InGaN diode with gradient In component and preparation method thereof

By introducing a graded InGaN layer with a gradient In content into the InGaN diode, the problem of poor P-type layer material quality of GaN PIN diodes is solved, the response time and carrier-hole transmission efficiency are improved, and the high-frequency characteristics and performance of the device are improved. Thermal stability meets the needs of high-power RF applications.

CN118738141APending Publication Date: 2024-10-01XIDIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410887349.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The P-type layer material of existing GaN PIN diodes is of poor quality and cannot meet the development needs of limiters, especially in high-power radio frequency applications.

Method used

An InGaN diode with gradient In composition is designed. By setting a gradient InGaN layer with gradient In content between the P-type InN layer and the intrinsic layer, the response time is shortened, the turn-on voltage is reduced, and the carrier-hole transport is improved. efficiency.

Benefits of technology

It improves the high-frequency characteristics of the diode, reduces the on-resistance, enhances the radiation resistance and thermal stability of the device, and meets the needs of high-power applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738141A_ABST
    Figure CN118738141A_ABST
Patent Text Reader

Abstract

The invention relates to an In component gradual change InGaN diode and a preparation method thereof, the diode comprises a substrate layer, an N-type layer, an intrinsic layer, a gradual change InGaN layer, a P-type InN layer, a cathode and an anode, and the substrate layer, the N-type layer, the intrinsic layer, the gradual change InGaN layer and the P-type InN layer are sequentially arranged from bottom to top; and the In content in the gradient InGaN layer is sequentially reduced from bottom to top. The P-type InN layer is used as the P-type region of the diode, so that the response time of the diode is shortened, and the turn-on voltage of the diode is reduced. And lattice mismatch between the P-type InN layer and the intrinsic layer is reduced through the gradually-changed InGaN layer with the In content gradually changed, and the carrier-hole transmission efficiency of the P-type InN layer is improved. According to the diode provided by the invention, the forward characteristic is improved, the turn-on voltage is reduced, the on-resistance is reduced, and the high-frequency characteristic of a device is greatly improved while the reverse breakdown characteristic is not influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductors, and in particular relates to an InGaN diode with a gradual In component change and a preparation method thereof. Background Art

[0002] With the vigorous development of new energy vehicles, 5G communications, aerospace and other fields, people have put forward requirements for electronic equipment such as integration, miniaturization, high power resistance and low loss. In order to ensure the stable working state of the equipment under high RF power, it is usually necessary to carry out specific RF protection design for the equipment. As the front end of the radar receiver, the low noise amplifier will be burned by high RF power input, resulting in its inability to work normally in high-power application scenarios. Therefore, a limiter is introduced in the radar system. The limiter selects the power transmitted to the input end of the low noise amplifier according to the input power to protect the low noise amplifier and enable the entire radar system to meet the requirements of high RF power input. When a low-power signal is input, the limiter will transmit the input power to the input end of the low noise amplifier with less loss; when a high-power signal is used as input, the high-power signal will be attenuated to a certain amplitude by the limiter before being transmitted.

[0003] In the prior art, the most commonly used device for limiters is the PIN diode, which consists of three layers: P-type, I-type, and N-type. Gallium nitride materials can be used to make high-voltage, high-frequency, and high-power electronic devices due to their wide bandgap, high electron drift velocity, high thermal conductivity, and high breakdown electric field. Compared with the limiting circuits made of traditional Si-based and GaAs devices, GaNPIN diodes can achieve smaller-sized high-voltage and low-on-resistance diodes.

