Cadmium telluride thin film solar cell and manufacturing method thereof

By using magnesium-doped tin oxide window layer and radio frequency magnetron sputtering process in cadmium telluride thin film solar cells, the problem of low open circuit voltage of cadmium telluride thin film solar cells is solved and the efficiency is improved.

CN118738150APending Publication Date: 2024-10-01BEIJING TIANYU SOLAR ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410831730.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The open circuit voltage of cadmium telluride thin film solar cells is low, which limits the improvement of their conversion efficiency.

Method used

Magnesium-doped tin oxide is used as the window layer material, manufactured through radio frequency magnetron sputtering process, and combined with heat treatment technology to reduce interface defects between the window layer and the absorption layer, improve crystal quality, and reduce carrier recombination.

Benefits of technology

The open circuit voltage and conversion efficiency of cadmium telluride thin film solar cells are significantly improved, and the battery performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738150A_ABST
    Figure CN118738150A_ABST
Patent Text Reader

Abstract

The invention provides a cadmium telluride thin-film solar cell and a manufacturing method thereof, the cadmium telluride thin-film solar cell comprises a first electrode layer, a window layer, an absorption layer and a second electrode layer which are sequentially stacked, and the material of the absorption layer at least comprises cadmium telluride, so that the absorption layer is utilized to absorb most sunlight for photoelectric conversion. The material of the window layer is magnesium-doped tin oxide, the window layer is manufactured by using a radio frequency magnetron sputtering process, the magnesium-doped tin oxide manufactured by using the radio frequency magnetron sputtering process can realize high crystal quality, and the interface defect between the window layer and the absorption layer is reduced. Therefore, interface recombination of carriers between the window layer and the absorption layer is reduced, the open-circuit voltage of the cadmium telluride thin film solar cell is improved, and finally the conversion efficiency of the cadmium telluride thin film solar cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solar cells, and in particular to a cadmium telluride thin-film solar cell and a manufacturing method thereof. Background Art

[0002] As the demand for environmental protection becomes higher and higher, a variety of renewable energy sources are currently used as energy supply systems. Solar energy is a renewable energy source with great development potential, and solar cells can be manufactured to realize the utilization of solar energy.

[0003] Solar cells include cadmium telluride (CdTe) thin film solar cells. Cadmium telluride (CdTe) is a II-VI group direct bandgap semiconductor material with an optical bandgap width of 1.45 eV and an absorption coefficient as high as 10 5 cm -1 , a CdTe film with a thickness of only 1 to 2 μm can absorb most of the sunlight. Based on the above characteristics, cadmium telluride thin film solar cells are regarded as a promising thin film solar cell. The theoretical conversion efficiency of cadmium telluride thin film solar cells can reach ~31%, while the current highest conversion efficiency in the laboratory is only 22.6%. The main performance parameter that limits its further improvement in conversion efficiency is the low open circuit voltage.

[0004] Therefore, how to increase the open circuit voltage of cadmium telluride thin film solar cells and thus improve their conversion efficiency is an urgent problem to be solved. Summary of the invention

[0005] In view of this, the purpose of the present application is to provide a cadmium telluride thin film solar cell and a manufacturing method thereof, which can improve the open circuit voltage of the cadmium telluride thin film solar cell and thus improve its conversion efficiency.

[0006] The present application provides a cadmium telluride thin film solar cell, the cadmium telluride thin film solar cell comprising:

[0007] A first electrode layer, a window layer, an absorption layer and a second electrode layer are stacked in sequence, the material of the window layer is magnesium-doped tin oxide, and the material of the absorption layer includes at least cadmium telluride; the window layer is manufactured by using a radio frequency magnetron sputtering process.

[0008] Optionally, in the window layer, the number of magnesium atoms accounts for 1-30% of the total number of tin atoms and magnesium atoms.

[0009] Optionally, in the window layer, the number of magnesium atoms accounts for 4%, 6%, 9% or 12% of the total number of tin atoms and magnesium atoms.

[0010] Optionally, the growth temperature of the window layer is in the range of 200-500°C.

[0011] Optionally, the thickness of the window layer is greater than or equal to 10 nm.

[0012] Optionally, the radio frequency magnetron sputtering process includes a co-sputtering process;

[0013] The target materials of the co-sputtering process include tin oxide and magnesium oxide.

[0014] Optionally, the sputtering power of the tin oxide is 60W, and the sputtering power of the magnesium oxide is in the range of 10 to 100W.

[0015] Optionally, the absorption layer is manufactured using a close-space sublimation process.

[0016] Optionally, the window layer is subjected to a heat treatment at a temperature ranging from 300 to 600° C. and for a time ranging from 10 to 60 minutes.

[0017] The present application provides a method for manufacturing a cadmium telluride thin film solar cell, the method comprising:

[0018] forming a first electrode layer on a transparent substrate;

[0019] forming a window layer on the first electrode layer, wherein the material of the window layer is magnesium-doped tin oxide;

[0020] forming an absorption layer on the window layer;

[0021] A second electrode layer is formed on the absorption layer.

