High-voltage electrolyte containing silicon-based additive and preparation method of high-voltage electrolyte
By using high-voltage electrolyte containing silicon-based additives in lithium-ion batteries, a thin protective layer is formed on the surface of the positive electrode, which solves the problem of the electrolyte being easily oxidized and decomposed under high pressure, improves the cycle stability and safety of the battery, and achieves for higher battery performance and service life.
Patent Information
- Application Number
- CN202310796236.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-02
- Publication Date
- 2024-10-01
AI Technical Summary
The existing high-voltage lithium-ion battery electrolyte is easily oxidized and decomposed under high pressure, resulting in an unstable electrode/electrolyte interface. The side reaction products lose electrolyte components, reducing the Coulombic efficiency and safety of the battery. In addition, the inorganic high-voltage electrolyte additives have a relatively single function. Limits large-scale application.
Using a high-voltage electrolyte containing silicon-based additives, through a specific ratio of solvent and lithium salt combination, silicon-based additives such as silicon dioxide, silicon monoxide and silicon carbide are added to form a thin protective layer on the surface of the positive active material. Reduce interface reaction and inhibit battery impedance growth.
It achieves a wide electrochemical window, oxidation resistance, and high-voltage characteristics, improves the cycle stability and safety performance of the battery, and enhances the service life and safety of the battery.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a high-voltage electrolyte containing a silicon-based additive and a preparation method thereof. Background Art
[0002] The 30 years of development of lithium-ion secondary batteries have changed all aspects of human life. From the initial application in portable electronic devices such as mobile phones and computers, it is currently developing towards emerging applications such as electric vehicles and grid energy storage. However, lithium-ion batteries are rapidly approaching the limit of their actual energy density. In order to continue the advantages of lithium-ion batteries, the application of new materials and the full utilization of the capacity of materials are crucial. High-nickel layered oxide cathode materials have occupied a place in the commercial cathode materials of lithium-ion batteries due to their high specific capacity, high tap density, high lithium insertion potential and environmental friendliness, and are considered to be the most promising cathode materials at present. To obtain higher capacity, it can be achieved by increasing the operating voltage. However, high voltage (≥4.5V) not only makes the stability of the active material worse, but also causes oxidative decomposition of the electrolyte, making the electrode / electrolyte interface unstable. Usually, the electrolyte solvent will decompose severely or even produce gas under high voltage, and the solute LiPF6 will react with trace water to generate corrosive Lewis acids such as HF, resulting in the loss of active components of the electrolyte. In addition, these side reaction products will lead to structural instability of the cathode material and reconstruction of the cathode electrolyte interface (CEI). As a result, the coulombic efficiency of the battery is reduced, the capacity decays rapidly, and even safety problems occur. In order to improve the stability of the electrolyte under high pressure and the cycle stability of high-nickel layered oxide positive electrode materials, single crystal structure design, surface coating of active materials, and addition of electrolyte additives can be used to achieve this. Electrolyte additives have been proven to be an effective way to improve the electrochemical properties of electrode materials. The organic high-voltage electrolyte additives currently used generally oxidize preferentially over solvent molecules during the cycle process. They reduce interfacial side reactions by decomposing and forming an interfacial film on the surface of the positive electrode, stabilize the electrode / electrolyte interface, and ultimately achieve stable existence of the electrolyte under high pressure. However, problems such as difficulty in forming a stable surface film, high viscosity, and high cost limit the large-scale application of organic high-voltage electrolyte additives. In comparison, the use of inorganic high-voltage electrolyte additives is not only cost-effective, but can also be easily used on a large scale in industry. However, the existing inorganic electrolyte additives have a relatively single function, mainly by attaching to the surface of the material to play a protective role similar to coating. The 30 years of development of lithium-ion secondary batteries have changed all aspects of human life. From its initial application in portable electronic devices such as mobile phones and computers, it is now developing towards emerging applications such as electric vehicles and grid energy storage. However, lithium-ion batteries are rapidly approaching the limit of their practical energy density. In order for the advantages of lithium-ion batteries to continue, the application of new materials and the full utilization of the material capacity are crucial.
[0003] High nickel layered oxide cathode materials have occupied a place in the commercial cathode materials of lithium-ion batteries due to their high specific capacity, high tap density, high lithium insertion potential and environmental friendliness, and are considered to be the most promising cathode materials at present. To obtain higher capacity, it can be achieved by increasing the operating voltage. However, high voltage (≥4.5V) not only deteriorates the stability of the active material, but also causes oxidative decomposition of the electrolyte, making the electrode / electrolyte interface unstable. Usually, the electrolyte solvent will seriously decompose or even produce gas under high voltage, and the solute LiPF6 and trace water will react to generate corrosive Lewis acids such as HF, resulting in the loss of effective components of the electrolyte. In addition, these side reaction products will lead to the instability of the cathode material structure and the reconstruction of the cathode electrolyte interface (CEI). The result is a decrease in the coulombic efficiency of the battery, rapid capacity decay and even safety issues.