[0004] However, the P-type layer material quality of the GaN PIN diode in the prior art is poor and it is difficult to meet the development requirements of the limiter. Summary of the invention

[0005] In order to solve the above problems existing in the prior art, the present invention provides an InGaN diode with a gradient In composition and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:

[0006] The first aspect of the present invention provides an InGaN diode with a gradient In composition, comprising: a substrate layer, an N-type layer, an intrinsic layer, a gradient InGaN layer, a P-type InN layer, a cathode and an anode, wherein:

[0007] The substrate layer, the N-type layer, the intrinsic layer, the graded InGaN layer and the P-type InN layer are arranged in sequence from bottom to top;

[0008] The content of In in the graded InGaN layer decreases from bottom to top;

[0009] The cathode is arranged on the upper surface of the N-type layer and located on both sides of the intrinsic layer;

[0010] The anode is arranged on the upper surface of the P-type InN layer.

[0011] In a specific embodiment, the content of In in the graded InGaN layer decreases uniformly from 10% to 0 from bottom to top.

[0012] In a specific embodiment, the thickness of the graded InGaN layer is 200-300 nm;

[0013] The doping type of the gradient InGaN layer is P-type doping, and the doping concentration is 1×10 18 ~5×10 18 cm -3 , the doping ions include Mg ions.

[0014] In a specific embodiment, the material of the substrate layer includes Si or SiC;

[0015] The material of the N-type layer includes GaN;

[0016] The material of the intrinsic layer includes InGaN.

[0017] In a specific embodiment, the doping concentration of the N-type layer is 1×10 18 ~1×10 19 cm -3 ;

[0018] The doping concentration of the P-type InN layer is 1×10 19 ~1×10 20 cm -3 .

[0019] In a specific embodiment, the thickness of the substrate layer is 5 to 10 μm;

[0020] The thickness of the N-type layer is 0.5 to 2 μm;

[0021] The thickness of the intrinsic layer is 1 to 3 μm;

[0022] The thickness of the P-type InN layer is 1-2 μm.

[0023] In a specific embodiment, the doping ions of the N-type layer include Si ions;

[0024] The doping ions of the P-type InN layer include Mg ions.

[0025] In a specific embodiment, the cathode includes: a first sub-cathode and a second sub-cathode;

[0026] The first sub-cathode is located on the upper surface of the N-type layer and on one side of the intrinsic layer;

[0027] The second sub-cathode is located on the upper surface of the N-type layer and on the other side of the intrinsic layer.

[0028] The second aspect of the present invention provides a method for preparing an InGaN diode with a gradient In composition, which is used to prepare the diode provided by the first aspect of the present invention, comprising the following steps:

[0029] S1: Get the substrate layer;

[0030] S2: preparing an N-type layer on the upper surface of the substrate layer;

[0031] S3: preparing an intrinsic layer on the upper surface of the N-type layer;

[0032] S4: preparing a gradient InGaN layer on the upper surface of the intrinsic layer; the content of In in the gradient InGaN layer decreases from bottom to top;

[0033] S5: preparing a P-type InN layer on the upper surface of the graded InGaN layer;

[0034] S6: preparing cathodes on the upper surfaces of the N-type layers on both sides of the intrinsic layer;

[0035] S7: preparing an anode on the upper surface of the P-type InN layer.

[0036] In a specific embodiment, the step S4 includes:

[0037] A gradient InGaN layer is prepared on the upper surface of the intrinsic layer by MOCVD; the content of In in the gradient InGaN layer decreases uniformly from 10% to 0 from bottom to top.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] The present invention provides an InGaN diode with a gradient In component, which uses a P-type InN layer as the P-type region of the diode to shorten the response time of the diode and reduce the turn-on voltage of the diode. A gradient InGaN layer with a gradient In content is provided between the P-type InN layer and the intrinsic layer to reduce the lattice mismatch between the P-type InN layer and the intrinsic layer, thereby improving the carrier-hole transmission efficiency of the P-type InN layer. The diode provided by the present invention improves the forward characteristics, reduces the turn-on voltage, reduces the on-resistance, and greatly improves the high-frequency characteristics of the device without affecting the reverse breakdown characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 is a schematic structural diagram of an InGaN diode with a gradual change in In composition provided by an embodiment of the present invention;

[0041] Figure 2a to Figure 2g It is a schematic diagram of the steps of a method for preparing an InGaN diode with a gradient In composition provided by an embodiment of the present invention.

