 (excluding the region where the source electrode 17 and the drain electrode 18 are formed). The undoped layer 14 is undoped GaN. The barrier layer 13 and the undoped layer 14 are hybridized, and a two-dimensional hole gas (2DHG) layer 22 is generated near the interface and in the undoped layer 14. The 2DHG layer 22 is not a layer that functions as a channel, but a layer that flattens the electric field distribution and improves the withstand voltage. The thickness of the undoped layer 14 is, for example, 10 nm to 1000 nm.
[0040] The p-layer 15 is located in a part of the region above the undoped layer 14 and in the region near the source electrode 17. The p-layer 15 is made of p-GaN. The Mg concentration is, for example, 1×10 17 cm -3 Above and 3×10 20 cm -3 The thickness of the p-layer 15 is, for example, 20 nm to 150 nm. The p-layer 15 may be composed of two layers: a low-concentration p-type layer and a high-concentration p-type layer.
[0041] The gate electrode 16 is located on the p-layer 15. The material of the gate electrode 16 is, for example, Ni / Au.
[0042] The depression 20 is a groove provided in the region where the source electrode 17 and the drain electrode 18 are provided on the surface of the barrier layer 13, and is a groove having a depth reaching the channel layer 12. The depression 20 has a two-step side surface, and has a shape including a side surface 20a that exposes the barrier layer 13, a terrace 20b that is continuous with the lower end of the side surface 20a and exposes the surface of the channel layer 12, a side surface 20c that is continuous with one end of the terrace 20b and exposes the channel layer 12, and a bottom surface 20d that is continuous with the lower end of the side surface 20c and exposes the channel layer 12 and is also a surface deeper than the surface of the channel layer 12.
[0043] The side surface 20a is a surface perpendicular to the main surface of the barrier layer 13, for example, the m-plane of AlGaN. It can also be a surface other than the m-plane, such as the a-plane. In addition, the side surface 20a does not have to be a surface perpendicular to the main surface of the barrier layer 13, and the inclination angle relative to the main surface of the substrate 10 can be larger than that of the side surface 20c. However, it is preferably as close to vertical as possible, for example, it is preferably an angle of more than 80 degrees and less than 90 degrees relative to the main surface of the substrate 10, and vertical is most preferred. The side surface 20a is a surface exposed by wet etching and is a surface without etching damage.
[0044] The terrace 20b is the surface of the channel layer 12 and is the c-plane of GaN. The terrace 20b is a surface exposed by wet etching and is a surface without etching damage. The terrace 20b is vertical and continuous with the side surface 20a.
[0045] The width of the terrace 20b is preferably 100 nm or more. Here, the width of the terrace 20b refers to the width of the terrace 20b in the straight line direction when the shortest straight line connecting the source electrode 17 and the drain electrode 18 is drawn in a plan view. Figure 3 In the case of , it is the width in the direction perpendicular to the stripe-shaped portion. By making the width of the terrace 20b larger than 100nm, the width of the terrace 20b is made sufficiently wide, thereby further improving the coverage of the source electrode 17 and the drain electrode 18 to the recess 20, and preventing the source electrode 17 and the drain electrode 18 from being separated by the step of the recess 20. The width is more preferably larger than 140nm.
[0046] In addition, the width of the terrace 20 b is preferably 1000 nm or less, because the area of the 2DEG layer 19 is reduced due to the increase in the width of the terrace 20 b.
[0047] The side surface 20c has an angle with respect to the main surface of the channel layer 12. This angle is smaller than the angle of the side surface 20a, for example, 40 to 80 degrees with respect to the main surface of the substrate 10. Since the side surface 20c is inclined, the coverage of the source electrode 17 and the drain electrode 18 to the recess 20 can be further improved. The side surface 20c is a surface exposed by wet etching and is a surface without etching damage. The side surface 20c is connected to the platform 20b at an angle. The side surface 20c is, for example, a surface that makes the m-plane inclined.
[0048] The bottom surface 20d is a surface parallel to the main surface of the channel layer 12 and is the c-plane of GaN. The bottom surface 20d is a surface located deeper than the surface of the channel layer 12 (position close to the substrate 10 side) and is a surface exposed by dry etching of the channel layer 12. The bottom surface 20d is connected to the side surface 20c at an angle. The height from the bottom surface 20d to the surface of the channel layer 12 is arbitrary as long as it is greater than 0, for example, it is greater than 10nm.