[0022] The present application provides a cadmium telluride thin film solar cell, which comprises: a first electrode layer, a window layer, an absorption layer, and a second electrode layer are stacked in sequence, and the material of the absorption layer comprises at least cadmium telluride, so as to realize photoelectric conversion by absorbing most of the sunlight by the absorption layer. The material of the window layer is magnesium-doped tin oxide, and the window layer is manufactured by radio frequency magnetron sputtering process. The magnesium-doped tin oxide manufactured by radio frequency magnetron sputtering process can achieve higher crystal quality, and the interface defects between the window layer and the absorption layer are reduced, thereby reducing the interface recombination of carriers between the window layer and the absorption layer, thereby improving the open circuit voltage of the cadmium telluride thin film solar cell, and finally improving the conversion efficiency of the cadmium telluride thin film solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0024] Figure 1 A schematic structural diagram of a cadmium telluride thin-film solar cell provided in an embodiment of the present application is shown;

[0025] Figure 2 A schematic diagram of energy band arrangement at a SnO2:Mg / CdTe interface provided in an embodiment of the present application is shown;

[0026] Figure 3 A schematic diagram of a current-voltage performance curve of a cadmium telluride thin-film solar cell provided in an embodiment of the present application is shown;

[0027] Figure 4 A schematic flow chart of a method for manufacturing a cadmium telluride thin-film solar cell provided in an embodiment of the present application is shown. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0029] In the following description, many specific details are set forth to facilitate a full understanding of the present application, but the present application may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.

[0030] This application is described in detail with reference to schematic diagrams. When describing the embodiments of this application in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of this application. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.

[0031] How to increase the open circuit voltage of cadmium telluride thin film solar cells and thus improve their conversion efficiency is an urgent problem to be solved.

[0032] Theoretically, the technical routes to increase the open circuit voltage of cadmium telluride thin film solar cells are: 1. Increase the P-type carrier concentration of CdTe; 2. Increase the minority carrier lifetime in CdTe; 3. Optimize the interface contact between the functional layers of the battery structure to reduce carrier recombination. Among them, optimizing the PN junction interface in the battery and reducing the defect state density to reduce carrier recombination at the interface is one of the important ways to increase the open circuit voltage.

[0033] The selection of window layer materials for cadmium telluride thin-film solar cells is very important. On the one hand, the window layer is required to be an N-type semiconductor material so that it can form a PN junction with the P-type CdTe; on the other hand, the window layer is required to be a transparent material to reduce the parasitic absorption of visible light in the window layer and avoid the reduction of short-circuit current density. Traditional cadmium telluride thin-film solar cells use cadmium sulfide (CdS) as the window layer, but the bandgap width of cadmium sulfide is ~2.4eV, which inevitably causes the absorption of short-wavelength photons in visible light, resulting in a decrease in cell performance. In recent years, researchers tend to use wide-bandgap semiconductor materials to replace cadmium sulfide as the window layer of cadmium telluride thin-film solar cells, such as N-type zinc oxide (ZnO) and tin dioxide (SnO2) and other oxides.

[0034] However, compared with the traditional cadmium sulfide window layer, the wide bandgap oxide window layer has obvious shortcomings. For example, there is almost no element interdiffusion between the oxide and cadmium telluride, and a thin buffer layer cannot be formed at the interface. At the same time, there is a serious lattice mismatch between the oxide and cadmium telluride. The above phenomenon leads to an increase in the defect state density at the interface, which triggers carrier recombination and reduces the open circuit voltage. Therefore, how to passivate the interface between oxide and cadmium telluride and reduce the interface defect state density between oxide and cadmium telluride to reduce recombination, increase open circuit voltage and improve conversion efficiency is an urgent problem to be solved when using oxide as a window layer.

[0035] Based on this, the present application provides a cadmium telluride thin film solar cell, which includes: a first electrode layer, a window layer, an absorption layer and a second electrode layer are stacked in sequence, and the material of the absorption layer includes at least cadmium telluride, so as to realize photoelectric conversion by absorbing most of the sunlight by the absorption layer. The material of the window layer is magnesium-doped tin oxide, and the window layer is manufactured by radio frequency magnetron sputtering process. The magnesium-doped tin oxide manufactured by radio frequency magnetron sputtering process can achieve higher crystal quality, and the interface defects between the window layer and the absorption layer are reduced, thereby reducing the interface recombination of carriers between the window layer and the absorption layer, thereby improving the open circuit voltage of the cadmium telluride thin film solar cell, and finally improving the conversion efficiency of the cadmium telluride thin film solar cell.

[0036] In order to better understand the technical solution and technical effects of the present application, specific embodiments will be described in detail below with reference to the accompanying drawings.

[0037] See also Figure 1 , which is a schematic diagram of the structure of a cadmium telluride thin film solar cell provided in an embodiment of the present application.