[0042] Reference numerals:

[0043] 1: substrate layer; 2: N-type layer; 3: intrinsic layer; 4: graded InGaN layer; 5: P-type InN layer; 6: cathode; 7: anode. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.

[0045] Embodiment 1

[0046] See also Figure 1 , Figure 1 It is a schematic diagram of the structure of an InGaN diode with a gradient In composition provided by an embodiment of the present invention.

[0047] The present embodiment provides an InGaN diode with a gradient In composition, comprising: a substrate layer 1, an N-type layer 2, an intrinsic layer 3, a gradient InGaN layer 4, a P-type InN layer 5, a cathode 6 and an anode 7. The substrate layer 1, the N-type layer 2, the intrinsic layer 3, the gradient InGaN layer 4 and the P-type InN layer 5 are arranged in sequence from bottom to top. The content of In in the gradient InGaN layer 4 decreases in sequence from bottom to top. The cathode 6 is arranged on the upper surface of the N-type layer 2 and is located on both sides of the intrinsic layer 3. The anode 7 is arranged on the upper surface of the P-type InN layer 5.

[0048] Specifically, the InN material has high hole mobility and low barrier characteristics. In this embodiment, the P-type InN layer 5 is used as the P-type region of the diode to shorten the response time of the diode and reduce the turn-on voltage of the diode. A gradient InGaN layer 4 with a gradient In content is provided between the P-type InN layer 5 and the intrinsic layer 3 to reduce the lattice mismatch between the P-type InN layer 5 and the intrinsic layer 3, thereby improving the carrier-hole transmission efficiency of the P-type InN layer 5. The diode provided in this embodiment improves the forward characteristics, reduces the turn-on voltage, reduces the on-resistance, and greatly improves the high-frequency characteristics of the device without affecting the reverse breakdown characteristics.

[0049] In this embodiment, the content of In in the graded InGaN layer 4 decreases uniformly from 10% to 0 from bottom to top. The thickness of the graded InGaN layer 4 is 200-300 nm. The doping type of the graded InGaN layer 4 is P-type doping, and the doping concentration is 1×10 18 ~5×10 18 cm -3 , the doping ions include Mg ions.

[0050] Specifically, the bottom end of the graded InGaN layer 4, i.e., the end close to the intrinsic layer 3, has the largest In content, which is 10%. The top end of the graded InGaN layer 4, i.e., the end close to the P-type InN layer 5, has the smallest In content, which is 0. Moreover, the In content in the graded InGaN layer 4 changes uniformly and linearly. The In content of the gradient InGaN layer 4 at one end close to the intrinsic layer 3 is large. When the In content is 10%, the gradient InGaN layer 4 and the intrinsic layer 3 have a high lattice matching degree. The In content of the gradient InGaN layer 4 at one end close to the P-type InN layer 5 is small. When the In content is 0, the gradient InGaN layer 4 and the P-type InN layer 5 have a high lattice matching degree. Moreover, since the In content in the gradient InGaN layer 4 changes uniformly and linearly, the lattice constant of the gradient InGaN layer 4 changes slowly and uniformly. Therefore, the gradient InGaN layer 4 can effectively reduce the lattice mismatch between the P-type InN layer 5 and the intrinsic layer 3, and improve the carrier-hole transmission efficiency of the P-type InN layer 5.

[0051] In this embodiment, the material of the substrate layer 1 includes Si or SiC, and the thickness of the substrate layer 1 is 5 to 10 μm. The material of the N-type layer 2 includes GaN, and the thickness of the N-type layer 2 is 0.5 to 2 μm. The doping ions of the N-type layer 2 include Si ions, and the doping concentration of the N-type layer 2 is 1×10 18 ~1×10 19 cm -3 The material of the intrinsic layer 3 includes InGaN, and the thickness of the intrinsic layer 3 is 1 to 3 μm. The doping concentration of the P-type InN layer 5 is 1×10 19 ~1×10 20 cm -3 The thickness of the P-type InN layer 5 is 1 to 2 μm, and the doping ions of the P-type InN layer 5 include Mg ions.

