Solder strip for photovoltaic module and preparation method thereof
By adding Sn, Pb and anti-corrosion fillers to the outer coating of the photovoltaic ribbon, and through ultrasonic treatment and thickness control, the problems of insufficient fatigue resistance, thermal cycle and corrosion resistance of the ribbon are solved, achieving environmental protection and The balance between health and performance significantly improves welding reliability and corrosion resistance.
Patent Information
- Application Number
- CN202410865480.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
Existing photovoltaic soldering ribbons cannot reach the level of traditional tin-lead soldering ribbons in terms of fatigue resistance, thermal cycle and corrosion resistance. At the same time, there are potential damages to the environment and health. How to achieve a balance between environmental protection, health and performance is an urgent technology to be solved. question.
A welding ribbon for photovoltaic modules is provided. The outer coating layer contains Sn, Pb and anti-corrosion fillers. The anti-corrosion fillers include hydroxides, metal oxides, metal carbonates, metal sulfides, etc., and the fillers are made uniform through ultrasonic treatment. Disperse, and control the thickness of the outer cladding layer to reduce lead content while improving corrosion resistance and welding reliability.
It improves the corrosion resistance and welding reliability of the soldering ribbon, reduces the damage to the environment and health during the welding process, and maintains the basic performance of the soldering ribbon, which is significantly better than traditional lead-free soldering ribbons.
Smart Images

Figure CN118738181A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of solar cells, and in particular to a welding strip for a photovoltaic module and a preparation method thereof. Background Art
[0002] With the development of solar cell technology, from PERC cells, TOPCON cells to HJT cells, these cells have weakened their resistance to water, oxygen and acid, so the requirements for the corrosion resistance of the module packaging and connection parts are becoming more and more stringent. As one of the main auxiliary materials of photovoltaic modules, photovoltaic welding ribbon plays the role of connecting cells and conducting electricity, and plays a vital role in the quality of photovoltaic modules.
[0003] For the purpose of environmental protection and health, the materials of photovoltaic ribbons are continuously innovating and improving. However, new materials will affect the performance of photovoltaic ribbons. How to achieve a balance between environmental protection, health and performance is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present disclosure provides a soldering strip for a photovoltaic module and a preparation method thereof. The soldering strip for a photovoltaic module has a low lead content and high corrosion resistance.
[0005] In a first aspect, the present disclosure provides a welding strip for a photovoltaic module, comprising a substrate and an outer coating layer, wherein the outer coating layer contains Sn, Pb and an anti-corrosion filler.
[0006] In some embodiments, based on the total mass of the outer coating layer being 100%, the outer coating layer comprises 55%-65% Sn, 10%-25% Pb, and 5%-35% anti-corrosion filler.
[0007] In some embodiments, the outer cladding layer comprises 60%-65% Sn, 10%-20% Pb, and 10%-30% anti-corrosion filler.
[0008] In some embodiments, the anti-corrosion filler comprises one or more of hydroxides, metal oxides, metal carbonates, metal sulfides, and rare metal compounds.
[0009] In some embodiments, the corrosion-resistant filler comprises one or more of magnesium hydroxide, calcium hydroxide, zinc hydroxide, barium hydroxide, aluminum hydroxide, magnesium oxide, calcium oxide, zinc oxide, barium oxide, aluminum oxide, magnesium carbonate, calcium carbonate, zinc carbonate, barium carbonate, cadmium sulfide, cadmium selenide, cadmium telluride, zinc sulfide, zinc selenide, lead sulfide, lead selenide, indium phosphide, indium arsenide, indium gallium nitride, gallium arsenide, indium arsenide nitride, indium gallium arsenide, and cadmium selenide sulfide.
[0010] In some embodiments, the corrosion resistant filler comprises 1%-6% hydroxide, 20%-50% metal carbonate and 20%-25% metal sulfide.
[0011] In some embodiments, the melting point of the outer coating layer is between 150°C and 250°C.