[0038] The cadmium telluride thin film solar cell provided in this embodiment includes: a first electrode layer 2, a window layer 3, an absorption layer 4 and a second electrode layer 6 are stacked in sequence, that is, the window layer 3 covers the first electrode layer 2, the absorption layer 4 covers the window layer 3, and the second electrode layer 6 covers the absorption layer 4, wherein the material of the absorption layer 4 includes at least cadmium telluride.

[0039] The absorption layer 4 can be used as a film layer in which photons are absorbed and electron-hole pairs are generated in cadmium telluride thin-film solar cells. Cadmium telluride is used as the material of the absorption layer 4 because the optical band gap width of cadmium telluride is moderate and the absorption coefficient is high. Specifically, the absorption layer 4 can adopt a CdTe single absorption layer 4 structure, or a CdSeTe / CdTe double absorption layer 4 structure. The total thickness of the absorption layer 4 can range from 3 to 5 μm. The absorption layer 4 can be manufactured using a close-space sublimation process, and the absorption layer 4 manufactured using the close-space sublimation process has a higher crystal quality.

[0040] In an embodiment of the present application, the material of the window layer 3 may be magnesium-doped tin oxide (SnO2:Mg). Since the ionic radius of magnesium ions is similar to that of tin ions, compared to the case where the material of the window layer 3 is undoped SnO2, the lattice structure of the window layer 3 made of SnO2:Mg does not change significantly, thereby ensuring the crystallization quality of SnO2:Mg, that is, magnesium-doped tin oxide can also achieve a higher crystallization quality. In addition, compared to the band structure of the window layer 3 made of undoped SnO2, the conduction band of SnO2:Mg is raised by 0.12 to 0.25 eV, referring to Figure 2 As shown in the figure, the offset between the conduction band of SnO2:Mg and the conduction band of CdTe is smaller, which is beneficial to reduce the carrier recombination at the interface between the window layer 3 and the absorption layer 4 and promote the migration of carriers at this interface. The defect state density at the undoped SnO2 / CdTe interface is inferred from the test model of space charge limited current to be 4.02×10 13 cm -3 , while the defect state density at the SnO2:Mg / CdTe interface in this application is 1.27×10 13 cm -3 That is to say, the material of the window layer 3 is SnO2:Mg, which is beneficial to suppress the defect state density at the interface between the window layer 3 and the absorption layer 4, which is beneficial to reduce carrier recombination, thereby increasing the open circuit voltage of the cadmium telluride thin film solar cell, and ultimately improving the conversion efficiency of the cadmium telluride thin film solar cell.

[0041] As an example, refer to Figure 3 As shown, Figure 3A schematic diagram of the current-voltage performance curve of a cadmium telluride thin film solar cell provided in an embodiment of the present application shows that the open circuit voltage of the cadmium telluride thin film solar cell whose window layer 3 is made of SnO2:Mg is 0.786V, and the conversion efficiency reaches 16.3%, which is significantly higher than the conversion efficiency of 14.5% when the window layer 3 is undoped SnO2.

[0042] That is to say, compared with the undoped SnO2 window layer 3, the SnO2:Mg window layer 3 as the N-type window layer 3 of the cadmium telluride thin-film solar cell can effectively suppress the defect state density at the interface of the window layer 3 / absorption layer 4 without significantly changing the lattice structure and crystal quality of SnO2. In addition, magnesium doping raises the conduction band of SnO2 by 0.12 to 0.25 eV, which is further beneficial to reduce the carrier recombination at the interface of the window layer 3 / absorption layer 4.

[0043] In the embodiment of the present application, in the window layer 3, the number of magnesium atoms accounts for 1 to 30% of the total number of tin atoms and magnesium atoms. This is because too much magnesium atoms doped into SnO2 will lead to poor crystal quality of SnO2:Mg, so high crystal quality SnO2:Mg can be achieved by controlling the concentration range of magnesium atoms doped into SnO2.

[0044] Specifically, in the window layer 3 , the number of magnesium atoms may account for 4%, 6%, 9% or 12% of the total number of tin atoms and magnesium atoms.

[0045] In the embodiment of the present application, the growth temperature of the window layer 3 is in the range of 200-500° C. The thickness of the window layer 3 is greater than or equal to 10 nm. The window layer 3 can be manufactured by radio frequency magnetron sputtering, electron beam evaporation, molecular beam epitaxy, chemical vapor deposition, sol-gel or pyrolysis spraying.

[0046] Specifically, compared with other manufacturing processes, the magnesium-doped tin oxide obtained by manufacturing the window layer 3 using the radio frequency magnetron sputtering process can achieve a higher crystallization quality, wherein the radio frequency magnetron sputtering process includes a co-sputtering process, that is, the window layer 3 can be manufactured using the co-sputtering process, and the target materials of the co-sputtering process include tin oxide and magnesium oxide, that is, the two target materials of tin oxide and magnesium oxide can be sputtered together to form the window layer 3.

