Electrode plate and preparation method thereof
By adopting a double-layer coating structure on the lithium-ion battery pole pieces and adjusting the gradient distribution of the binder content, the problem of insufficient adhesion at the interface between the pole pieces and the separator is solved, and the high-temperature fast charge cycle performance and ion transmission efficiency of the battery are improved. Reduced costs.
Patent Information
- Application Number
- CN202310316220.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
The interface adhesion between the lithium-ion battery pole pieces and the separator is insufficient, resulting in increased lithium ion transmission paths, increased internal resistance, and poor cycle stability. The uniform distribution of the binder content in the traditional coating cannot meet the requirements of the separator and current collector. Specific bonding requirements are required, and increasing the amount of adhesive will increase costs and worsen the pole piece impedance.
Adopting a double-layer coating structure, the first coating binder content is 0.3~0.7wt%, the second coating binder content is 2.2~3.8wt%, and the weight ratio per unit area of the two is 2:8. The dual-cavity die is coated and dried simultaneously to achieve gradient distribution of binder content, specifically meeting the bonding needs of the separator and current collector.
The high-temperature fast charging cycle performance of the electrode sheet is improved, the interface resistance is reduced, the bonding requirements of the separator and the current collector are specifically met, the cost is reduced, and the ion transmission efficiency is improved.
Smart Images

Figure CN118738262A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to an electrode sheet and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have become one of the preferred power sources for commercial electric vehicles due to their high energy density, high power density, and low self-discharge rate. As the charging rate continues to increase, the dynamic requirements for lithium battery pole pieces are also getting higher and higher. Lithium-ion batteries are composed of four main functional parts: positive electrode, negative electrode, electrolyte, and diaphragm. The main function of the diaphragm is to provide a physical barrier between the electrodes to prevent short circuits, and it also provides a transmission channel for lithium ions. The interfacial adhesion between the electrode and the diaphragm has a great influence on the battery performance. If the adhesion between the pole piece and the diaphragm is not good and there is an interfacial gap, it will lead to an increase in the lithium ion transmission path, an increase in internal resistance, and a deterioration in cycle stability.
[0003] Due to the different materials of the diaphragm and the pole piece, their interface adhesion is different. The binder content in the traditional pole piece coating is evenly distributed in the thickness direction of the pole piece, which cannot specifically meet the bonding requirements of the diaphragm and the current collector. If the amount of binder is simply increased, it will not only increase the material cost, but also worsen the pole piece impedance and affect the battery's cycle rate performance. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to:
[0005] In a first aspect, an electrode sheet is provided, the key of which is that it comprises:
[0006] current collector;
[0007] A coating layer is applied on the surface of the current collector, wherein the raw materials of the coating layer at least include active materials, conductive agents and binders;
[0008] The content of the binder in the coating increases gradually from near to far relative to the current collector surface in the thickness direction.
[0009] In combination with the first aspect, in one implementation, the coating includes:
[0010] A first coating layer is provided on the surface of the current collector;
[0011] A second coating layer is provided on the surface of the first coating layer;
[0012] The binder content of the first coating layer is less than the binder content of the second coating layer.
[0013] In combination with the first aspect, in one implementation, the binder content in the first coating is 0.3-0.7 wt %.
[0014] In combination with the first aspect, in one implementation, the binder content in the second coating layer is 2.2-3.8 wt %.
[0015] In combination with the first aspect, in one implementation, the binder content of the first coating layer is 0.5 wt %; the binder content of the second coating layer is 3.0 wt %.
[0016] In combination with the first aspect, in one implementation, the weight ratio per unit area of the second coating layer to the first coating layer is 2:8.
[0017] In combination with the first aspect, in one implementation, the current collector includes a positive electrode current collector or a negative electrode current collector.
[0018] In combination with the first aspect, in one implementation, the current collector is a negative electrode current collector, and the binder in the coating is any one or more of styrene acrylic rubber and styrene butadiene rubber.
