Lithium-rich oxyhalide solid electrolyte material, preparation method and application thereof, and lithium ion secondary battery

By developing lithium-rich oxyhalide solid electrolyte materials, the problems of safety and low energy density of lithium-ion batteries are solved, high ion conductivity and stability are achieved, which is suitable for lithium-ion secondary batteries and improves the safety of energy storage equipment. sex and efficiency.

CN118738527APending Publication Date: 2024-10-01SHENZHEN UNIV
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202310368893.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have poor safety and low energy density. The liquid electrolyte is prone to leakage, combustion or explosion. Moreover, the existing halide solid electrolyte has low ionic conductivity and insufficient electrochemical stability.

Method used

Develop a lithium-rich oxyhalide solid electrolyte material with the general chemical formula Li4+xA1-xBxCl4-xO2+0.5x. A and B are specific metal ions, which are prepared by mixing and processing methods in different proportions to form high ionic conductivity. efficiency and stable electrochemical performance.

Benefits of technology

It achieves high ionic conductivity, wide electrochemical window, good compatibility and stability, avoids reaction and combustion with oxygen, and improves the safety performance and energy storage efficiency of lithium-ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738527A_ABST
    Figure CN118738527A_ABST
Patent Text Reader

Abstract

The invention provides a lithium-rich oxyhalide solid electrolyte material, a preparation method and application thereof, and a lithium ion secondary battery. The preparation method of the lithium-rich oxyhalide solid electrolyte material provided by the invention is simple and convenient, the raw materials are low in price, and actual production is facilitated. The prepared lithium-rich oxyhalide solid electrolyte material has a wide electrochemical window, good compatibility with a high-voltage positive electrode, good stability in dry air, extremely high oxygen resistance, no reaction with oxygen, no combustion and higher safety; the ionic conductivity at room temperature reaches 1 * 10 <-3 > S cm <-1 > or above, and the obtained material is stable in electrochemical performance and can be applied to a lithium ion secondary battery. When the lithium-rich oxyhalide solid electrolyte material disclosed by the invention is applied to preparation of a lithium secondary battery, the obtained secondary battery is high in first-circle coulombic efficiency, good in cycling stability and safety performance and extremely high in application prospect in various energy storage devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of rechargeable lithium-ion batteries, and in particular to a lithium-rich oxygen halide solid electrolyte material, a preparation method and application thereof, and a lithium-ion secondary battery. Background Art

[0002] Lithium-ion batteries have been widely used in new energy vehicles, wearable devices, electronic products and other fields. However, with the large-scale application of lithium-ion batteries, their poor safety and low energy density have also been infinitely magnified. Safety is an important metric for portable electronic devices and new energy vehicles. However, there are endless safety accidents in the current lithium-ion battery applications, such as mobile phone battery explosions, new energy vehicles spontaneous combustion without other external interference, etc. The potential safety hazards of lithium batteries are the main cause of these safety accidents. Currently, commercial lithium batteries all use liquid electrolytes, which leads to safety hazards such as leakage, fire and even explosion when lithium batteries are squeezed and collided. The emergence of inorganic solid electrolytes is expected to fundamentally solve the above problems. All components of all-solid-state lithium batteries are composed of inorganic solid materials, which can perfectly solve the safety problems of liquid lithium batteries such as leakage, combustion and even explosion. In addition, all-solid-state ion batteries also have the potential advantages of high energy density and low self-discharge and are widely regarded as one of the next generation of new lithium-ion batteries. Solid electrolyte materials are an important component of all-solid-state batteries and play a decisive role in the performance of all-solid-state batteries.

[0003] There are many types of solid electrolytes, mainly oxides (LLZO, LAGP, LATP, etc.), sulfides (Li6PS5Cl, Li 10 GP2S 12 ), polymers (PEO, PVDF) and halides (Li3InCl6, Li3YCl6). Although oxide solid electrolytes have 10 -4 ~10 -3 S cm -1 The ionic conductivity, relatively stable air stability and theoretically relatively stable electrochemical performance of sulfide solid electrolytes are simple to prepare, with high ionic conductivity (maximum 10 mS cm -1 However, its commercialization is hampered by the fact that it produces highly toxic hydrogen sulfide gas when exposed to air, reacts more complexly with electrodes, and is easily flammable in air. Polymer solid electrolytes, however, are difficult to meet actual needs due to their very low ionic conductivity at room temperature.

[0004] Halide solid electrolyte materials have become a hot topic of research due to their wide electrochemical window, good compatibility with high-voltage cathodes, and good stability in dry air. x ScCl 3+x , Li3InCl6, Li2ZrCl6, etc. Among them, Li2ZrCl6 has good application prospects due to its low preparation cost, but the low ionic conductivity of Li2ZrCl6 limits its further development. 2+ x ZrCl 6-z C z (0<x≤1, 0<z≤1, C is O or S), it improves the ionic conductivity of Li2ZrCl6 by doping, but its physical phase is still mainly Li2ZrCl6. At the same time, although its lithium ion concentration has increased to a certain extent, it is still relatively low, and after doping, the electrochemical stability of the material is reduced.