[0047] As an example, the sputtering power of tin oxide is 60W, and the sputtering power of magnesium oxide ranges from 10 to 100W.

[0048] In an embodiment of the present application, after the window layer 3 is manufactured by using a radio frequency magnetron sputtering process, the window layer 3 may be heat treated, wherein the temperature range of the heat treatment may be 300 to 600° C., and the time range of the heat treatment may be 10 to 60 minutes.

[0049] Specifically, the heat treatment of the window layer 3 may be performed in air.

[0050] In the embodiment of the present application, the first electrode layer 2 may be a transparent electrode layer, and the transparent electrode layer may have a high transmittance, which can prevent light from being absorbed by the first electrode layer 2 when it is incident from the first electrode layer 2. The material of the first electrode layer 2 may be a transparent conductive glass oxide with a high transmittance, which is usually a doped wide bandgap semiconductor, such as fluorine-doped tin dioxide (SnO2:F), which may be referred to as FTO for short, and its superior transmittance can prevent light from being absorbed when light is incident into the battery, so as to ensure that more photons are absorbed by the absorption layer 4, thereby increasing the short-circuit current density of the solar cell. The transparent conductive glass oxide has excellent conductivity, which is conducive to effectively transmitting electrons in the solar cell to the negative electrode of the solar cell.

[0051] As an example, a 400 nm thick FTO conductive glass may be selected as the first electrode layer 2 .

[0052] In an embodiment of the present application, the second electrode layer 6 can be used as the positive electrode of the solar cell. The material of the second electrode layer 6 can be selected from metal materials with good conductivity, such as gold (Au) with a high work function. In addition, in order to improve the carrier transfer efficiency, the absorption layer 4 can be doped with a small amount of copper (Cu) to reduce the Schottky barrier when the second electrode layer 6 and the absorption layer 4 are in contact, so as to form an ohmic contact.

[0053] In an embodiment of the present application, the cadmium telluride thin film solar cell may further include a back electrode buffer layer 5. The material of the back electrode buffer layer 5 may be a P-type semiconductor material with a high work function. The back electrode buffer layer 5 is used to promote the transmission of holes when the second electrode layer 6 and the absorption layer 4 are in contact, and to prevent excessive diffusion of copper in the solar cell, thereby avoiding attenuation of the cell performance.

[0054] Specifically, the material of the back electrode buffer layer 5 can be ZnTe, MoO X , WO X , VO X or NiO X The thickness of the back electrode buffer layer 5 can be in the range of 50 to 100 nm.

[0055] In the embodiment of the present application, the cadmium telluride thin film solar cell may further include a transparent substrate 1, a first electrode layer 2, a window layer 3, an absorption layer 4 and a second electrode layer 6 are sequentially stacked on the transparent substrate 1, that is, the transparent substrate 1 plays the role of a device carrier and support in the solar cell. The material of the transparent substrate 1 may be glass or sapphire, and the glass may be soda-lime glass, which has the characteristics of high temperature resistance and high transmittance.

[0056] As an example, 3.2 mm thick soda lime glass may be selected as the transparent substrate 1 .

[0057] In an embodiment of the present application, the cadmium telluride thin film solar cell may further include a metal electrode layer 7, which is disposed on a side of the first electrode layer 2 away from the transparent substrate 1, and the metal electrode layer 7 and the window layer 3 are disposed together on the surface of the first electrode layer 2. The metal electrode layer 7 may serve as the negative electrode of the solar cell for electron transmission.

[0058] Specifically, the material of the metal electrode layer 7 may be a metal material with good electrical conductivity, such as gold with a high work function.

[0059] It can be seen that by using the radio frequency magnetron sputtering process to dope the tin dioxide (SnO2) window layer with an appropriate amount of magnesium, a window layer with higher crystal quality is obtained, the interface defect states of the window layer / absorption layer are passivated, and the open circuit voltage and conversion efficiency of the solar cell are effectively improved.

[0060] Based on the cadmium telluride thin film solar cell provided in the above embodiment, the present application embodiment also provides a method for manufacturing a cadmium telluride thin film solar cell, and the working principle thereof is described in detail below in conjunction with the accompanying drawings. Figure 4 , which is a schematic diagram of a process for manufacturing a cadmium telluride thin film solar cell provided in an embodiment of the present application.

[0061] The manufacturing method of the cadmium telluride thin film solar cell provided in this embodiment comprises the following steps:

[0062] S101, forming a first electrode layer on a transparent substrate.

[0063] In an embodiment of the present application, a transparent substrate may be provided, and a first electrode layer may be formed on the transparent substrate.

[0064] S102, forming a window layer on the first electrode layer.

[0065] In an embodiment of the present application, after forming the first electrode layer, a window layer is formed on the first electrode layer. The material of the window layer is magnesium-doped tin oxide. The window layer can be manufactured by radio frequency magnetron sputtering process, electron beam evaporation process, molecular beam epitaxy process, chemical vapor deposition process, sol-gel process or pyrolysis spraying process.