[0052] Specifically, the material of the N-type layer 2 is GaN, which can provide a higher reverse breakdown voltage while achieving higher thermal power diffusion, so that the device has higher radiation resistance and thermal stability, meeting the needs of high-power applications. The material of the intrinsic layer 3 is InGaN with a low In component. Furthermore, the material of the intrinsic layer 3 is InGaN with an In component content of 1 to 5%, and the doping concentration of the intrinsic layer 3 is 10 14 ~10 17 cm-3 , the doping ions of the intrinsic layer 3 include Mg. The intrinsic layer 3 is used as the I layer in the PIN diode. The holes of the P-type InN layer 5 and the electrons of the N-type layer 2 are recombined in the I-layer intrinsic layer 3 to form a current. The lattice mismatch between the low In component InGaN and the gradient InGaN layer 4 is small. The material of the intrinsic layer 3 is selected from the low In component InGaN, which can effectively improve the lattice quality of the diode and improve the carrier-hole transmission efficiency of the diode.

[0053] In an achievable manner, the cathode 6 includes: a first sub-cathode and a second sub-cathode. The first sub-cathode is located on the upper surface of the N-type layer 2 and on one side of the intrinsic layer 3. The second sub-cathode is located on the upper surface of the N-type layer 2 and on the other side of the intrinsic layer 3.

[0054] Specifically, the materials of the cathode 6 and the anode 7 include Ti / Ni or Ti / Al or Ti / Pt or Ni / Ti / Al. When the cathode 6 and the anode 7 are two-layer laminated metals, the thickness of the first metal layer is 20 to 100 nm, and the thickness of the second metal layer is 30 to 300 nm. When the cathode 6 and the anode 7 are three-layer laminated metals, the thickness of the first metal layer is 20 to 100 nm, the thickness of the second metal layer is 30 to 300 nm, and the thickness of the third metal layer is 20 to 200 nm.

[0055] The present embodiment provides an InGaN diode with a gradient In component, which shortens the response time of the diode and reduces the turn-on voltage of the diode by using the P-type InN layer 5 as the P-type region of the diode. A gradient InGaN layer 4 with a gradient In content is provided between the P-type InN layer 5 and the intrinsic layer 3 to reduce the lattice mismatch between the P-type InN layer 5 and the intrinsic layer 3, thereby improving the carrier-hole transmission efficiency of the P-type InN layer 5. The diode provided in the present embodiment improves the forward characteristics, reduces the turn-on voltage, reduces the on-resistance, and greatly improves the high-frequency characteristics of the device without affecting the reverse breakdown characteristics.

[0056] Embodiment 2

[0057] See also Figure 2a to Figure 2g , Figure 2a to Figure 2g It is a schematic diagram of the steps of a method for preparing an InGaN diode with a gradient In composition provided by an embodiment of the present invention.

[0058] The present embodiment provides a method for preparing an InGaN diode with a gradient In composition, which is used to prepare the diode provided in the first embodiment of the present invention, and comprises the following steps:

[0059] S1: Get substrate layer 1.

[0060] Specifically, see Figure 2a, Si or SiC is selected as the substrate material, the substrate material is ultrasonically cleaned in acetone and anhydrous ethanol for 10 minutes respectively, then the substrate material is immersed in a 10% HF solution for 3 minutes, and then cleaned with deionized water and dried with nitrogen to obtain a substrate layer 1. In this embodiment, SiC is selected as the substrate material.

[0061] S2: preparing an N-type layer 2 on the upper surface of the substrate layer 1 .