[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a lithium-rich oxyhalide solid electrolyte material and its preparation method and application, and a lithium-ion secondary battery. By providing a new lithium-rich oxyhalide solid electrolyte material with stable electrochemical properties and high ionic conductivity, it aims to solve the problem of insufficient types of solid electrolyte materials with good compatibility, stability and high ionic conductivity.

[0007] The technical solution of the present invention is as follows:

[0008] A lithium-rich oxyhalide solid electrolyte material, wherein the general chemical formula of the lithium-rich oxyhalide solid electrolyte material is: Li 4+x A 1-x B x Cl 4-x O 2+0.5x ; Wherein, 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3+ , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

[0009] The lithium-rich oxyhalide solid electrolyte material, wherein the positions of the main characteristic peaks of the lithium-rich oxyhalide solid electrolyte material include at least three of 29-31.4°, 31.5-32.5°, 32.6-33.7° and 33.8-35°.

[0010] The lithium-rich oxyhalide solid electrolyte material is in any one of a crystalline, glassy, ​​or glass-ceramic phase.

[0011] The lithium-rich oxyhalide solid electrolyte material, wherein the ratio of the number of Li ions to the number of anions in the lithium-rich oxyhalide solid electrolyte material is greater than 0.75.

[0012] A method for preparing a lithium-rich oxyhalide solid electrolyte material as described above, wherein a lithium source, ACl4 and BCl3 are mixed and ground according to a stoichiometric ratio to obtain the lithium-rich oxyhalide solid electrolyte material;

[0013] or,

[0014] The lithium source, ACl4 and BCl3 are mixed evenly according to a stoichiometric ratio and then ground in an inert solvent. After the grinding, the inert solvent is removed in an oven to obtain the lithium-rich oxyhalide solid electrolyte material;

[0015] or,

[0016] The lithium source, ACl4 and BCl3 are mixed and ground according to a stoichiometric ratio, and then solid-phase sintered to obtain the lithium-rich oxyhalide solid electrolyte material;

[0017] or,

[0018] Mixing the raw materials lithium source, ACl4 and BCl3 according to the stoichiometric ratio and heating them to melt together to obtain the lithium-rich oxyhalide solid electrolyte material;

[0019] or,

[0020] After mixing the lithium source, ACl4 and BCl3 according to the stoichiometric ratio, a solvent co-dissolution recrystallization method is adopted to obtain the lithium-rich oxyhalide solid electrolyte material;

[0021] or,

[0022] The lithium source, ACl4 and BCl3 are mixed and ground according to a stoichiometric ratio, and then a solvent co-dissolution recrystallization method is used to obtain the lithium-rich oxygen halide solid electrolyte material.

[0023] A use of any of the above-mentioned lithium-rich oxygen halide solid electrolyte materials in the preparation of lithium-ion secondary batteries.

[0024] The application includes any one of the following: the application of lithium-rich oxyhalide solid electrolyte material as an electrolyte layer of a lithium-ion secondary battery, the application of lithium-rich oxyhalide solid electrolyte material as an electrode additive of a lithium-ion secondary battery, the application of lithium-rich oxyhalide solid electrolyte material as an interface buffer layer of a lithium-ion secondary battery, and the application of lithium-rich oxyhalide solid electrolyte material mixed with a liquid electrolyte or an ionic liquid as a semi-solid or quasi-solid electrolyte of a lithium-ion secondary battery.

[0025] A lithium-ion secondary battery, wherein at least one of the positive electrode layer, electrolyte layer, negative electrode layer and buffer layer of the lithium-ion secondary battery contains any of the above-mentioned lithium-rich oxygen halide solid electrolyte materials.

[0026] The lithium-ion secondary battery includes any one of a liquid lithium-ion secondary battery, a solid-liquid hybrid lithium-ion secondary battery, a semi-solid lithium-ion secondary battery, a quasi-solid lithium-ion secondary battery, and an all-solid lithium-ion secondary battery.

[0027] An application of the lithium-ion secondary battery as described above, wherein the lithium-ion secondary battery is applied to electronic products, electric bicycles, electric vehicles, robots, aerospace, solar power generation, wind power generation, smart grid peak regulation, distributed power stations, backup power supplies or energy storage devices for communication base stations.