[0066] After the window layer is manufactured, the window layer may be heat treated to improve the crystal quality.

[0067] S103, forming an absorption layer on the window layer.

[0068] In the embodiment of the present application, after the window layer is formed, an absorption layer may be formed on the window layer. After the absorption layer is formed, the absorption layer may also be heat treated to improve the crystal quality.

[0069] S104, forming a second electrode layer on the absorption layer.

[0070] In an embodiment of the present application, after the absorption layer is formed, a second electrode layer may be further formed on the absorption layer.

[0071] In practical applications, before forming the second electrode layer, a back electrode buffer layer may be formed on the absorption layer, and then the second electrode layer is formed on the back electrode buffer layer, with the second electrode layer serving as the positive electrode of the solar cell.

[0072] While forming the second electrode layer, a metal electrode layer can also be formed on the first electrode layer to form the negative electrode of the solar cell.

[0073] It can be seen that the manufacturing method of the cadmium telluride thin film solar cell provided in the embodiment of the present application has a simple manufacturing process for manufacturing the window layer material of SnO2:Mg, and can manufacture a cadmium telluride thin film solar cell with stable performance.

[0074] The following is a detailed introduction to the manufacturing process of cadmium telluride thin film solar cells using several specific embodiments as examples:

[0075] Example 1

[0076] S1, cleaning the transparent substrate and the first electrode layer. The transparent substrate including the first electrode layer is sequentially immersed in acetone, ethanol and deionized water, cleaned in a water bath ultrasonic instrument for 1 hour, and the water on the surface of the transparent substrate is blown dry with a high-purity nitrogen gas flow.

[0077] S2, preparation of window layer. The window layer is manufactured by RF magnetron sputtering process with dual target co-sputtering process. The transparent substrate containing the first electrode layer cleaned in S1 is placed in the magnetron sputtering chamber; SnO2 target and MgO target are placed respectively, the diameter of both targets is 2 inches, and the distance between the target and the transparent substrate is about 8 cm. Turn on the transparent substrate heating function and set the temperature to 300 °C. Turn on the mechanical pump and molecular pump to evacuate the vacuum degree in the magnetron sputtering chamber to 5×10 -4 Pa. Set the power of SnO2 target to 60W, set the power of MgO target to 40W, adjust the sputtering atmosphere Ar / O2 ratio to 8:2, and the working pressure to 1.2Pa. After pre-sputtering for 10 minutes to remove pollutants adsorbed on the target surface, open the sample baffle, use a crystal oscillator film thickness meter to control the film thickness, and grow an 80nm thick SnO2:Mg film. According to EDS and other energy spectrum test methods, the atomic percentage of magnesium in the SnO2:Mg film is 4%.

[0078] S3, heat treatment of the window layer. The prepared SnO2:Mg film needs to be heat treated at high temperature to improve the electrical, optical and other properties. The prepared SnO2:Mg film is heat treated in a rapid thermal processing furnace. Specifically, the rapid thermal processing furnace is pre-adjusted to 500°C. After maintaining this temperature for 10 minutes, the transparent substrate containing the prepared SnO2:Mg film is pushed into the central working area of ​​the rapid thermal processing furnace. The heat treatment atmosphere is a dry air atmosphere, and the heat treatment time is set to 30 minutes. After the heat treatment is completed, the transparent substrate containing the SnO2:Mg film is pushed out of the cavity of the rapid thermal processing furnace and slowly cooled to room temperature.

[0079] S4, preparation and heat treatment of the absorption layer.

[0080] The absorption layer is a CdSeTe / CdTe absorption layer. First, a CdSe layer is prepared by vacuum thermal evaporation, and the required CdSeTe layer is formed by interdiffusion with subsequent CdTe. Specifically, the sample prepared by S3, which includes a transparent substrate, a first electrode layer and SnO2:Mg, is placed in a thermal evaporation instrument, and a crystal oscillator film thickness meter is used to control the growth of a 100nm CdSe film. The sample is then placed in a rapid thermal treatment furnace for a 400°C heat treatment for 15 minutes.

[0081] The CdTe absorption layer is prepared by close-space sublimation. Specifically, the above sample is placed in a close-space sublimation device, with a graphite plate supporting a CdTe powder source underneath, and the distance between the sample surface and the powder source is 3 mm. The substrate temperature is set to 560°C, the source temperature is set to 670°C, and the total thickness of the absorption layer is controlled to be 3 to 5 μm by controlling the growth time. For example, if the growth time is 400 seconds, the CdTe thickness is about 4 μm. The sample including the transparent substrate, the first electrode layer, SnO2:Mg and the absorption layer is placed in a CdCl2 atmosphere for a high-temperature heat treatment at 400°C to improve the crystallization quality of CdTe.