[0012] In some embodiments, the melting point of the outer coating layer is between 180°C and 240°C.
[0013] In some embodiments, the melting point of the outer coating layer is between 190°C and 210°C.
[0014] In a second aspect, the present disclosure provides a method for preparing a welding tape for a photovoltaic module, which comprises the following steps: unwinding a substrate; coating an outer coating layer on the surface of the substrate, wherein the outer coating layer comprises Sn, Pb and an anti-corrosion filler; heating the outer coating layer to make it in a semi-molten state; and controlling the thickness of the outer coating layer.
[0015] In some embodiments, in the step of coating the outer coating layer, ultrasonic treatment is used to uniformly disperse the anti-corrosion filler in the outer coating layer.
[0016] In some embodiments, the ultrasonic treatment has an ultrasonic power of 150W-350W, an ultrasonic temperature of 150°C-300°C, and a holding time of 15min-50min.
[0017] In the method for preparing the welding strip for photovoltaic modules, the total thickness of the outer coating layer is controlled to account for 3%-6% of the diameter of the welding strip.
[0018] The present disclosure provides an anti-corrosion filler, which improves the corrosion resistance and welding reliability while reducing the lead content of the outer coating layer of the solder strip. It can not only reduce the damage to the environment and health caused by the lead content in the solder strip during the welding process, but also maintain the performance of the solder strip. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the structure of a welding strip for a photovoltaic module according to an embodiment of the present disclosure.
[0020] Figure 2 The present invention is a flow chart of a method for preparing a welding ribbon for a photovoltaic module according to an embodiment of the present disclosure. DETAILED DESCRIPTION
[0021] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the technical solution of the present disclosure is described in detail below with reference to the accompanying drawings.
[0022] Example embodiments will be described more fully below with reference to the accompanying drawings, but the example embodiments may be embodied in different forms and should not be construed as limited to the embodiments set forth herein. On the contrary, the purpose of providing these embodiments is to make the present disclosure thorough and complete and to enable those skilled in the art to fully understand the scope of the present disclosure.
[0023] In the absence of conflict, the various embodiments of the present disclosure and the various features therein may be combined with each other.
[0024] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.
[0025] The terms used herein are only used to describe specific embodiments and are not intended to limit the present disclosure. As used herein, the singular forms "a", "an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. It will also be understood that when the terms "comprising" and / or "made of" are used in this specification, the presence of the features, wholes, steps, operations, elements and / or components is specified, but the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or groups thereof is not excluded.
[0026] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art. It will also be understood that terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and the present disclosure, and will not be interpreted as having an idealized or overly formal meaning unless explicitly defined as such herein.
[0027] Photovoltaic solder strips are divided into tin-lead solder strips and lead-free solder strips. A lead-containing solder strip has a base material of Cu or Al, and an outer layer coated with Sn60Pb40, with a melting point of 183°C. With the advancement of the lead-free process, traditional tin-lead solder strips are gradually replaced by lead-free solder strips. A lead-free solder strip has a base material of Cu, and an outer layer coated with Sn96.5Ag3Cu0.5. The inventors of the present disclosure have found that lead-free solder strips cannot reach the same level as tin-lead solder strips in terms of fatigue resistance, thermal cycling and corrosion resistance.
[0028] In view of this, the present disclosure aims to provide a solder strip for photovoltaic modules with a low lead content, which appropriately reduces the lead content in the outer coating layer of the solder strip, but at the same time has good corrosion resistance and welding reliability.
[0029] In a first aspect, the present disclosure provides a welding strip for a photovoltaic module, referring to Figure 1 The welding strip includes a substrate and an outer coating layer, and the outer coating layer contains Sn, Pb and anti-corrosion filler.
[0030] In the present disclosure, the anti-corrosion filler is uniformly distributed in the outer coating layer.
[0031] The present disclosure does not specifically limit the ratio of Sn, Pb and corrosion-resistant filler in the outer coating layer.