[0028] Beneficial effects: The present invention provides a lithium-rich oxyhalide solid electrolyte material, a preparation method and application thereof, and a lithium-ion secondary battery. The lithium-rich oxyhalide solid electrolyte material provided by the present invention has the following advantages: 1) The preparation method is simple and convenient, and the raw material price is low, which is conducive to actual production; 2) The lithium-rich oxyhalide solid electrolyte material provided by the present invention has a wide electrochemical window, good compatibility with high-voltage positive electrodes, and good stability under dry air; 3) Sulfide solid electrolytes will react with oxygen when exposed to air to produce highly toxic H2S gas and are easily ignited. The lithium-rich oxyhalide solid electrolyte provided by the present invention has extremely high oxygen resistance, will not react with oxygen and will not burn, and has higher safety; 4) The ratio of the number of Li to anion atoms in the lithium-rich oxyhalide solid electrolyte provided by the present invention is greater than 0.75, and the room temperature ionic conductivity reaches 1×10 -4 S cm -1 The above, and the electrochemical performance of the obtained material is stable, and it can be applied to lithium-ion secondary batteries; 5) When the lithium-rich oxygen halide solid electrolyte material of the present invention is applied to the preparation of lithium secondary batteries, the obtained secondary battery has high first-cycle coulombic efficiency, good cycle stability and safety performance, and has extremely high application prospects in various energy storage devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is Li in Example 1 of the present invention 4.5 Sn 0.5 Fe 0.5 Cl 3.5 O 2.25 X-ray diffraction spectrum of lithium-rich oxygen halide solid electrolyte material.

[0030] Figure 2 is Li in Example 1 of the present invention 4.5 Sn 0.5 Fe 0.5 Cl 3.5 O 2.25 AC impedance spectrum of lithium-rich oxygen halide solid electrolyte material.

[0031] Figure 3 is Li in Example 2 of the present invention 4.5 Sn 0.5 Fe 0.5 Cl 3.5 O 2.25 X-ray diffraction spectrum of lithium-rich oxygen halide solid electrolyte material.

[0032] Figure 4 is Li in Example 2 of the present invention 4.5 Sn 0.5 Fe 0.5 Cl 3.5 O2.25 AC impedance spectrum of lithium-rich oxygen halide solid electrolyte material.

[0033] Figure 5 is Li in Example 3 of the present invention 4.3 Zr 0.7 Y 0.3 Cl 3.7 O 2.15 X-ray diffraction spectrum of lithium-rich oxygen halide solid electrolyte material.

[0034] Figure 6 is Li in Example 3 of the present invention 4.3 Zr 0.7 Y 0.3 Cl 3.7 O 2.15 AC impedance spectrum of lithium-rich oxygen halide solid electrolyte material.

[0035] Figure 7 is Li in Example 4 of the present invention 4.3 Zr 0.7 Y 0.3 Cl 3.7 O 2.15 X-ray diffraction spectrum of lithium-rich oxygen halide solid electrolyte material.

[0036] Figure 8 is Li in Example 4 of the present invention 4.3 Zr 0.7 Y 0.3 Cl 3.7 O 2.15 AC impedance spectrum of lithium-rich oxygen halide solid electrolyte material.

[0037] Fig. 9 This is a charge and discharge curve diagram of the first cycle of the lithium secondary battery in Test Example 3 of the present invention.

[0038] Fig.10 This is a long cycle performance diagram of the lithium secondary battery in Test Example 3 of the present invention. DETAILED DESCRIPTION

[0039] The present invention provides a lithium-rich oxygen halide solid electrolyte material and a preparation method and application thereof, and a lithium-ion secondary battery. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0040] The embodiment of the present invention provides a lithium-rich oxyhalide solid electrolyte material, the chemical formula of the lithium-rich oxyhalide solid electrolyte material is: Li 4+x A 1-x B x Cl4-x O 2+0.5x ; Wherein, 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3+ , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

[0041] In some specific embodiments, x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, but is not limited to the above values. As long as other unlisted values ​​are within this range, they are also applicable.

[0042] As a preferred embodiment, A is selected from Ti 4+ Sn 4+ 、Zr 4 、Si 4+ At least one of; B is selected from Fe 3+ , Y 3+ 、Al 3 + Sc 3+ , Yb 3+ At least one of .

[0043] The lithium-rich oxygen halide solid electrolyte material provided in the embodiment of the present invention has stable electrochemical properties and high ionic conductivity. Similar to the halide solid electrolyte material, the lithium-rich oxygen halide solid electrolyte material also has the characteristics of a wide electrochemical window, good compatibility with high-voltage positive electrodes, and good stability under dry air. The present invention provides a variety of solid electrolyte materials, which can promote the further rapid development of all-solid-state batteries. Not only that, sulfide solid electrolytes will react with oxygen when exposed to air to produce highly toxic H2S gas and are easily ignited, while the lithium-rich oxygen halide solid electrolyte provided by the present invention has extremely high oxygen resistance, will not react with oxygen and will not burn, and has higher safety.

[0044] In some embodiments, the positions of the main characteristic peaks of the lithium-rich oxyhalide solid electrolyte material are 29-31.4°, 31.5-32.5°, 32.6-33.7°, and 33.8-35°, respectively.

[0045] The present invention tests the physical phase of the lithium-rich oxyhalide solid electrolyte material obtained by X-ray diffraction (XRD), and finds that within the range of 25° to 60°, the positions (2θ) of its four main characteristic peaks are characteristic peak (1) 29° to 31.4°, characteristic peak (2) 31.5° to 32.5°, characteristic peak (3) 32.6° to 33.7°, and characteristic peak (4) 33.8° to 35°. Moreover, the peak intensities of the four main characteristic peaks of the lithium-rich oxyhalide solid electrolyte material are arranged from high to low as follows: characteristic peak (2)>characteristic peak (3)>characteristic peak (1)>characteristic peak (4).