[0082] S5, preparation of back electrode buffer layer. A back electrode buffer layer with high work function is deposited on the CdTe layer by vacuum thermal evaporation, and a 100nm ZnTe film is deposited according to the reading of the crystal oscillator film thickness meter. About 5nm of metal copper is deposited on the ZnTe layer to reduce the Schottky barrier at the contacted part.

[0083] S6, preparation of the second electrode layer and the metal electrode layer. A layer of gold nanoparticles with a thickness of about 200 nm is deposited on the ZnTe:Cu film and the first electrode layer in S1 by vacuum thermal evaporation, respectively, to serve as the positive electrode and negative electrode of the solar cell.

[0084] Comparative Example 1

[0085] The difference from Example 1 is that the window layer prepared in S2 is a SnO2 layer. The specific description of S2 is as follows:

[0086] S2, preparation of SnO2 layer. Place the cleaned transparent substrate containing the first electrode layer in S1 in the magnetron sputtering chamber. Place SnO2 targets with a diameter of 2 inches each, and the distance between the target and the transparent substrate is about 8 cm. Turn on the mechanical pump and molecular pump, and draw the vacuum degree in the chamber to 5×10 -4 Pa. The SnO2 target power was set to 60W, the sputtering atmosphere Ar / O2 ratio was adjusted to 8:2, and the working pressure was 1.2 Pa. After pre-sputtering for 10 minutes to remove the pollutants adsorbed on the target surface, the sample baffle was opened, and the film thickness was controlled by a crystal oscillator film thickness meter to grow a 80nm thick SnO2 film.

[0087] The remaining steps S1, S3, S4, S5 and S6 are consistent with the operation process in Example 1.

[0088] refer to Figure 3As shown, the open circuit voltage of the solar cell containing the window layer of SnO2:Mg prepared in Example 1 is 0.786V, while the open circuit voltage of the solar cell containing the window layer of SnO2 prepared in Comparative Example 1 is only 0.732V. Therefore, the SnO2:Mg window layer used in Example 1 significantly improves the open circuit voltage of the solar cell, so that the energy conversion efficiency of the solar cell is increased from 14.5% of the battery with the SnO2 window layer in Comparative Example 1 to 16.3% presented in Example 1.

[0089] Example 2

[0090] The difference from Example 1 is that the power of the MgO target used for magnetron sputtering mentioned in S2 is set to 60 W. The specific description of S2 is as follows:

[0091] S2, preparation of window layer. The window layer is manufactured by RF magnetron sputtering process with dual target co-sputtering process. The transparent substrate containing the first electrode layer cleaned in S1 is placed in the magnetron sputtering chamber; SnO2 target and MgO target are placed respectively, the diameter of both targets is 2 inches, and the distance between the target and the transparent substrate is about 8 cm. Turn on the transparent substrate heating function and set the temperature to 300 °C. Turn on the mechanical pump and molecular pump to evacuate the vacuum degree in the magnetron sputtering chamber to 5×10 -4 Pa. Set the power of SnO2 target to 60W, set the power of MgO target to 60W, adjust the sputtering atmosphere Ar / O2 ratio to 8:2, and the working pressure to 1.2Pa. After pre-sputtering for 10 minutes to remove pollutants adsorbed on the target surface, open the sample baffle, use a crystal oscillator film thickness meter to control the film thickness, and grow an 80nm thick SnO2:Mg film. According to EDS and other energy spectrum test methods, the atomic percentage of magnesium in the SnO2:Mg film is 6%.

[0092] The remaining steps S1, S3, S4, S5 and S6 are consistent with the operation process in Example 1.

[0093] The conversion efficiency of the solar cell in Example 2 reaches 15.9%, which is higher than the conversion efficiency of 14.5% in Comparative Example 1.

[0094] Example 3

[0095] The difference from Example 1 is that the power of the MgO target used for magnetron sputtering mentioned in S2 is set to 80 W. The specific description of S2 is as follows:

[0096] S2, preparation of window layer. The window layer is manufactured by RF magnetron sputtering process with dual target co-sputtering process. The transparent substrate containing the first electrode layer cleaned in S1 is placed in the magnetron sputtering chamber; SnO2 target and MgO target are placed respectively, the diameter of both targets is 2 inches, and the distance between the target and the transparent substrate is about 8 cm. Turn on the transparent substrate heating function and set the temperature to 300 °C. Turn on the mechanical pump and molecular pump to evacuate the vacuum degree in the magnetron sputtering chamber to 5×10 -4 Pa. Set the power of SnO2 target to 60W, set the power of MgO target to 80W, adjust the sputtering atmosphere Ar / O2 ratio to 8:2, and the working pressure to 1.2Pa. After pre-sputtering for 10 minutes to remove pollutants adsorbed on the target surface, open the sample baffle, use a crystal oscillator film thickness meter to control the film thickness, and grow an 80nm thick SnO2:Mg film. According to EDS and other energy spectrum test methods, the atomic percentage of magnesium in the SnO2:Mg film is 9%.

[0097] The remaining steps S1, S3, S4, S5 and S6 are consistent with the operation process in Example 1.