[0049] The source electrode 17 and the drain electrode 18 are separated and arranged in a predetermined area above the barrier layer 13. In addition, the source electrode 17 and the drain electrode 18 are arranged to cover the recess 20. In other words, they are arranged to be in contact with the side 20a, the terrace 20b, the side 20c, and the bottom 20d of the recess 20. Therefore, the source electrode 17 and the drain electrode 18 are in contact with the 2DEG layer 19 near the corner formed by the side 20a and the terrace 20b of the recess 20. Thus, the contact resistance of the source electrode 17 and the drain electrode 18 is reduced. The materials of the source electrode 17 and the drain electrode are, for example, Ti / Al / Ti and V / Al / Ti.
[0050] Next, the planar pattern of the recess 20 and the electrode will be described. In a plan view, the source electrode 17 and the drain electrode 18 are provided at a predetermined interval and the gate electrode 16 is sandwiched between the source electrode 17 and the drain electrode 18 .
[0051] like Figure 3 In this way, the source electrode 17 and the drain electrode 18 are comb-shaped planar patterns. In other words, there are stripe-shaped portions in which thin and long linear patterns are arranged in parallel at predetermined intervals and portions connected to the linear patterns. The stripe-shaped portions of the source electrode 17 and the stripe-shaped portions of the drain electrode 18 are configured to alternately bite.
[0052] Furthermore, the gate electrode 16 is provided in each of the elongated linear patterns of the source electrode 17 as a ring-shaped pattern surrounding the linear pattern.
[0053] In addition, if Figure 3In this way, inside each linear pattern of the source electrode 17 and the drain electrode 18, a plurality of recesses 20 are arranged along the line at predetermined intervals. The planar shape of the recess 20 is, for example, a regular hexagon. This is because the side surface 20a of the recess 20 is an m-plane. Of course, the planar shape of the recess is not limited to a regular hexagon. For example, it can also be an equilateral triangle, a square, a rectangle, a circle, etc.
[0054] In a plan view, the diameter of the recess 20 only needs to be large enough to be contained within the pattern of the source electrode 17 and the drain electrode 18. Figure 3 In the case of , it only needs to be smaller than the width of the linear pattern of the source electrode 17 and the drain electrode 18. For example, the width of the linear pattern is 20 μm, and the diameter of the recess 20 is 5 μm.
[0055] The planar pattern of the gate electrode 16, the source electrode 17, and the drain electrode 18 is an example and is not limited to Figure 3 The pattern shown.
[0056] 2. Operation of semiconductor components
[0057] The semiconductor element in the first embodiment is a normally-on element that allows current to flow from the drain electrode 18 to the source electrode 17 via the 2DEG layer 19 when no voltage is applied to the gate electrode 16. If a voltage (negative voltage) below the threshold voltage is applied to the gate electrode 16, the current flowing from the drain electrode 18 to the source electrode 17 is disconnected.
[0058] If a voltage below the threshold voltage (negative voltage) is applied to the gate electrode 16, holes are extracted from the 2DHG layer 22 and disappear, and electrons disappear from the 2DEG layer 19 below the undoped layer 14. Therefore, the lower region of the undoped layer 14 is depleted as a whole, and the electric field strength is constant. As a result, the electric field applied from the drain electrode 18 to the gate electrode 16 can be evenly dispersed, and there is no area where the electric field is concentrated. As a result, a very high withstand voltage can be achieved.
[0059] Furthermore, when a voltage greater than the threshold voltage is applied to the gate electrode 16, current flows from the drain electrode 18 to the source electrode 17, and the gate electrode 16 is turned on. At this time, the current flows from the drain electrode 18 to the 2DEG layer 19 via the surface of the barrier layer 13 and the side surface 20a of the recess 20. Then, the current flows from the 2DEG layer 19 to the source electrode 17 via the surface of the barrier layer 13 and the side surface 20a of the recess 20.
[0060] Here, since the depression 20 is Figure 2 With such a structure, the source electrode 17 and the drain electrode 18 can be in good contact with the 2DEG layer 19. The details are as follows.
[0061] The side surface 20a of the recess 20 is perpendicular to the main surface of the substrate 10, so there is no substantial reduction in the thickness of the barrier layer 13. If the side surface 20a has an inclination, the deformation is moderated and the substantial thickness of the barrier layer 13 is reduced. Since there is no substantial reduction in the thickness of the barrier layer 13, it is possible to prevent the 2DEG concentration of the 2DEG layer 19 near the side surface of the recess 20 from being reduced. As a result, the source electrode 17 and the drain electrode 18 can be in good contact with the 2DEG layer 19.