[0046] In other embodiments, the positions of the main characteristic peaks of the lithium-rich oxygen halide solid electrolyte material include at least three of 29-31.4°, 31.5-32.5°, 32.6-33.7°, and 33.8-35°. Solid electrolyte materials having three or more of the above four main characteristic peaks at the same time are within the scope of protection of the present invention.

[0047] In some embodiments, the ratio of the number of Li ions to the number of anions in the lithium-rich oxyhalide solid electrolyte is greater than 0.75. The ratio of the number of Li ions to the number of anions in the lithium-rich oxyhalide solid electrolyte provided by the present invention is greater than 0.75, and the room temperature ionic conductivity reaches 1×10 -4 S cm -1 The electrochemical performance of the obtained material is stable and can be applied to lithium ion secondary batteries.

[0048] In some embodiments, the lithium-rich oxyhalide solid electrolyte material is in any one of a crystalline, glassy, ​​and glass-ceramic phase.

[0049] In some embodiments, the lithium-rich oxyhalide solid electrolyte material is spherical particles with a particle size of 50-5000 nm.

[0050] The embodiment of the present invention also provides a method for preparing a lithium-rich oxyhalide solid electrolyte material, the specific steps of which are: mixing a raw material lithium source, ACl4 and BCl3 in a stoichiometric ratio and then grinding to obtain the lithium-rich oxyhalide solid electrolyte material; wherein the chemical formula of the lithium-rich oxyhalide solid electrolyte material is: Li 4+x A 1-x B x Cl 4- x O 2+0.5x ; 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3+ , Y 3+ 、Co 3 + 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

[0051] Specifically, the grinding method includes any one of high-mix mixing, planetary ball milling, jar mill roller milling or sand milling.

[0052] More specifically, the ball milling method used for grinding has a ball-to-material ratio of (5-50):1, a ball milling time of 1-100 hours, and a ball milling speed of 100-1000 rpm.

[0053] More specifically, the ball milling method used in grinding is a ball milling jar made of zirconium oxide, polyurethane, nylon, etc.

[0054] In other embodiments, the preparation method of the lithium-rich oxyhalide solid electrolyte material comprises the following specific steps: mixing the raw materials lithium source, ACl4 and BCl3 in a stoichiometric ratio and grinding them in an inert solvent; after grinding, removing the inert solvent in an oven to obtain the lithium-rich oxyhalide solid electrolyte material; wherein the general chemical formula of the lithium-rich oxyhalide solid electrolyte material is: Li 4+x A 1-x B x Cl 4-x O 2+0.5x ; 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4 + 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3+ , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

[0055] Specifically, the inert solvent includes but is not limited to toluene (C7H8), xylene (C8H 10 ), acetonitrile (CH3CN), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), hexamethylphosphoric triamide (HMPA) or more.

[0056] Specifically, the grinding method includes any one of high-mix mixing, planetary ball milling, jar mill roller milling or sand milling.

[0057] More specifically, the ball milling method used for grinding has a ball-to-material ratio of (5-50):1, a ball milling time of 1-100 hours, and a ball milling speed of 100-1000 rpm.

[0058] More specifically, the ball milling method used in grinding is a ball milling jar made of zirconium oxide, polyurethane, nylon, etc.

[0059] In other embodiments, the preparation method of the lithium-rich oxyhalide solid electrolyte material comprises the following specific steps: mixing the raw materials lithium source, ACl4 and BCl3 in a stoichiometric ratio, grinding them, and then solid-phase sintering them to obtain the lithium-rich oxyhalide solid electrolyte material; wherein the chemical formula of the lithium-rich oxyhalide solid electrolyte material is: Li 4+ x A 1-x B x Cl 4-x O 2+0.5x ; 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3 + , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3 + 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

[0060] Specifically, the temperature of the solid phase sintering is 80° C.-600° C., and the time of the solid phase sintering is 0.01-100 hours.

[0061] Specifically, the grinding method includes any one of high-mix mixing, planetary ball milling, jar mill roller milling or sand milling.

[0062] More specifically, the ball milling method used for grinding has a ball-to-material ratio of (5-50):1, a ball milling time of 1-100 hours, and a ball milling speed of 100-1000 rpm.

[0063] More specifically, the ball milling method used in grinding is a ball milling jar made of zirconium oxide, polyurethane, nylon, etc.

[0064] In other embodiments, the preparation method of the lithium-rich oxyhalide solid electrolyte material comprises the following specific steps: mixing the raw materials lithium source, ACl4 and BCl3 uniformly according to the stoichiometric ratio and then heating them to melt together to obtain the lithium-rich oxyhalide solid electrolyte material; wherein the chemical formula of the lithium-rich oxyhalide solid electrolyte material is: Li 4+x A 1- x B x Cl 4-x O 2+0.5x ; 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3+ , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La3+ At least one of .