[0019] In combination with the first aspect, in one implementation, both surfaces of the current collector are provided with a first coating and a second coating.
[0020] In a second aspect, a method for preparing the electrode sheet in any implementation of the first aspect is provided, the key of which is that the method comprises the following steps:
[0021] a. Prepare the slurry of the first coating and the slurry of the second coating according to the requirements of the raw material binder content;
[0022] b. Applying the slurry of the first coating layer and the slurry of the second coating layer simultaneously, wherein the slurry of the first coating layer covers the surface of the current collector as the first coating layer, and the slurry of the second coating layer covers the surface of the first coating layer as the second coating layer; after the first coating layer and the second coating layer are blended and dried, an electrode sheet is obtained.
[0023] As described above, an electrode sheet and a method for preparing the same according to the present invention have at least the following beneficial effects:
[0024] 1. The content of the binder changes gradually in the thickness direction of the electrode sheet, and according to the different interfacial adhesion between the diaphragm and the current collector, the content of the binder on the side of the coating bonded to the diaphragm is higher than the content of the binder on the side bonded to the current collector. The coating on the diaphragm side and the coating on the current collector side can independently adjust the binder content to specifically meet the bonding requirements of the diaphragm and the current collector; it can ensure the required interfacial adhesion on the current collector side and improve the interfacial adhesion on the diaphragm side without changing the overall ratio of the coating slurry.
[0025] 2. When multiple layers of coating are applied simultaneously, before drying, the interfaces between adjacent coatings can be fully blended, which can reduce the interface gaps between the coatings and improve the adhesion between adjacent coatings, thereby reducing the interface impedance between the double layers and improving the ion transmission efficiency, which has a positive effect on improving the fast charging cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic structural diagram of an electrode sheet shown in an exemplary embodiment of the present invention;
[0027] Figure 2 is a schematic diagram of the microstructure of an electrode sheet shown in an exemplary embodiment of the present invention;
[0028] Figure 3 It is a schematic diagram of applying a double-layer coating by a double-cavity die head in Examples 1 to 3 of the present invention;
[0029] Figure 4 This is a schematic diagram of the structure of a single side of a double-layer coating according to Example 3 of the present invention;
[0030] Figure 5 It is a schematic structural diagram of a single surface of a single-layer coating in Comparative Example 1 of the present invention.
[0031] Among them, 1 is current collector; 2 is first coating; 3 is second coating; 4 is double-cavity die. DETAILED DESCRIPTION
[0032] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.
[0033] In the following description, numerous details are discussed to provide a more thorough explanation of the embodiments of the present invention. However, it is obvious to those skilled in the art that the embodiments of the present invention can be implemented without these specific details. In other embodiments, well-known structures and devices are shown in schematic form rather than in detail to avoid making the embodiments of the present invention difficult to understand.
[0034] It should be noted that:
[0035] The current collector refers to a conductor that collects the generated current, extracts electrical energy from the battery, and connects to the tab to transmit electricity to the outside. It is also the path for current to flow from the electrode layer coated with active materials to the tab.
[0036] The diaphragm is a flexible membrane material used to separate the positive and negative electrodes of a battery. It prevents the two electrodes from contacting and causing a short circuit while allowing ions in the electrolyte to pass through.
[0037] Binder, also known as adhesive, is a substance that tightly binds the active material, conductive agent and current collector in the electrode material to enhance the electrical connection between the active material and the conductive agent and between the active material and the current collector, and stabilize the electrode structure. In the scheme of the present invention, the current collector includes a negative electrode current collector or a positive electrode current collector, wherein the negative electrode current collector generally adopts one or more of styrene-propylene rubber and styrene-butadiene rubber, and the positive electrode current collector generally adopts polyvinylidene fluoride, referred to as PVDF.
[0038] The conductive agent is an additive that is interposed between active material particles to improve conductivity (secure a conductive path).