[0032] In some embodiments, based on the total mass of the outer coating layer being 100%, the outer coating layer comprises 55%-65% Sn, 10%-25% Pb, and 5%-35% anti-corrosion filler.
[0033] In some embodiments, the outer cladding layer comprises 60%-65% Sn, 10%-20% Pb, and 10%-30% anti-corrosion filler.
[0034] The present disclosure provides an anti-corrosion filler, which improves the corrosion resistance and welding reliability of the solder strip while reducing the lead content of the outer coating layer of the solder strip. It can not only reduce the damage to the environment and health caused by the lead content in the solder strip during the welding process, but also maintain the performance of the solder strip.
[0035] In some embodiments, the corrosion resistant filler comprises one or more of hydroxides, metal oxides, metal carbonates, metal sulfides, and rare metal compounds.
[0036] In some embodiments, the corrosion-resistant filler comprises one or more of magnesium hydroxide, calcium hydroxide, zinc hydroxide, barium hydroxide, aluminum hydroxide, magnesium oxide, calcium oxide, zinc oxide, barium oxide, aluminum oxide, magnesium carbonate, calcium carbonate, zinc carbonate, barium carbonate, cadmium sulfide, cadmium selenide, cadmium telluride, zinc sulfide, zinc selenide, lead sulfide, lead selenide, indium phosphide, indium arsenide, indium gallium nitride, gallium arsenide, indium arsenide nitride, indium gallium arsenide, and cadmium selenide sulfide.
[0037] In the welding strip for photovoltaic modules of the present disclosure, the anti-corrosion filler may include one or more of the above substances. For example, the anti-corrosion filler includes hydroxide and metal oxide; hydroxide and metal carbonate; hydroxide, metal oxide and metal carbonate; or hydroxide, metal sulfide and rare metal compound.
[0038] In some embodiments, the corrosion-resistant filler of the solder strip for photovoltaic modules contains alkaline compounds, such as aluminum hydroxide, magnesium carbonate, etc., which can absorb the acid (such as acetic acid) generated in the EVA film after encapsulation, thereby reducing the corrosion rate and degree of the acid on the solder strip.
[0039] In some embodiments, the corrosion-resistant filler of the solder strip for photovoltaic modules contains metal oxides, which can absorb water vapor generated in the module and convert it into alkaline salts, thereby absorbing the acid generated in the EVA film after packaging, reducing the corrosion rate and degree of acid on the solder strip.
[0040] In some embodiments, the corrosion-resistant filler of the solder strip for photovoltaic modules contains metal sulfides and / or rare earth compounds. When the photovoltaic module is powered on, if used as an anode, the metal sulfide and / or rare earth compound will lose electrons and be oxidized; if used as a cathode, the metal sulfide and / or rare earth compound will play a protective role to prevent metal elements such as Cu, Pb, Zn in the solder strip from being corroded.
[0041] In some embodiments, the corrosion-resistant filler of the solder strip for photovoltaic modules includes a combination of one or more alkaline compounds, metal oxides, metal sulfides, and rare earth compounds. Through the above-mentioned mechanism and its combination, the one or more combinations of alkaline compounds, metal oxides, metal sulfides, and rare earth compounds can protect the solder strip and improve the corrosion resistance.
[0042] When the anti-corrosion filler contains multiple substances, the content of each substance is not particularly limited in the present disclosure. In the present disclosure, the content of each substance can be adjusted as needed.
[0043] In some embodiments, the anti-corrosion filler comprises 1%-20% hydroxide and 80%-99% metal oxide.
[0044] In some embodiments, the corrosion resistant filler comprises 1%-6% hydroxide, 20%-50% metal carbonate, and 44%-79% metal sulfide.
[0045] In some embodiments, the anti-corrosion filler includes 1%-6% magnesium hydroxide + 20%-50% indium phosphide + 44%-79% zinc sulfide.
[0046] In some embodiments, in the welding tape for photovoltaic modules provided by the present disclosure, the melting point of the outer coating layer is between 150°C and 250°C.