[0065] In other embodiments, the preparation method of the lithium-rich oxyhalide solid electrolyte material comprises the following specific steps: mixing the raw materials lithium source, ACl4 and BCl3 uniformly according to the stoichiometric ratio, and then adopting the solvent co-dissolution recrystallization method to obtain the lithium-rich oxyhalide solid electrolyte material; wherein the chemical formula of the lithium-rich oxyhalide solid electrolyte material is: Li 4+x A 1-x B x Cl 4-x O 2+0.5x ; 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3 + 、V 3+ , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3 + 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

[0066] In other embodiments, the preparation method of the lithium-rich oxyhalide solid electrolyte material comprises the following specific steps: mixing the raw materials lithium source, ACl4 and BCl3 in a stoichiometric ratio and then grinding them, and then using a solvent co-dissolution recrystallization method to obtain the lithium-rich oxyhalide solid electrolyte material; wherein the general chemical formula of the lithium-rich oxyhalide solid electrolyte material is:

[0067] Li 4+x A 1-xB x Cl 4-x O 2+0.5x ; 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3+ , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

[0068] Specifically, the solvent co-dissolution recrystallization method includes the following steps: putting the raw materials into a polar solvent (water or ethanol) containing a hydrolysis inhibitor (NH4X, X is a halogen), mixing them evenly and heating them to 120-600°C for recrystallization, and further dehydrating and drying the resulting product under a vacuum environment to obtain a lithium-rich oxygen halide solid electrolyte material.

[0069] Specifically, the grinding method includes any one of high-mix mixing, planetary ball milling, jar mill roller milling or sand milling.

[0070] More specifically, the ball milling method used for grinding has a ball-to-material ratio of (5-50):1, a ball milling time of 1-100 hours, and a ball milling speed of 100-1000 rpm.

[0071] More specifically, the ball milling method used in grinding is a ball milling jar made of zirconium oxide, polyurethane, nylon, etc.

[0072] The method for preparing the lithium-rich oxygen halide solid electrolyte material provided by the embodiment of the present invention is simple and convenient, has low raw material prices, is conducive to actual production, and has high application value.

[0073] The embodiment of the present invention also provides a use of the above-mentioned lithium-rich oxygen halide solid electrolyte material in the preparation of a lithium-ion secondary battery.

[0074] In some embodiments, the application includes any one of the application of lithium-rich oxygen halide solid electrolyte material as an electrolyte layer of a lithium-ion secondary battery, the application of lithium-rich oxygen halide solid electrolyte material as an electrode additive of a lithium-ion secondary battery, the application of lithium-rich oxygen halide solid electrolyte material as an interface buffer layer of a lithium-ion secondary battery, and the application of lithium-rich oxygen halide solid electrolyte material mixed with a liquid electrolyte or an ionic liquid as a semi-solid or quasi-solid electrolyte of a lithium-ion secondary battery.

[0075] Preferably, the application includes using the lithium-rich oxygen halide solid electrolyte material as an electrolyte layer of a lithium-ion secondary battery.

[0076] In a secondary battery prepared by using a lithium-rich oxygen halide solid electrolyte material as the electrolyte layer of a lithium-ion secondary battery, a lithium-ion layered positive electrode material is mixed with the lithium-rich oxygen halide solid electrolyte material and a conductive additive to form a composite positive electrode, and metal Li and graphite are used as the negative electrode. The assembled all-solid-state battery has a high first-cycle coulomb efficiency, stable cycle and good safety performance when cycled at room temperature.

[0077] An embodiment of the present invention further provides a lithium-ion secondary battery, wherein at least one of the positive electrode layer, the electrolyte layer, the negative electrode layer or the buffer layer of the lithium-ion secondary battery contains the above-mentioned lithium-rich oxygen halide solid electrolyte material.

[0078] In some embodiments, the lithium ion secondary battery includes any one of a liquid lithium ion secondary battery, a solid-liquid hybrid lithium ion secondary battery, a semi-solid lithium ion secondary battery, a quasi-solid lithium ion secondary battery, and an all-solid lithium ion secondary battery.

[0079] Preferably, the secondary battery is an all-solid-state lithium-ion secondary battery.

[0080] An embodiment of the present invention also provides an application of the above-mentioned lithium-ion secondary battery, wherein the lithium-ion secondary battery is applied to consumer electronic products, electric bicycles, electric vehicles, robots, aerospace, solar power generation, wind power generation, smart grid peak regulation, distributed power stations, backup power supplies or energy storage devices of communication base stations.