[0062] The side surface of the recess 20 includes a side surface 20a perpendicular to the main surface of the substrate 10, a terrace 20b as the surface of the channel layer 12, and a side surface 20c inclined relative to the main surface of the substrate 10, and the side surface of the recess 20 has two steps. By forming such a step structure, the coverage of the source electrode 17 and the drain electrode 18 with respect to the recess 20 can be improved, and the separation of the source electrode 17 and the drain electrode 18 can be prevented. As a result, the source electrode 17 and the drain electrode 18 are firmly attached to the corner formed by the terrace 20b and the side surface 20c, and can be well contacted with the 2DEG layer 19 near the corner.
[0063] In addition, although the side surface 20a, the platform 20b, and the side surface 20c of the recess 20 will be described in detail in the manufacturing method, they are the surfaces exposed by wet etching after dry etching. Therefore, these surfaces are surfaces without etching damage. The source electrode 17 and the drain electrode 18 are in contact with the surfaces without etching damage, so the contact resistance can be reduced.
[0064] As described above, in the semiconductor element of the first embodiment, Figure 2 As shown, the recess 20 is a shape having a side surface 20a, a platform 20b, a side surface 20c, and a bottom surface 20d. Therefore, the coverage of the source electrode 17 and the drain electrode 18 is high, the disconnection of the source electrode 17 and the drain electrode 18 can be prevented, and the contact resistance of the source electrode 17 and the drain electrode 18 can be reduced.
[0065] 3. Method for manufacturing semiconductor element
[0066] Next, a method for manufacturing a semiconductor element in Embodiment 1 will be described with reference to the drawings.
[0067] First, a channel layer 12, a barrier layer 13, an undoped layer 14, and a p-layer 15 are sequentially stacked on a substrate 10 by MOCVD with a buffer layer 11 interposed therebetween (see Figure 4 ). For example, TMG (trimethylgallium) is used as Ga raw material gas, TMA (trimethylaluminum) is used as Al raw material gas, and ammonia is used as nitrogen raw material gas. In addition, hydrogen gas and nitrogen gas are used as carrier gas.
[0068] Next, a predetermined area on the surface of the p-layer 15 is dry-etched to expose the undoped layer 14. Further, the exposed undoped layer 14 is dry-etched in the area where the source electrode 17 and the drain electrode 18 are to be formed to expose the barrier layer 13 (see Figure 5 ).
[0069] Next, a predetermined region of the barrier layer 13 is dry-etched to form a recess 21 (see Figure 6 Here, the etching conditions are set so that the side surface of the recess 21 is inclined. The inclination angle of the side surface of the recess 21 is, for example, 30 to 70 degrees relative to the main surface of the substrate 10. In addition, the recess 21 is formed deeper than the surface of the channel layer 12. Due to the dry etching, etching damage occurs on the side surface and bottom surface of the recess 21.
[0070] Next, the side of the recess 21 is wet-etched with a TMAH aqueous solution. The concentration of the TMAH aqueous solution is, for example, 15 wt% to 25 wt%. In addition, the temperature of the TMAH aqueous solution is, for example, 60° C. to 90° C. If the concentration and temperature are within this range, the difference in etching rate between the barrier layer 13 and the channel layer 12 is appropriate, and the recess 20 is easily formed.
[0071] In addition, the etching time is, for example, 10 to 30 minutes. If the etching time is shorter than 10 minutes, the width of the platform 20b is not sufficiently enlarged, and the coverage of the source electrode 17 and the drain electrode 18 may be reduced or disconnected. In addition, if the etching time is longer than 30 minutes, the etching of the channel layer 12 continues to progress, the m-plane is exposed, and the side surface 20c becomes vertical, which may cause the coverage of the source electrode 17 and the drain electrode 18 to be reduced or disconnected.
[0072] In the wet etching of the III-nitride semiconductor based on the TMAH aqueous solution, the side of the recess 20 is a surface other than the c-plane, so it is etched, but the surface of the barrier layer 13, the surface of the channel layer 12, and the bottom surface of the recess 20 are c-planes, so they are not etched. In addition, the higher the Al composition, the faster the etching speed. In addition, as the etching proceeds, the m-plane is exposed, and the etching continues while keeping the m-plane as it is.
[0073] Therefore, by wet etching the recess 21, a recess 20 having a side surface 20a, a terrace 20b, a side surface 20c, and a bottom surface 20d is formed (see Figure 6 (b)). The details are as follows.