[0047] In some embodiments, in the welding tape for photovoltaic modules provided by the present disclosure, the melting point of the outer coating layer is between 180°C and 240°C.
[0048] In some embodiments, in the welding tape for photovoltaic modules provided by the present disclosure, the melting point of the outer coating layer is between 190°C and 210°C.
[0049] In a second aspect, the present disclosure provides a method for preparing a solder strip for a photovoltaic module, referring to Figure 2 , which comprises the following steps:
[0050] S1, unwinding substrate;
[0051] S2, coating an outer coating layer on the surface of the substrate, wherein the outer coating layer comprises Sn, Pb and an anti-corrosion filler;
[0052] S3, heating the outer coating layer to make it in a semi-molten state; and
[0053] S4. Control the thickness of the outer coating layer.
[0054] The present disclosure does not specifically limit the substrate in the photovoltaic module welding strip, and a suitable substrate can be selected as needed. In some embodiments, multiple quenched oxygen-free copper is selected as the substrate to ensure the conductivity of the welding strip and reduce the volume resistance.
[0055] In some embodiments, a substrate is unwound by an unwinding device; an outer coating layer is coated on the surface of the substrate by a tinning device, wherein the outer coating layer comprises Sn, Pb and an anti-corrosion filler; the outer coating layer is heated by a heating device to be in a semi-molten state; and the thickness of the outer coating layer is controlled by a coating device.
[0056] In the process of preparing the solder strip for the photovoltaic module, the unwinding device is used to unwind the substrate, the tinning device is arranged on one side of the unwinding device, and the tinning device may include a moving component and a tin furnace or a tinning tank arranged on the moving component, and the tin furnace or the tinning tank is provided with a SnPb outer coating material.
[0057] The present disclosure does not specifically limit how to prepare the outer coating material with anti-corrosion filler into the outer coating layer, and a suitable process can be selected as needed to prepare the outer coating material with anti-corrosion filler into the outer coating layer. In some embodiments, the outer coating material with anti-corrosion filler is placed in a tinning bath, and the outer coating layer is processed by hot dipping.
[0058] In the present disclosure, the outer coating layer is heated by a heating device to make the SnPb outer coating material in a semi-molten state. In some embodiments, the anti-corrosion filler added to the SnPb outer coating material is added in a ratio of 5wt%-35wt%.
[0059] In some embodiments, when coating the outer coating layer, ultrasonic treatment is used to evenly distribute the anti-corrosion filler in the outer coating layer. For example, an ultrasonic dispersion process is added to the tinning tank of the tinning device to evenly disperse the anti-corrosion filler in the tinning tank.
[0060] In some embodiments, during the ultrasonic treatment, the ultrasonic power is 150W-350W, the ultrasonic temperature is 150°C-300°C, and the holding time is 15min-50min.
[0061] In some embodiments, during the ultrasonic treatment, the ultrasonic power is 200 W, the ultrasonic time is 30 min, and the ultrasonic temperature is 200° C.
[0062] In the present disclosure, ultrasonic treatment is used when coating the outer coating layer to increase the dispersion density of the anti-corrosion filler in the tin-lead alloy plating solution and reduce agglomeration.
[0063] In some embodiments, controlling the thickness of the outer coating layer includes removing a portion of the coating in a semi-molten state using a coating device to control the thickness of the outer coating layer. In some embodiments, by controlling the thickness of the outer coating layer, the thickness of the outer coating layer accounts for 3%-6% of the diameter of the welding strip. For example, the thickness of the outer coating layer accounts for 4.5% of the diameter of the welding strip.
[0064] For example, the coating device includes a wind knife structure and a coating mold. The wind knife structure includes a wind knife bracket and a manual slide. The wind knife bracket is connected to the wind knife. The manual slide is connected to the wind knife bracket. The manual slide is used to control the distance between the wind knife and the tinning device.