[0004] In order to improve the stability of the electrolyte under high pressure and the cycle stability of high-nickel layered oxide positive electrode materials, this can be achieved through single crystal structure design, surface coating of active materials, and addition of electrolyte additives. Electrolyte additives have been proven to be an effective way to improve the electrochemical properties of electrode materials. The organic high-voltage electrolyte additives currently used generally oxidize preferentially over solvent molecules during the cycle process. They reduce interfacial side reactions by decomposing and forming an interfacial film on the surface of the positive electrode, stabilize the electrode / electrolyte interface, and ultimately achieve stable existence of the electrolyte under high pressure. However, problems such as difficulty in forming a stable surface film, high viscosity, and high cost limit the large-scale application of organic high-voltage electrolyte additives. In comparison, the use of inorganic high-voltage electrolyte additives is not only cost-effective, but can also be easily used on a large scale in industry. However, the existing inorganic electrolyte additives have a relatively single function, mainly by attaching to the surface of the material to play a protective role similar to coating. Summary of the invention
[0005] The object of the present invention is to provide a high-voltage electrolyte containing a silicon-based additive and a preparation method thereof, aiming to solve the problems existing in the above-mentioned background technology.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a high-voltage electrolyte containing a silicon-based additive, the high-voltage electrolyte comprising a solvent, a lithium salt and a silicon-based additive; the solvent comprises the following components in parts by weight: 20-30 parts of ethylene glycol, 5-10 parts of fluoroethylene carbonate, 5-10 parts of ammonium pentaborate, 5-10 parts of trifluoropropylene carbonate, 5-10 parts of polyvinyl alcohol, 5-10 parts of diethylene glycol, 5-10 parts of dodecanedionate ammonium, 5-10 parts of ammonium hypophosphite, 2-5 parts of o-nitroanisole, 2-5 parts of mercaptobenzothiazole, 20-30 parts of citric acid, 5-10 parts of diammonium phosphate, and 30-40 parts of deionized water; 20-30 parts of a silicon-based additive and 10-20 parts of a lithium salt; the silicon-based additive is one or more of silicon dioxide, silicon monoxide, silicon carbide and silicon element, and the addition amount of the silicon-based additive is 5-10 mg / mL.
[0007] Furthermore, the lithium salt is one or a combination of two or more of lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium difluorophosphate, and lithium trifluoromethanesulfonate.
[0008] Furthermore, the concentration of the lithium salt is 0.8 mol / L-1.5 mol / L.
[0009] Furthermore, a method for preparing a high-voltage electrolyte containing a silicon-based additive comprises the following steps:
[0010] (1) ethylene glycol, fluoroethylene carbonate, trifluoropropylene carbonate, ammonium pentaborate, polyvinyl alcohol, diethylene glycol, dodecanedioic acid, ammonium hypophosphite, citric acid, o-nitroanisole, mercaptobenzothiazole, diammonium phosphate and deionized water are weighed according to the above ratio and set aside;
[0011] (2) heating ethylene glycol to 80-90°C, then adding citric acid and trifluoropropylene carbonate, continuing to heat to 90-95°C, stirring until completely dissolved, at a stirring speed of 100-200 r / min;
[0012] (3) Heat deionized water to 90-100° C., then add mannitol and ammonium hypophosphite, continue heating to 100-120° C., and stir until completely dissolved at a stirring speed of 200-400 r / min;
[0013] (4) mixing the product obtained in step (2) with the product obtained in step (3), stirring and reacting at 85-100° C. for 2-4 h at a stirring speed of 150-200 r / min;
[0014] (5) mixing the product obtained in step (4) with fluoroethylene carbonate, ammonium dodecanedioate, lithium salt and diammonium phosphate, stirring and reacting at 85-95° C. for 0.3-0.5 h at a stirring speed of 600-800 r / min;
[0015] (6) Cooling the product obtained in step (5) to 50-60° C., adding o-nitroanisole, silicon-based additives, and mercaptobenzothiazole, stirring continuously until completely clarified, the stirring speed being 800-1000 r / min; cooling naturally to obtain a high-voltage electrolyte containing silicon-based additives.
[0016] Further, in step (3), deionized water is heated to 88° C., and then mannitol, silicon-based additives, sodium borate and citric acid are added, and the mixture is heated to 97° C. and stirred until completely dissolved at a stirring speed of 300 r / min.
[0017] Furthermore, in step (4), the product obtained in step (2) is mixed with the product obtained in step (3), and the mixture is stirred at 90° C. for 5 h at a stirring speed of 200 r / min.
[0018] Furthermore, in step (5), the product obtained in step (4) is mixed with fluoroethylene carbonate, ammonium dodecanedioate, lithium salt and ammonium dihydrogen phosphate, and the mixture is stirred at 90° C. for 0.5 h at a stirring speed of 800 r / min.
[0019] Further, in step (6), the product obtained in step (5) is cooled to 55° C., o-nitroanisole, a silicon-based additive, and mercaptobenzothiazole are added, and the mixture is stirred continuously until it is completely clarified at a stirring speed of 800 r / min; the mixture is cooled naturally to obtain a high-voltage electrolyte containing a silicon-based additive.