[0074] The area on the side of the recess 21 where the barrier layer 13 is exposed is etched quickly in the lateral direction. In comparison, the area on the side of the recess 21 where the channel layer 12 is exposed is etched slowly. This is because the barrier layer 13 has a higher Al composition than the channel layer 12. The surface of the channel layer 12 is exposed by this etching. The surface of the exposed channel layer 12 is a c-plane, and therefore, is not etched. Thus, a platform 20b of the recess 20 is formed. The platform 20b is a surface that is not exposed when the recess 21 is formed, and therefore, is a surface that is not damaged by etching.
[0075] As the barrier layer 13 is etched, the m-plane of the barrier layer 13 is exposed, forming a side surface 20a of the recess 20 that is perpendicular to the main surface of the barrier layer 13. As the barrier layer 13 is etched, etching damage on the side surface 20a is removed.
[0076] In addition, the area of the side surface of the recess 21 where the channel layer 12 is exposed is GaN with a lower Al composition than the barrier layer 13 (Al composition is 0), and therefore, the etching speed is slower than that of the barrier layer 13. As a result, the etching does not proceed to such an extent that the side surface becomes vertical, but the side surface has an inclination. The side surface of the channel layer 12 with this inclination becomes the side surface 20c of the recess 20. In addition, the inclination angle of the side surface 20c is equal to the inclination angle of the side surface of the recess 21, or is larger than the inclination angle of the side surface of the recess 21. The etching damage of the side surface 20c is removed by etching the channel layer 12.
[0077] Furthermore, the bottom surface of the recess 21 is a c-plane, and therefore is not etched, but directly becomes the bottom surface 20d of the recess 20. In this way, the recess 20 having the side surface 20a, the terrace 20b, the side surface 20c, and the bottom surface 20d is formed.
[0078] In addition, as the wet etching solution, an alkaline solution such as KOH or NaOH can be used in addition to TMAH. In addition, the solvent is not limited to water.
[0079] Next, source electrode 17 and drain electrode 18 are formed in predetermined regions on barrier layer 13. Source electrode 17 and drain electrode 18 are formed to cover recess 20. When source electrode 17 and drain electrode 18 are made of the same material, they can be formed simultaneously.
[0080] Here, the recess 20 has a terrace 20b that exposes the surface of the channel layer 12, and the side surface 20c has an inclination. Therefore, the source electrode 17 and the drain electrode 18 can be formed with good coverage along the step of the recess 20, and disconnection can be prevented. In particular, the source electrode 17 and the drain electrode 18 can be made to be firmly in contact with the 2DEG layer 19 exposed near the corner formed by the terrace 20b and the side surface 20c.
[0081] The source electrode 17 and the drain electrode 18 can be formed by evaporation, sputtering, etc. It is particularly preferable to use evaporation such as EB evaporation. In the past, in order to cover the recesses without causing disconnection of the source electrode 17 and the drain electrode 18, a formation method with good coverage, that is, sputtering, was used, but sometimes the semiconductor layer was damaged during sputtering. In this case, the recess 20 in the first embodiment has good coverage of the source electrode 17 and the drain electrode 18 due to its shape, so even if the source electrode 17 and the drain electrode 18 are formed by evaporation, disconnection can be prevented.
[0082] Furthermore, the source electrode 17 and the drain electrode 18 are in contact with the side surface 20 a , the terrace 20 b , and the side surface 20 c of the recess 20 that are not damaged by etching, and therefore, the contact resistance can be reduced.
[0083] Next, heat treatment is performed to reduce the contact resistance of the source electrode 17 and the drain electrode 18. The heat treatment conditions are, for example, 500° C. to 700° C. for 60 seconds to 600 seconds in a nitrogen atmosphere.
[0084] Next, gate electrode 16 is formed on p-layer 15 by vapor deposition or the like. Gate electrode 16 may be formed first, and then recess 20, source electrode 17, and drain electrode 18 may be formed. As described above, the semiconductor element in Embodiment 1 is manufactured.
[0085] 4. Experimental Results
[0086] As sample A, a semiconductor element in Embodiment 1 in which a depression 20 was formed was prepared as follows. First, a depression 21 having a depth reaching the channel layer 12 was formed by dry etching, and then wet etching was performed at 50° C. for 20 minutes using a TMAH aqueous solution having a concentration of 2.3 wt%. Thus, a depression 20 having a platform 20 b having a width of 40 nm was formed. Then, an electrode was formed across the upper surface, side surface, and bottom surface of the depression 20. The electrode was Ti / Al / Ti, and the alloy temperature was 600° C.
[0087] On the other hand, as sample B, the wet etching method after forming the recess 21 was changed as follows to form the recess 20. Other than this, it was the same as sample A. The wet etching was performed at 85° C. for 20 minutes using a 22 wt % TMAH aqueous solution. Thus, the recess 20 with a terrace 20 b having a width of 140 nm was formed.