[0065] The solder strip for photovoltaic modules prepared by the preparation method provided by the present invention has a low lead content in the outer coating layer, and the basic properties of the solder strip, such as yield strength, tensile strength, elongation, and resistivity per meter, are substantially equivalent to those of the solder strip in the related art. At the same time, the corrosion resistance and welding reliability of the solder strip are improved, which can reduce the damage to the environment and health caused by the lead content in the solder strip during the welding process, and can also maintain the performance of the solder strip.
[0066] In order to enable those skilled in the art to more clearly understand the technical solution of the present disclosure, the technical solution of the present disclosure is described in detail below through specific embodiments:
[0067] Example 1
[0068] Oxygen-free copper (Cu≥99.97%) of brand TU1 is used as the substrate, and the substrate is unwound by an unwinding device;
[0069] An outer coating layer is coated on the surface of the substrate by a tin plating device, wherein the outer coating layer contains 55% Sn, 10% Pb and 35% anti-corrosion filler, and the anti-corrosion filler includes 3% magnesium hydroxide + 22% indium phosphide + 75% zinc sulfide; the anti-corrosion filler is evenly dispersed in the outer coating layer by ultrasonic treatment, the power of the ultrasonic treatment is 350W, the ultrasonic temperature is 200°C, and the holding time is 20min.
[0070] Heating the outer coating layer by a heating device to make it in a semi-molten state; and
[0071] The coating device is used to control the thickness of the outer coating layer to be 3% of the diameter of the welding strip.
[0072] Example 2
[0073] The welding strip was prepared using the same processing steps and conditions as in Example 1, except that:
[0074] The outer coating layer contains 60% Sn, 15% Pb and 25% anti-corrosion filler, and the anti-corrosion filler includes 5% calcium hydroxide + 25% zinc carbonate + 70% lead sulfide;
[0075] The ultrasonic treatment power is 200W, the ultrasonic temperature is 300°C, and the holding time is 40min; and
[0076] The thickness of the outer coating layer is controlled to be 5% of the diameter of the welding strip.
[0077] Example 3
[0078] The welding strip was prepared using the same processing steps and conditions as in Example 1, except that:
[0079] The outer coating layer comprises 65% Sn, 25% Pb and 10% corrosion resistant filler, wherein the corrosion resistant filler comprises 40% calcium carbonate + 60% alumina;
[0080] The ultrasonic treatment power is 250W, the ultrasonic temperature is 200°C, and the holding time is 50min; and
[0081] The thickness of the outer coating layer is controlled to be 6% of the diameter of the welding strip.
[0082] Comparative Example
[0083] A commercially available PbSn solder strip was used as a representative of a conventional solder strip, and various indicators shown in Table 1 were tested and compared with the products of Examples 1-3 in the present disclosure.
[0084] Table 1
[0085]
[0086]
[0087] It can be seen from the data in Table 1 that the photovoltaic module soldering strips provided in Examples 1-3 are substantially equivalent to the commercially available soldering strips in terms of yield strength, tensile strength, elongation, and resistivity per meter. That is, the photovoltaic module soldering strips provided in Examples 1-3 reduce the lead content of the outer covering layer while ensuring that the basic performance of the soldering strips will not deteriorate.
[0088] In addition, corrosion resistance test and power attenuation test were performed on the welding strips in Examples 1-3 of the present disclosure and the comparative examples.
[0089] Corrosion resistance test:
[0090] Under the same conditions, the welding strips of the comparative example and the embodiment were placed in a 3% acetic acid solution, then sealed and heated to 85°C and left for 24 hours. The resistance of the welding strip line was tested. The resistance of the welding strip line of the comparative example increased by 30%, and the resistance increase of the welding strips for photovoltaic modules provided by Examples 1-3 was less than 10%. Obviously, the welding strips for photovoltaic modules provided by Examples 1-3 are far superior to the welding strips of the comparative example.
[0091] Power reduction test:
[0092] The photovoltaic modules were packaged using the welding strips of the embodiment and the comparative example and the power attenuation of the modules was tested. The attenuation of the photovoltaic modules provided by the welding strips of the embodiments 1 to 3 after the TOPCON single-glass DH1000 test was less than 2%, and the attenuation of the comparative example welding strips after the TOPCON single-glass DH1000 test was greater than 5%.