[0062] Specifically, see Figure 2b , the substrate layer 1 is placed in a reaction chamber, and a 0.5-2 μm thick N-type heavily doped GaN is deposited on the upper surface of the substrate layer 1 by a low pressure chemical vapor deposition LPCVD process to obtain an N-type layer 2. In this embodiment, the doping ions of the N-type layer 2 include Si ions, and the doping concentration is 1×10 18 ~1×10 19 cm -3 .

[0063] S3 : preparing an intrinsic layer 3 on the upper surface of the N-type layer 2 .

[0064] Specifically, see Figure 2c , a metal organic chemical vapor deposition (MOCVD) process is used to grow an intrinsic type InGaN layer with a thickness of 1 μm on the upper surface of the N-type layer 2 as the intrinsic layer 3. In this embodiment, the growth temperature is 860°C, and the TMIn flow rate is 25 sccm. In this embodiment, the In content of the intrinsic layer 3 is 1-5%, the doping ions of the intrinsic layer 3 are Mg ions, and the doping concentration of the intrinsic layer 3 is 1×10 15 cm -3 .

[0065] S4: forming a graded InGaN layer 4 on the upper surface of the intrinsic layer 3. The content of In in the graded InGaN layer 4 decreases from bottom to top.

[0066] Specifically, see Figure 2d A graded InGaN layer 4 is prepared on the upper surface of the intrinsic layer 3 by an MOCVD process. The content of In in the graded InGaN layer 4 decreases from 10 to 0 from bottom to top.

[0067] Specifically, a P-type doped InGaN with a gradient In content is grown on the upper surface of the intrinsic layer 3 by using an MOCVD process as the gradient InGaN layer 4. In this embodiment, the growth thickness is 200-300nm, the growth temperature is 860°C, the growth time is 5-10min, and the TMIn flow rate is continuously reduced from 175sccm to 0sccm as the growth time changes. When the TMIn flow rate is 175sccm, the In content in the obtained gradient InGaN layer 4 is 10%. In this embodiment, the doping type of the gradient InGaN layer 4 is P-type doping, and the doping concentration is 1×10 18 ~5×10 18 cm -3 , the doping ions include Mg ions.

[0068] S5 : preparing a P-type InN layer 5 on the upper surface of the graded InGaN layer 4 .

[0069] Specifically, see Figure 2e The MOCVD process is used to grow a P-type InN layer 5 with a thickness of 1 to 2 μm on the upper surface of the graded InGaN layer 4. In this embodiment, the doping concentration of the P-type InN layer 5 is 1×10 19 ~1×10 20 cm -3 , the doping ions of the P-type InN layer 5 include Mg ions.

[0070] S6 : preparing a cathode 6 on the upper surface of the N-type layer 2 on both sides of the intrinsic layer 3 .

[0071] Specifically, cathode metal is deposited on the upper surface of the N-type layer 2 on both sides of the intrinsic layer 3 to obtain the cathode 6 .

[0072] In this example, see Figure 2f , a cathode metal is deposited on the upper surface of the N-type layer 2 on one side of the intrinsic layer 3 by evaporation or magnetic sputtering to obtain a first sub-cathode, and a cathode metal is deposited on the upper surface of the N-type layer 2 on the other side of the intrinsic layer 3 by evaporation or magnetic sputtering to obtain a second sub-cathode, and annealing is performed at high temperature after the deposition is completed. The first sub-cathode and the second sub-cathode form a cathode 6. The cathode metal includes Ti / Ni or Ti / Al or Ti / Pt or Ni / Ti / Al.

[0073] S7 : preparing an anode 7 on the upper surface of the P-type InN layer 5 .

[0074] Specifically, see Figure 2g, a mask is made on the upper surface of the P-type InN layer 5, the sample obtained in step S6 is placed in an electron beam evaporation table, an anode metal is deposited on the P-type InN layer 5 by an evaporation process, and annealed at a high temperature to obtain an anode 7. In this embodiment, the anode metal includes Ti / Ni or Ti / Al or Ti / Pt or Ni / Ti / Al.