[0098] The conversion efficiency of the solar cell in Example 3 reaches 15.1%, which is higher than the conversion efficiency of 14.5% in Comparative Example 1.

[0099] Example 4

[0100] The difference from Example 1 is that the power of the MgO target used for magnetron sputtering mentioned in S2 is set to 100 W. The specific description of S2 is as follows:

[0101] S2, preparation of window layer. The window layer is manufactured by RF magnetron sputtering process with dual target co-sputtering process. The transparent substrate containing the first electrode layer cleaned in S1 is placed in the magnetron sputtering chamber; SnO2 target and MgO target are placed respectively, the diameter of both targets is 2 inches, and the distance between the target and the transparent substrate is about 8 cm. Turn on the transparent substrate heating function and set the temperature to 300 °C. Turn on the mechanical pump and molecular pump to evacuate the vacuum degree in the magnetron sputtering chamber to 5×10 -4 Pa. Set the power of SnO2 target to 60W, set the power of MgO target to 100W, adjust the sputtering atmosphere Ar / O2 ratio to 8:2, and the working pressure to 1.2Pa. After pre-sputtering for 10 minutes to remove pollutants adsorbed on the target surface, open the sample baffle, use a crystal oscillator film thickness meter to control the film thickness, and grow an 80nm thick SnO2:Mg film. According to EDS and other energy spectrum test methods, the atomic percentage of magnesium in the SnO2:Mg film is 12%.

[0102] The remaining steps S1, S3, S4, S5 and S6 are consistent with the operation process in Example 1.

[0103] The conversion efficiency of the solar cell in Example 4 reaches 15.8%, which is higher than the conversion efficiency of 14.5% in Comparative Example 1.

[0104] Example 5

[0105] The difference from Example 1 is that the method for preparing the window layer in S2 is electron beam evaporation. The specific description of S2 is as follows:

[0106] S2, preparation of window layer. High-purity SnO2 powder and MgO powder are used as powder sources for electron beam evaporation. The atomic ratio of Sn / Mg in the prefabricated powder source is 9:1. The two powders are fully and evenly mixed and placed in a copper crucible in the electron beam evaporation equipment. The cleaned transparent substrate containing the first electrode layer in S1 is transferred to the sample stage area of ​​the coating chamber through the sample inlet chamber in the instrument. The coating chamber is evacuated to 5×10 -4 After Pa, the electron gun is turned on and the working voltage is set to 4kV. The spot position generated by the electron beam on the surface of the powder source is adjusted to the central area of ​​the powder source, and pre-growth is performed for 10 minutes. The sample baffle is opened for formal coating, and the thickness of the SnO2:Mg film is controlled to 80nm using a crystal oscillator film thickness meter. According to EDS and other energy spectrum test methods, the atomic percentage of magnesium in the SnO2:Mg film is 8%.

[0107] The remaining steps S1, S3, S4, S5 and S6 are consistent with the operation process in Example 1.

[0108] The conversion efficiency of the solar cell in Example 5 reaches 15.5%, which is higher than the conversion efficiency of 14.5% in Comparative Example 1.

[0109] Example 6

[0110] The difference from Example 1 is that the heat treatment temperature of the window layer in S3 is 400° C. The specific description of S3 is as follows:

[0111] S3, heat treatment of the window layer. The prepared SnO2:Mg film needs to be heat treated at high temperature to improve the electrical, optical and other properties. The prepared SnO2:Mg film is heat treated in a rapid thermal processing furnace. Specifically, the rapid thermal processing furnace is pre-adjusted to 400°C. After maintaining this temperature for 10 minutes, the transparent substrate containing the prepared SnO2:Mg film is pushed into the central working area of ​​the rapid thermal processing furnace. The heat treatment atmosphere is a dry air atmosphere, and the heat treatment time is set to 30 minutes. After the heat treatment is completed, the transparent substrate containing the SnO2:Mg film is pushed out of the cavity of the rapid thermal processing furnace and slowly cooled to room temperature.

[0112] The remaining steps S1, S2, S4, S5 and S6 are consistent with the operation process in Example 1.

[0113] Example 7

[0114] The difference from Example 1 is that the absorption layer in S4 is a CdTe single absorption layer. The specific description of S4 is as follows:

[0115] S4, preparation and heat treatment of the absorption layer. The absorption layer is a single absorption layer of CdTe. The CdTe absorption layer is prepared by close-space sublimation method. Specifically, the above sample is placed in a close-space sublimation method device, with a graphite plate supporting the CdTe powder source underneath, and the distance between the sample surface and the powder source is 3 mm. The substrate temperature is set to 560°C and the source temperature is set to 670°C. The total thickness of the absorption layer is controlled to be 3 to 5 μm by controlling the growth time. For example, if the growth time is 400 seconds, the CdTe thickness is about 4 μm. The sample including the transparent substrate, the first electrode layer, SnO2:Mg and the absorption layer is placed in a CdCl2 atmosphere for high-temperature heat treatment at 400°C to improve the crystallization quality of CdTe.