[0088] Figure 7 : is a graph showing the results of contact resistance measurement and comparison of samples A and B using TLM patterns. Figure 7 Thus, the average value and the median value of the contact resistivity of sample B are lower than those of sample A.
[0089] Furthermore, a plurality of semiconductor devices according to the first embodiment having the recess 20 of the samples A and B were manufactured, and the on-resistance of each device was measured. Figure 8 is a coordinate diagram showing the distribution of the on-resistance of each element. Figure 8 It can be seen that the mode value of the on-resistance of sample B is 1 mΩcm lower than that of sample A. 2 .
[0090] Fig. 9 The following are cross-sectional SEM images of the concave cross-sections of samples A and B. Fig. 9 As shown in (a), it can be seen that a break occurs in sample A. On the other hand, Fig. 9 As shown in (b), no electrode disconnection occurred in sample B.
[0091] according to Figure 7 to Figure 9 It is known that by making the width of the terrace 20b in the depression 20 sufficiently wide, the electrode can cover the depression 20 better and prevent disconnection. In addition, it is known that by improving the coverability and preventing disconnection, the contact resistivity of the electrode can be reduced, and the on-resistance can be reduced.
[0092] 5. Various deformation methods
[0093] The present invention is not limited to the semiconductor element shown in Embodiment 1, and can be applied to any semiconductor element as long as it has a structure including a channel layer composed of a group III nitride semiconductor and a barrier layer composed of a group III nitride semiconductor having a higher Al composition than the channel layer, and an electrode connected to a 2DEG layer via a recess. For example, the present invention can also be applied to HFETs and the like.
Claims
1. A semiconductor element comprising: a substrate, a channel layer disposed on the substrate and composed of a group III nitride semiconductor, and a barrier layer disposed on the channel layer and in contact with the channel layer and composed of a group III nitride semiconductor having a higher Al composition than the channel layer, The semiconductor element is characterized by having: a recess provided in a partial region of the surface of the barrier layer and having a depth reaching the channel layer; and an electrode arranged to cover along the depression, The depression has: a first side surface, which is a surface on which the barrier layer is exposed and is a surface having an angle with respect to the main surface of the substrate; a terrace connected to the first side surface and exposing a surface of the channel layer; and The second side surface is a surface connected to the terrace and exposing the channel layer, and is a surface inclined with respect to the main surface of the substrate and having an inclination angle smaller than that of the first side surface.
2. The semiconductor device according to claim 1, characterized in that The width of the platform is greater than 100 nm.
3. The semiconductor device according to claim 1 or 2, characterized in that: The first side surface is a surface having an angle of not less than 80 degrees and not more than 90 degrees with respect to the main surface of the substrate.
4. The semiconductor device according to claim 1 or 2, characterized in that: The first side surface is the m-plane of the barrier layer.
5. A method for manufacturing a semiconductor element, the semiconductor element comprising: a substrate, a channel layer disposed on the substrate and composed of a Group III nitride semiconductor, and a barrier layer disposed on and in contact with the channel layer and composed of a Group III nitride semiconductor having a higher Al composition than the channel layer, The method for manufacturing a semiconductor element is characterized by comprising: a first recess forming step, in which a predetermined region of the barrier layer surface is dry-etched to form a first recess having a side surface inclined relative to the main surface of the substrate and a bottom surface deeper than the channel layer surface; a second recess forming step, in which the side surface of the first recess is wet-etched with an alkaline solution to form a second recess; and an electrode forming step, in which an electrode is formed on the barrier layer so as to cover the second recess, In the second recess forming step, The barrier layer is wet-etched to form a first side surface which is an angled surface with respect to the main surface of the substrate, and a surface of the channel layer is exposed to form a terrace. The channel layer is wet-etched to form a second side surface which is inclined with respect to the main surface of the substrate and has a smaller inclination angle than the first side surface.
6. The method for manufacturing a semiconductor device according to claim 5, wherein: In the second recess forming step, the terrace is formed so that the width of the terrace becomes greater than or equal to 100 nm.
7. The method for manufacturing a semiconductor element according to claim 5 or 6, characterized in that: In the second recess forming step, the first side surface is formed to have an angle of not less than 80 degrees and not more than 90 degrees with respect to the main surface of the substrate.
8. The method for manufacturing a semiconductor element according to claim 5 or 6, characterized in that: In the second recess forming step, the first side surface is formed to be an m-plane.
9. The method for manufacturing a semiconductor element according to claim 5 or 6, characterized in that: The alkaline solution is a TMAH aqueous solution.