[0039] The thickness direction usually refers to the longitudinal cutting direction of the material, and in the case of the present invention, it specifically refers to the direction perpendicular to the surface of the current collector and from one surface of the current collector to the other surface.
[0040] Figure 1 This is a schematic diagram of the structure of an electrode sheet of the present invention. Figure 1 As shown, an electrode sheet includes a current collector and a coating applied on the surface of the current collector, wherein the raw materials of the coating include at least an active material, a conductive agent and a binder, and may also include a thickener and a solvent, etc.; the content of the binder in the coating increases in a gradient from near to far relative to the surface of the current collector in the thickness direction. If the technology permits, the binder content in the coating can be increased uniformly with a minimum gradient, or the coating can be divided into multiple layers, and the binder content of each layer increases in sequence from near to far along the thickness direction of the current collector.
[0041] Of course, at present, the best choice is to use two layers of coating, namely the first coating and the second coating, the first coating is arranged on the surface of the current collector; the second coating is arranged on the surface of the first coating; the binder content of the first coating is less than the binder content of the second coating. Two layers of coating can specifically meet the bonding requirements of the diaphragm and the current collector. If more coatings are provided, the process difficulty will increase.
[0042] Examples 1 to 3 are specifically described using a negative electrode sheet with a double-sided double-layer coating as an example:
[0043] 1. Steps and methods:
[0044] (1) The binder is mixed with graphite, a conductive agent, a thickener, and a solvent according to the content ratio requirements in Table 1 to prepare the slurry of the first coating layer and the slurry of the second coating layer respectively.
[0045] (2) Figure 3As shown, the output of the first coating slurry and the second coating slurry is controlled by a double-cavity die head, and the second coating slurry is coated simultaneously at a weight ratio of 2:8 per unit area of the first coating slurry, and the first coating slurry is covered on the surface of the current collector as the first coating; the second coating slurry is covered on the surface of the first coating as the second coating; after drying in an oven, a negative electrode sheet with different binder contents in the upper and lower coatings is obtained, as shown in Figure 1 and 2 shown.
[0046] 2. High temperature fast charging cycle performance test:
[0047] In an oven at 45°C, cyclic charge and discharge were performed in a specified potential range with a 20-min fast charge process, and the discharge capacity of each cycle was recorded. The test was terminated when the battery capacity reached 80% of the first cycle capacity.
[0048] 3. Parameters and results:
[0049] The specific parameters and high temperature fast charging cycle performance test results of each embodiment are shown in Table 1:
[0050] Table 1 shows the high temperature fast charge cycle performance test results of electrode sheets with different binder contents in the scheme of the present invention
[0051] Among them, the total binder content A in the two coating layers is:
[0052] Example 1: A = 3.8wt% × 0.2 + 0.3wt × 0.8 = 1wt%;
[0053] Example 2: A = 2.2wt% × 0.2 + 0.7wt × 0.8 = 1wt%;
[0054] Example 3: A = 3.0wt% x 0.2 + 0.5wt x 0.8 = 1wt%.
[0055] Comparative Example 1 is specifically described by taking a negative electrode sheet with a double-sided single-layer coating as an example:
[0056] The binder content ratio is according to the requirements of Table 2, and the graphite, conductive agent, thickener, and solvent are mixed to obtain a coating slurry, and a single layer of the coating slurry is applied on the surface of the negative electrode current collector, such as Figure 5 As shown, a single-layer coating with uniform binder distribution is obtained, and the weight per unit area of the single-layer coating is the same as the weight per unit area of the first coating and the second coating in Example 1, 2 or 3, and the weight percentage content of the binder in the single-layer coating is consistent with the weight percentage content of the binder in the first coating and the second coating in Example 1, 2 or 3, both reaching 1wt%. Then, a "high-temperature fast-charge cycle performance test" is carried out, and the results are shown in Table 2.
[0057] Among them, compared with Examples 1 and 2, the high-temperature fast-charging cycle performance of the electrode sheet of Example 3 is the best.