[0081] The following is a further explanation of a lithium-rich oxygen halide solid electrolyte material, a preparation method and application thereof, and a lithium-ion secondary battery of the present invention through specific embodiments:

[0082] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0083] Example 1

[0084] This embodiment provides a lithium-rich oxygen halide solid electrolyte material

[0085] Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Sn 4+ ,B=Fe 3+ , x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9); that is, the oxygen-halogen solid electrolyte materials of this embodiment are Li4SnCl4O2, Li 4.1 Sn 0.9 Fe 0.1 Cl 3.9 O 2.05 , Li 4.2 Sn 0.8 Fe 0.2 Cl 3.8 O 2.1 , Li 4.3 Sn 0.7 Fe 0.3 Cl 3.7 O 2.15 , Li 4.4 Sn 0.6 Fe 0.4 Cl 3.6 O 2.2 , Li 4.5 Sn 0.5 Fe 0.5 Cl 3.5 O 2.25 , Li 4.6 Sn 0.4 Fe 0.6 Cl 3.4 O 2.3 , Li 4.7 Sn 0.3 Fe 0.7 Cl 3.3 O 2.35 , Li 4.8 Sn 0.2 Fe 0.8 Cl 3.2 O 2.4, Li 4.9 Sn 0.1 Fe 0.9 Cl 3.1 O 2.45 .

[0086] The lithium-rich oxygen halide solid electrolyte material Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Sn 4+ ,B=Fe 3+ , x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9) are prepared as follows:

[0087] In the glove box, weigh the raw materials with different stoichiometric ratios:

[0088] Sample (1): Li2O:SnCl4=2:1; (x=0)

[0089] Sample (2): Li2O:SnCl4:FeCl3=41:18:2; (x=0.1)

[0090] Sample (3): Li2O:SnCl4:FeCl3=21:8:2; (x=0.2)

[0091] Sample (4): Li2O:SnCl4:FeCl3=43:14:6; (x=0.3)

[0092] Sample (5): Li2O:SnCl4:FeCl3=11:3:2; (x=0.4)

[0093] Sample (6): Li2O:SnCl4:FeCl3=9:2:2; (x=0.5)

[0094] Sample (7): Li2O:SnCl4:FeCl3=23:4:6; (x=0.6)

[0095] Sample (8): Li2O:SnCl4:FeCl3=47:6:14; (x=0.7)

[0096] Sample (9): Li2O:SnCl4:FeCl3=12:1:4; (x=0.8)

[0097] Sample (10): Li2O:SnCl4:FeCl3=49:2:18; (x=0.9)

[0098] The raw materials of various proportions were poured into a zirconia ball mill, with a ball diameter of 3 mm and a ball-to-material ratio of 10:1. A planetary ball mill was used with a ball milling speed of 200 rpm for 30 h. After the ball milling was completed, the ball mill was returned to the glove box, and the powder obtained by ball milling was taken out to obtain a lithium-rich oxygen halide solid electrolyte Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Sn 4+ ,B=Fe 3+ ,x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9).

[0099] Example 2

[0100] The difference between this embodiment and embodiment 1 is that after the ball milling is completed, the ball mill is returned to the glove box, the powder obtained by ball milling is pressed into a tablet, and the tablet is sintered at 200° C. for 0.5 h in an argon atmosphere, and then naturally cooled to room temperature. The sintered product is taken out and manually ground to powder to obtain a lithium-rich oxyhalide solid electrolyte Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Sn 4+ ,B=Fe 3+ ,x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9).

[0101] Example 3

[0102] This embodiment provides a lithium-rich oxygen halide solid electrolyte material

[0103] Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Zr 4+ ,B=Y 3+ , x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9); that is, the oxygen-halogen solid electrolyte materials of this embodiment are Li4ZrCl4O2, Li 4.1 Zr 0.9 Y 0.1 Cl 3.9 O 2.05 , Li 4.2 Zr 0.8 Y 0.2 Cl 3.8 O 2.1 , Li4.3 Zr 0.7 Y 0.3 Cl 3.7 O 2.15 , Li 4.4 Zr 0.6 Y 0.4 Cl 3.6 O 2.2 , Li 4.5 Zr 0.5 Y 0.5 Cl 3.5 O 2.25 , Li 4.6 Zr 0.4 Y 0.6 Cl 3.4 O 2.3 , Li 4.7 Zr 0.3 Y 0.7 Cl 3.3 O 2.35 , Li 4.8 Zr 0.2 Y 0.8 Cl 3.2 O 2.4 , Li 4.9 Zr 0.1 Y 0.9 Cl 3.1 O 2.45 .

[0104] The lithium-rich oxygen halide solid electrolyte material Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Zr 4+ ,B=Y 3+ , x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9) are prepared as follows:

[0105] In the glove box, weigh the raw materials with different stoichiometric ratios:

[0106] Sample (1): Li2O:ZrCl4=2:1; (x=0)

[0107] Sample (2): Li2O:ZrCl4:YCl3=41:18:2; (x=0.1)

[0108] Sample (3): Li2O:ZrCl4:YCl3=21:8:2; (x=0.2)

[0109] Sample (4): Li2O:ZrCl4:YCl3=43:14:6; (x=0.3)

[0110] Sample (5): Li2O:ZrCl4:YCl3=11:3:2; (x=0.4)

[0111] Sample (6): Li2O:ZrCl4:YCl3=9:2:2; (x=0.5)

[0112] Sample (7): Li2O:ZrCl4:YCl3=23:4:6; (x=0.6)

[0113] Sample (8): Li2O:ZrCl4:YCl3=47:6:14; (x=0.7)

[0114] Sample (9): Li2O:ZrCl4:YCl3=12:1:4; (x=0.8)

[0115] Sample (10): Li2O:ZrCl4:YCl3=49:2:18; (x=0.9)

[0116] The raw materials of various proportions were poured into a zirconia ball mill, with a diameter of 5 mm for the middle ball mill and a ball-to-material ratio of 15:1. A planetary ball mill was used with a ball milling speed of 300 rpm for 40 h. After the ball milling was completed, the ball mill was returned to the glove box, and the powder obtained by ball milling was taken out to obtain a lithium-rich oxygen halide solid electrolyte Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Zr 4+ ,B=Y 3+ ,x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9).