[0075] The present embodiment provides a method for preparing an InGaN diode with a gradient In content, by preparing a gradient InGaN layer 4 with a gradient In content between the P-type InN layer 5 and the intrinsic layer 3, the lattice mismatch between the P-type InN layer 5 and the intrinsic layer 3 is reduced, and the carrier-hole transmission efficiency of the P-type InN layer 5 is improved. The diode obtained by the preparation method provided by the present embodiment improves the forward characteristics, reduces the turn-on voltage, reduces the on-resistance, and greatly improves the high-frequency characteristics of the device without affecting the reverse breakdown characteristics.

[0076] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. An InGaN diode with a gradient In composition, characterized in that: include: substrate layer, N-type layer, intrinsic layer, graded InGaN layer, P-type InN layer, cathode and anode, wherein: The substrate layer, the N-type layer, the intrinsic layer, the graded InGaN layer and the P-type InN layer are arranged in sequence from bottom to top; The content of In in the graded InGaN layer decreases from bottom to top; The cathode is arranged on the upper surface of the N-type layer and located on both sides of the intrinsic layer; The anode is arranged on the upper surface of the P-type InN layer.

2. The InGaN diode with a gradient In composition according to claim 1, characterized in that: The content of In in the graded InGaN layer decreases uniformly from 10% to 0 from bottom to top.

3. The InGaN diode with a gradient In composition according to claim 1, characterized in that: The thickness of the gradient InGaN layer is 200-300 nm; The doping type of the gradient InGaN layer is P-type doping, and the doping concentration is 1×10 18 ~5×10 18 cm -3 , the doping ions include Mg ions.

4. The InGaN diode with a gradient In composition according to claim 1, characterized in that: The material of the substrate layer includes Si or SiC; The material of the N-type layer includes GaN; The material of the intrinsic layer includes InGaN.

5. The InGaN diode with a gradient In composition according to claim 4, characterized in that: The doping concentration of the N-type layer is 1×10 18 ~1×10 19 cm -3 ; The doping concentration of the P-type InN layer is 1×10 19 ~1×10 20 cm -3 .

6. The InGaN diode with a gradient In composition according to claim 4, characterized in that: The thickness of the substrate layer is 5 to 10 μm; The thickness of the N-type layer is 0.5 to 2 μm; The thickness of the intrinsic layer is 1 to 3 μm; The thickness of the P-type InN layer is 1-2 μm.

7. The InGaN diode with a gradient In composition according to claim 4, characterized in that: The doping ions of the N-type layer include Si ions; The doping ions of the P-type InN layer include Mg ions.

8. The InGaN diode with a gradient In composition according to claim 1, characterized in that: The cathode comprises: a first sub-cathode and a second sub-cathode; The first sub-cathode is located on the upper surface of the N-type layer and on one side of the intrinsic layer; The second sub-cathode is located on the upper surface of the N-type layer and on the other side of the intrinsic layer.

9. A method for preparing an InGaN diode with a gradient In composition, characterized in that: The method for preparing the diode according to any one of claims 1 to 8 comprises the following steps: S1: Get the substrate layer; S2: preparing an N-type layer on the upper surface of the substrate layer; S3: preparing an intrinsic layer on the upper surface of the N-type layer; S4: preparing a gradient InGaN layer on the upper surface of the intrinsic layer; the content of In in the gradient InGaN layer decreases from bottom to top; S5: preparing a P-type InN layer on the upper surface of the graded InGaN layer; S6: preparing cathodes on the upper surfaces of the N-type layers on both sides of the intrinsic layer; S7: preparing an anode on the upper surface of the P-type InN layer.

10. The method for preparing an InGaN diode with a gradient In composition according to claim 9, characterized in that: The step S4 comprises: A gradient InGaN layer is prepared on the upper surface of the intrinsic layer by MOCVD; the content of In in the gradient InGaN layer decreases uniformly from 10% to 0 from bottom to top.