[0058] Comparative Examples 2 and 3 are specifically described by taking the negative electrode sheet with double-sided double-layer coating as an example:
[0059] 1. Mix the binder with graphite, conductive agent, thickener and solvent according to the content ratio requirements in Table 2 to prepare the slurry of the first coating layer and the slurry of the second coating layer respectively.
[0060] 2. If Figure 3 As shown, the output of the first coating slurry and the second coating slurry is controlled by a double-cavity die head, and the second coating slurry is coated simultaneously at a weight ratio of 2:8 per unit area of the first coating slurry, and the first coating slurry is covered on the surface of the current collector as the first coating; the second coating slurry is covered on the surface of the first coating as the second coating; after oven drying, the negative electrode sheet with different binder contents in the upper and lower coatings is obtained. Then the "high temperature fast charging cycle performance test" is carried out, and the results are shown in Table 2.
[0061] Table 2 shows the high temperature fast charge cycle performance test results of the electrode sheets in Comparative Examples 1 to 3
[0062]
[0063] 3. Results comparison and analysis:
[0064] (1) Comparison of the single-layer coating of Comparative Example 1 with the double-layer coating of Examples 1 to 3
[0065] Results: The high temperature fast charge cycle performance of Examples 1 to 3 is higher than that of Comparative Example 1.
[0066] Analysis: The two sides of the coating will be bonded to the current collector and the diaphragm respectively, and the bonding requirements of the current collector and the diaphragm are different. The adhesive in Example 1 is evenly distributed. While meeting the bonding requirements on one side of the current collector, the amount of adhesive is not increased, so the bonding requirements on one side of the diaphragm are not met. As a result, when the coating and the diaphragm are bonded, the bonding effect is not optimal and there is an interface gap, which affects the high-temperature fast charging performance.
[0067] In Examples 1 to 3, the binder content in the first coating layer close to the current collector is higher than that in the second coating layer away from the current collector. Compared with Comparative Example 1, this is equivalent to redistributing the same amount of binder in the thickness direction of the coating layer. While meeting the bonding requirements on the current collector side, the excess binder is used on the diaphragm side. This not only ensures the bonding requirements on the current collector side, but also specifically meets the bonding requirements on the diaphragm side. There is no need to increase the amount of binder, thereby reducing costs and improving the high-temperature fast charging cycle performance of the electrode.
[0068] (2) Comparison of the double-layer coatings in Comparative Examples 2 and 3 with the double-layer coatings in Examples 1 to 3
[0069] Results: The high temperature fast charge cycle performance of Examples 1 to 3 is higher than that of Comparative Examples 2 and 3.
[0070] Analysis: A high binder content helps improve the adhesion between the coating and the current collector and separator, reduces the interfacial gap, and improves the high-temperature fast-charge cycle performance of the electrode. The binder content should not be too high, because on the one hand, it cannot significantly improve the adhesion and fast-charge performance, and on the other hand, it will increase the cost. Similarly, if the binder content is too low, the interfacial adhesion will decrease, so a suitable binder content distribution range is required.
[0071] In Comparative Example 2, the binder content of the second coating is too low to meet the interface bonding requirements of the diaphragm. The binder content of the first coating is relatively high. On the basis of meeting the bonding requirements, the binder content is somewhat redundant. Although the binder content of the double-layer coating has a gradient change, it cannot specifically meet the bonding requirements of the current collector side and the diaphragm side. Therefore, in Comparative Example 2, the fast charging performance of the electrode is reduced due to the low content of the second coating.
[0072] In Comparative Example 3, the binder content of the second coating is relatively high. On the basis of meeting the bonding requirements, the binder content is sufficient. The binder content of the first coating is too low and cannot meet the interface bonding requirements of the current collector. Although the binder content of the double-layer coating changes gradually, it also cannot specifically meet the bonding requirements of the current collector side and the diaphragm side. Therefore, in Comparative Example 3, the fast charging performance of the electrode is reduced due to the low content of the first coating.