[0117] Example 4

[0118] The difference between this embodiment and embodiment 3 is that after the ball milling is completed, the ball mill is returned to the glove box, the powder obtained by ball milling is pressed into a tablet, and the tablet is sintered at 160° C. for 0.2 h in an argon atmosphere, and then naturally cooled to room temperature. The sintered product is taken out and manually ground to powder to obtain a lithium-rich oxyhalide solid electrolyte Li 4+x A 1-x B x Cl 4-x O 2+0.5x (A=Zr 4+ ,B=Y 3+ ,x=0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9).

[0119] Test Example 1

[0120] In this test example, the sample (5) provided in the above-mentioned embodiment 1, the sintered sample (5) provided in the embodiment 2, the sample (13) provided in the embodiment 3, and the sintered sample (13) provided in the embodiment 4 were subjected to X-ray diffraction at a diffraction angle of 25-60°. The results are as follows: Figure 1 , 3 , 5, and 7 as shown.

[0121] Test Example 2

[0122] In this test example, the sample (5) provided in the above-mentioned embodiment 1, the sintered sample (5) provided in the embodiment 2, the sample (13) provided in the embodiment 3, and the sintered sample (13) provided in the embodiment 4 were subjected to AC impedance test. The results are as follows: Figure 2 , 4 , 6, and 8.

[0123] Test Example 3

[0124] This test example provides an all-solid-state lithium secondary battery comprising the lithium-rich oxyhalide solid electrolyte material;

[0125] The preparation method of the lithium secondary battery is as follows:

[0126] The specific steps include:

[0127] 1) Take a certain amount of Li provided in Example 1 4.5 Sn 0.5 Fe 0.5 Cl 3.5 O 2.25 The lithium-rich oxyhalide solid electrolyte material is pressed into tablets at a pressure of 220 MPa to obtain a lithium-rich oxyhalide solid electrolyte material solid electrolyte sheet.

[0128] 2) Add a certain mass of lithium cobalt oxide positive electrode material to one side of the solid electrolyte sheet of the lithium-rich oxyhalide solid electrolyte material prepared in step 1); add a certain amount of Li6PS5Cl sulfide solid electrolyte, lithium indium alloy and steel sheet in sequence to the other side of the lithium-rich oxyhalide solid electrolyte material, and press at 60 MPa to obtain an all-solid-state lithium secondary battery.

[0129] 3) The all-solid-state lithium secondary battery obtained in step 2) was subjected to a charge and discharge test at a rate of 0.1C, with a voltage range of 3-4.3V vs. Li / Li + .

[0130] The all-solid-state lithium secondary battery using the sample (5) provided in Example 1 as the solid electrolyte was subjected to charge and discharge tests. The first cycle coulombic efficiency was as follows: Fig. 9As shown in the figure, it can be seen that the all-solid-state battery composed of the lithium-rich oxygen halide solid electrolyte material prepared by the present invention has a first-cycle coulomb efficiency of more than 96.7%, showing a very high reversible capacity; at the same time, the discharge capacity of the battery composed of the lithium-rich oxygen halide solid electrolyte material prepared by the present invention is 138 mAh g -1 (like Fig.10 shown).

[0131] In summary, the present invention provides a lithium-rich oxyhalide solid electrolyte material, a preparation method and application thereof, and a lithium-ion secondary battery. The preparation method of the lithium-rich oxyhalide solid electrolyte material provided by the present invention is simple and convenient, the raw materials are inexpensive, and it is conducive to actual production. The lithium-rich oxyhalide solid electrolyte material provided by the present invention has a broad electrochemical window, good compatibility with high-voltage positive electrodes, and good stability under dry air. The lithium-rich oxyhalide solid electrolyte provided by the present invention has extremely high oxygen resistance, will not react with oxygen and will not burn, and has higher safety. The lithium-rich oxyhalide solid electrolyte provided by the present invention has a ratio of Li to anion atoms greater than 0.75, and the room temperature ionic conductivity reaches 1×10 -4 S cm -1 When the lithium-rich oxygen halide solid electrolyte material of the present invention is used in the preparation of lithium secondary batteries, the obtained secondary batteries have high first-cycle coulombic efficiency, good cycle stability and safety performance, and have extremely high application prospects in various energy storage devices.