[0093] According to the comparison of the above test results, it can be seen that the basic properties of the welding strip provided by the present invention, such as yield strength, tensile strength, elongation, and resistance per meter, are guaranteed, while the corrosion resistance and welding reliability are improved, which is beneficial to improving the performance of the photovoltaic modules using the welding strip provided by the present invention.
[0094] Example embodiments have been disclosed herein, and although specific terms are employed, they are used and should be interpreted only in a general illustrative sense and not for limiting purposes. In some instances, it will be apparent to those skilled in the art that, unless otherwise expressly noted, features, characteristics, and / or elements described in conjunction with a particular embodiment may be used alone or in combination with features, characteristics, and / or elements described in conjunction with other embodiments. Therefore, those skilled in the art will appreciate that various changes in form and detail may be made without departing from the scope of the present disclosure as set forth in the appended claims.
Claims
1. A welding ribbon for a photovoltaic module, comprising: A substrate and an outer cladding layer, wherein the outer cladding layer comprises Sn, Pb and an anti-corrosion filler.
2. The photovoltaic module welding strip according to claim 1, wherein: Based on the total mass of the outer coating layer being 100%, the outer coating layer comprises 55%-65% of Sn, 10%-25% of Pb and 5%-35% of the anti-corrosion filler.
3. The photovoltaic module welding strip according to claim 1, wherein: Based on the total mass of the outer coating layer being 100%, the outer coating layer comprises 60%-65% of Sn, 10%-15% of Pb and 10%-35% of anti-corrosion filler.
4. The photovoltaic module welding strip according to claim 1, wherein: The anti-corrosion filler comprises one or more of hydroxides, metal oxides, metal carbonates, metal sulfides, and rare metal compounds.
5. The photovoltaic module welding strip according to claim 4, wherein: The corrosion-resistant filler comprises one or more of magnesium hydroxide, calcium hydroxide, zinc hydroxide, barium hydroxide, aluminum hydroxide, magnesium oxide, calcium oxide, zinc oxide, barium oxide, aluminum oxide, magnesium carbonate, calcium carbonate, zinc carbonate, barium carbonate, cadmium sulfide, cadmium selenide, cadmium telluride, zinc sulfide, zinc selenide, lead sulfide, lead selenide, indium phosphide, indium arsenide, indium gallium nitride, gallium arsenide, indium arsenide nitride, indium gallium arsenide, and cadmium selenide sulfide.
6. The welding strip for photovoltaic modules according to any one of claims 1 to 4, wherein: The anti-corrosion filler contains 1%-6% of hydroxide, 20%-50% of metal carbonate and 20%-25% of metal sulfide.
7. The welding strip for photovoltaic modules according to any one of claims 1 to 4, wherein the melting point of the outer coating layer is between 150°C and 250°C.
8. A method for preparing a welding ribbon for a photovoltaic module, comprising the following steps: Unwinding the substrate; Coating an outer coating layer on the surface of the substrate, wherein the outer coating layer comprises Sn, Pb and an anti-corrosion filler; Heating the outer coating layer to make it in a semi-molten state; as well as Controls the thickness of the outer cladding layer.
9. The method for preparing the welding strip for photovoltaic modules according to claim 8, wherein: In the step of coating the outer coating layer, ultrasonic treatment is used to uniformly distribute the anti-corrosion filler in the outer coating layer.
10. The method for preparing the welding ribbon for photovoltaic modules according to claim 9, wherein: The ultrasonic treatment has an ultrasonic power of 150W-350W, an ultrasonic temperature of 150°C-300°C, and a holding time of 15min-50min.
11. The method for preparing a welding ribbon for a photovoltaic module according to claim 8, wherein: The total thickness of the outer coating layer is controlled to be 3%-6% of the diameter of the welding strip.