[0116] The remaining steps S1, S2, S3, S5 and S6 are consistent with the operation process in Example 1.

[0117] Example 8

[0118] The difference from Example 7 is that the thickness of the SnO2:Mg film in S2 is 60 nm. The specific description of S2 is as follows:

[0119] S2, preparation of window layer. The window layer is manufactured by RF magnetron sputtering process with dual target co-sputtering process. The transparent substrate containing the first electrode layer cleaned in S1 is placed in the magnetron sputtering chamber; SnO2 target and MgO target are placed respectively, the diameter of both targets is 2 inches, and the distance between the target and the transparent substrate is about 8 cm. Turn on the transparent substrate heating function and set the temperature to 300 °C. Turn on the mechanical pump and molecular pump to evacuate the vacuum degree in the magnetron sputtering chamber to 5×10 -4 Pa. Set the SnO2 target power to 60W, set the MgO target power to 40W, adjust the sputtering atmosphere Ar / O2 ratio to 8:2, and the working pressure to 1.2Pa. After pre-sputtering for 10 minutes to remove pollutants adsorbed on the target surface, open the sample baffle, use a crystal oscillator film thickness meter to control the film thickness, and grow a 60nm thick SnO2:Mg film. According to EDS and other energy spectrum test methods, the atomic percentage of magnesium in the SnO2:Mg film is 4%.

[0120] The remaining steps S1, S3, S4, S5 and S6 are consistent with the operation process in Example 7.

[0121] Example 9

[0122] The difference from Example 1 is that the back electrode buffer layer in S5 is MoO3. The specific description of S5 is as follows:

[0123] S5, preparation of the back electrode buffer layer. A 30 nm MoO3 film is prepared on the CdTe layer using a radio frequency magnetron sputtering process. Specifically, a high-purity MoO3 target is used and the vacuum degree of the chamber is pumped to 5×10 -4 After 100 Pa, a mixed gas of argon and oxygen was introduced as the working atmosphere, and the Ar / O2 ratio was controlled to be 9:1. At this time, the working pressure was 0.6 Pa. The target power was set to 50 W, and after 10 minutes of pre-sputtering, the sample baffle was opened for coating, and the MoO3 film was controlled to be 30 nm by a crystal oscillator film thickness meter.

[0124] The remaining steps S1, S2, S3, S4 and S6 are consistent with the operation process in Example 1.

[0125] The above is only a preferred implementation of the present application. Although the present application has been disclosed as a preferred embodiment, it is not intended to limit the present application. Any technician familiar with the art can use the above disclosed methods and technical contents to make many possible changes and modifications to the technical solution of the present application without departing from the scope of the technical solution of the present application, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application still falls within the scope of protection of the technical solution of the present application.

Claims

1. A cadmium telluride thin film solar cell, characterized in that: The cadmium telluride thin film solar cell comprises: a first electrode layer, a window layer, an absorption layer and a second electrode layer stacked in sequence, the material of the window layer is magnesium-doped tin oxide, and the material of the absorption layer includes at least cadmium telluride; the window layer is manufactured by using a radio frequency magnetron sputtering process.

2. The cadmium telluride thin film solar cell according to claim 1, characterized in that: In the window layer, the number of magnesium atoms accounts for 1 to 30% of the total number of tin atoms and magnesium atoms.

3. The cadmium telluride thin film solar cell according to claim 2, characterized in that: In the window layer, the number of magnesium atoms accounts for 4%, 6%, 9% or 12% of the total number of tin atoms and magnesium atoms.

4. The cadmium telluride thin film solar cell according to claim 1, characterized in that: The growth temperature range of the window layer is 200-500°C.

5. The cadmium telluride thin film solar cell according to claim 1, characterized in that: The thickness of the window layer is greater than or equal to 10 nm.

6. The cadmium telluride thin film solar cell according to claim 1, characterized in that: The radio frequency magnetron sputtering process includes a co-sputtering process; The target materials of the co-sputtering process include tin oxide and magnesium oxide.

7. The cadmium telluride thin film solar cell according to claim 6, characterized in that: The sputtering power of the tin oxide is 60W, and the sputtering power of the magnesium oxide is in the range of 10 to 100W.

8. The cadmium telluride thin film solar cell according to claim 1, characterized in that: The absorption layer is manufactured by using a close-space sublimation process.

9. The cadmium telluride thin film solar cell according to any one of claims 1 to 8, characterized in that: The window layer is subjected to a heat treatment at a temperature ranging from 300 to 600° C. and a time ranging from 10 to 60 minutes.

10. A method for manufacturing a cadmium telluride thin film solar cell, characterized in that: The method comprises: forming a first electrode layer on a transparent substrate; forming a window layer on the first electrode layer, wherein the material of the window layer is magnesium-doped tin oxide; forming an absorption layer on the window layer; A second electrode layer is formed on the absorption layer.