[0132] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A lithium-rich oxygen halide solid electrolyte material, It is characterized in that The general chemical formula of the lithium-rich oxygen halide solid electrolyte material is: Li 4+x A 1-x B x Cl 4-x O 2+0.5x ; Wherein, 0≤x<1; A is selected from Ti 4+ Sn 4+ 、Zr 4+ , Hf 4+ 、Si 4+ ,Ge 4+ At least one of; B is selected from Cr 3+ 、V 3+ , Y 3+ 、Co 3+ 、Ni 3+ 、Ti 3+ Sc 3+ 、Lu 3+ , Fe 3+ 、Al 3+ , Ga 3+ 、In 3+ , Yb 3+ 、Tm 3+ , Er 3+ 、Ho 3+ 、Dy 3+ , Tb 3+ , Gd 3+ 、Eu 3+ 、Sm 3+ 、Pm 3+ 、Nd 3+ , Pr 3+ 、Ce 3+ ,La 3+ At least one of .

2. The lithium-rich oxyhalide solid electrolyte material according to claim 1, It is characterized in that The positions of the main characteristic peaks of the lithium-rich oxyhalide solid electrolyte material include at least three of 29-31.4°, 31.5-32.5°, 32.6-33.7° and 33.8-35°.

3. The lithium-rich oxyhalide solid electrolyte material according to claim 1, It is characterized in that The lithium-rich oxyhalide solid electrolyte material is in any one of a crystalline, glassy, ​​and glass-ceramic phase.

4. The lithium-rich oxyhalide solid electrolyte material according to claim 1, It is characterized in that The ratio of the number of Li ions to the number of anions in the lithium-rich oxyhalide solid electrolyte material is greater than or equal to 0.

75.

5. A method for preparing the lithium-rich oxyhalide solid electrolyte material according to any one of claims 1 to 4, It is characterized in that According to the stoichiometric ratio, lithium source, ACl 4 and BCl 3 Grinding after mixing to obtain the lithium-rich oxygen halide solid electrolyte material; or, According to the stoichiometric ratio, lithium source, ACl 4 and BCl 3 After being uniformly mixed, the mixture is ground in an inert solvent, and after the grinding is completed, the inert solvent is removed in an oven to obtain the lithium-rich oxygen halide solid electrolyte material; or, According to the stoichiometric ratio, lithium source, ACl 4 and BCl 3 Grinding after mixing, and then solid phase sintering to obtain the lithium-rich oxygen halide solid electrolyte material; or, The raw materials lithium source, ACl 4 and BCl 3 After mixing, heating and eutectic melting are performed to obtain the lithium-rich oxygen halide solid electrolyte material; or, According to the stoichiometric ratio, lithium source, ACl 4 and BCl 3 After mixing, a solvent co-dissolution recrystallization method is used to obtain the lithium-rich oxygen halide solid electrolyte material; or, According to the stoichiometric ratio, lithium source, ACl 4 and BCl 3 The mixture is mixed and ground, and then a solvent co-dissolution recrystallization method is used to obtain the lithium-rich oxygen halide solid electrolyte material.

6. Use of the lithium-rich oxygen halide solid electrolyte material as claimed in any one of claims 1 to 4 in the preparation of a lithium-ion secondary battery.

7. The use according to claim 6, It is characterized in that The applications include any one of the following: the application of lithium-rich oxyhalide solid electrolyte materials as electrolyte layers of lithium-ion secondary batteries, the application of lithium-rich oxyhalide solid electrolyte materials as electrode additives of lithium-ion secondary batteries, the application of lithium-rich oxyhalide solid electrolyte materials as interface buffer layers of lithium-ion secondary batteries, and the application of lithium-rich oxyhalide solid electrolyte materials mixed with liquid electrolytes or ionic liquids as semi-solid or quasi-solid electrolytes of lithium-ion secondary batteries.

8. A lithium ion secondary battery, It is characterized in that At least one of the positive electrode layer, electrolyte layer, negative electrode layer and buffer layer of the lithium-ion secondary battery contains the lithium-rich oxyhalide solid electrolyte material according to any one of claims 1 to 4.

9. The lithium ion secondary battery according to claim 8, It is characterized in that The lithium ion secondary battery includes any one of a liquid lithium ion secondary battery, a solid-liquid hybrid lithium ion secondary battery, a semi-solid lithium ion secondary battery, a quasi-solid lithium ion secondary battery, and an all-solid lithium ion secondary battery.

10. Use of the lithium ion secondary battery as claimed in claim 8, It is characterized in that The lithium-ion secondary battery is applied to electronic products, electric bicycles, electric vehicles, robots, aerospace, solar power generation, wind power generation, smart grid peak regulation, distributed power stations, backup power supplies or energy storage devices for communication base stations.

Citation Information

Cited By

  • Oxygen chloride solid electrolyte as well as preparation method and application thereof

    CN119542517A

  • A kind of oxychloride solid electrolyte and its preparation method and application

    CN119542517B

  • Battery cell and preparation method therefor, battery and application thereof, and solid electrolyte powder and preparation method therefor

    WO2026129538A1

  • Solid-state electrolyte, and preparation method therefor and use thereof

    WO2026179141A1