[0073] In summary:
[0074] In the traditional coating and its coating process, it is impossible to specifically meet the bonding requirements of the same diaphragm and current collector. In the coating method of the electrocoating of the present invention, the double-layer coating is extruded and coated simultaneously through a double-cavity die head. Before drying, the interface between adjacent coatings can be fully blended, which can reduce the interface gap between the coatings and improve the bonding strength between adjacent coatings, thereby reducing the interface impedance between the double layers, improving the ion transmission efficiency, and having a positive effect on improving the fast charging cycle.
[0075] Under high-rate charge and discharge conditions, liquid phase transmission impedance is increasingly becoming a bottleneck factor limiting fast charging capabilities, so improving interfacial adhesion and reducing interfacial gaps have a positive effect on improving fast charging performance. Therefore, a high binder content in the coating away from the current collector helps improve the adhesion between the coating and the diaphragm, and can reduce the interfacial gap between the coating and the diaphragm, thereby improving fast charging performance.
[0076] The cycle stability depends on both the transmission rate of the interface, reducing the impedance and lithium deposition during the cycle, and the bonding effect between the membrane and the current collector, reducing the occurrence of film peeling. Therefore, the binder content of the outer coating should not be too high, which will increase the cost and the improvement of fast charging performance will not be obvious; at the same time, the binder content in the coating close to the current collector should not be too low, otherwise it will cause the adhesion between the active material and the current collector to decrease.
[0077] Therefore, a suitable binder content distribution range is required, and the binder content in the first coating layer is determined to be 0.3-0.7 wt %, and the binder content in the second coating layer is determined to be 2.2-3.8 wt %.
[0078] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. An electrode sheet, characterized in that: include: current collector; A coating layer is applied on the surface of the current collector, wherein the raw materials of the coating layer at least include active materials, conductive agents and binders; The content of the binder in the coating increases gradually from near to far relative to the current collector surface in the thickness direction.
2. The electrode sheet according to claim 1, characterized in that: The coating comprises: A first coating layer is provided on the surface of the current collector; A second coating layer is provided on the surface of the first coating layer; The binder content of the first coating layer is less than the binder content of the second coating layer.
3. The electrode sheet according to claim 2, characterized in that: The binder content in the first coating layer is 0.3-0.7 wt %.
4. The electrode sheet according to claim 2, characterized in that: The binder content in the second coating layer is 2.2-3.8 wt %.
5. The electrode sheet according to claim 2, characterized in that: The binder content of the first coating layer is 0.5 wt %; the binder content of the second coating layer is 3.0 wt %.
6. The electrode sheet according to any one of claims 1 to 5, characterized in that: The weight ratio per unit area of the second coating layer to the first coating layer is 2:
8.
7. The electrode sheet according to any one of claims 1 to 5, characterized in that: The current collector includes a positive electrode current collector or a negative electrode current collector.
8. The electrode sheet according to any one of claims 1 to 5, characterized in that: The current collector is a negative electrode current collector, and the binder in the coating is any one or more of styrene acrylic rubber and styrene butadiene rubber.
9. The electrode sheet according to claim 1, characterized in that: Both surfaces of the current collector are provided with a first coating layer and a second coating layer.
10. A method for preparing the electrode sheet according to any one of claims 1 to 9, characterized in that: The following steps are involved: a. Prepare the slurry of the first coating and the slurry of the second coating according to the binder content requirements; b. Applying the slurry of the first coating layer and the slurry of the second coating layer simultaneously, wherein the slurry of the first coating layer covers the surface of the current collector as the first coating layer, and the slurry of the second coating layer covers the surface of the first coating layer as the second coating layer; The first coating layer and the second coating layer are blended and dried to obtain an electrode sheet.
Citation Information
Cited By
Safety coating and application thereof, electrode plate and lithium ion battery
CN118970023A