[0020] Beneficial effects of the present invention: By adopting the above technical scheme, a high-voltage electrolyte containing a silicon-based additive and a preparation method thereof of the present invention have a wider electrochemical window and better oxidation resistance and high-voltage resistance, and at the same time have higher electrical conductivity, which can ensure the high rate and power characteristics of the power battery, and also have higher safety, which can greatly improve the safety performance of the power battery. The silicon-based additive has good dispersibility in the electrolyte and can be deposited on the surface of the positive electrode active material to form a thin protective layer with good mechanical strength. Compared with the coating method, the surface layer is more uniform and dense due to the electrochemical action, which can effectively reduce the contact between the electrolyte and the active material and reduce the interfacial reaction activity; in addition, the silicon-based additive can spontaneously react with LiPF6 in the electrolyte to generate lithium difluorophosphate (LiPO2F2), which helps to inhibit the growth of battery impedance and effectively improve the cycle stability and service life of the battery. DETAILED DESCRIPTION
[0021] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0022] Embodiment 1: A high-voltage electrolyte containing a silicon-based additive, the high-voltage electrolyte comprising a solvent, a lithium salt and a silicon-based additive; the solvent comprises the following components in parts by weight: 20 parts of ethylene glycol, 5 parts of fluoroethylene carbonate, 5 parts of ammonium pentaborate, 5 parts of trifluoropropylene carbonate, 5 parts of polyvinyl alcohol, 5 parts of diethylene glycol, 5 parts of dodecanedionate ammonium, 5 parts of ammonium hypophosphite, 2 parts of o-nitroanisole, 2 parts of mercaptobenzothiazole, 20 parts of citric acid, 5 parts of diammonium phosphate, and 30 parts of deionized water; 20 parts of a silicon-based additive and 10 parts of a lithium salt; the silicon-based additive is one or more of silicon dioxide, silicon monoxide, silicon carbide and silicon element, and the amount of the silicon-based additive added is 5-10 mg / mL.
[0023] In this embodiment, a method for preparing a high-voltage electrolyte containing a silicon-based additive comprises the following steps:
[0024] (1) ethylene glycol, fluoroethylene carbonate, trifluoropropylene carbonate, ammonium pentaborate, polyvinyl alcohol, diethylene glycol, dodecanedioic acid, ammonium hypophosphite, citric acid, o-nitroanisole, mercaptobenzothiazole, diammonium phosphate and deionized water are weighed according to the above ratio and set aside;
[0025] (2) Heat ethylene glycol to 80°C, then add citric acid and trifluoropropylene carbonate, continue heating to 90°C, and stir until completely dissolved at a stirring speed of 100 r / min;
[0026] (3) Heat deionized water to 90°C, then add mannitol and ammonium hypophosphite, continue heating to 100°C, and stir until completely dissolved at a stirring speed of 200 r / min;
[0027] (4) mixing the product obtained in step (2) with the product obtained in step (3), stirring the mixture at 85° C. for 2-4 hours at a stirring speed of 150 r / min;
[0028] (5) mixing the product obtained in step (4) with fluoroethylene carbonate, ammonium dodecanedioate, lithium salt and diammonium phosphate, and stirring the mixture at 85° C. for 0.3 h at a stirring speed of 600 r / min;
[0029] (6) Cool the product obtained in step (5) to 50° C., add o-nitroanisole, silicon-based additives, and mercaptobenzothiazole, and stir continuously until the product is completely clarified at a stirring speed of 800 r / min; cool naturally to obtain a high-voltage electrolyte containing silicon-based additives.
[0030] Embodiment 2: A high-voltage electrolyte containing a silicon-based additive, the high-voltage electrolyte comprising a solvent, a lithium salt and a silicon-based additive; the solvent comprises the following components in parts by weight: 25 parts of ethylene glycol, 8 parts of fluoroethylene carbonate, 8 parts of ammonium pentaborate, 8 parts of trifluoropropylene carbonate, 8 parts of polyvinyl alcohol, 8 parts of diethylene glycol, 8 parts of ammonium dodecanedioate, 8 parts of ammonium hypophosphite, 3 parts of o-nitroanisole, 3 parts of mercaptobenzothiazole, 25 parts of citric acid, 8 parts of diammonium phosphate, and 35 parts of deionized water; 25 parts of a silicon-based additive and 15 parts of a lithium salt; the silicon-based additive is one or more of silicon dioxide, silicon monoxide, silicon carbide and silicon element, and the amount of the silicon-based additive added is 8 mg / mL.
[0031] In this embodiment, a method for preparing a high-voltage electrolyte containing a silicon-based additive comprises the following steps:
[0032] (1) ethylene glycol, fluoroethylene carbonate, trifluoropropylene carbonate, ammonium pentaborate, polyvinyl alcohol, diethylene glycol, dodecanedioic acid, ammonium hypophosphite, citric acid, o-nitroanisole, mercaptobenzothiazole, diammonium phosphate and deionized water are weighed according to the above ratio and set aside;
[0033] (2) Heat ethylene glycol to 85°C, then add citric acid and trifluoropropylene carbonate, continue heating to 92°C, and stir until completely dissolved at a stirring speed of 150 r / min;
[0034] (3) Heat deionized water to 95°C, then add mannitol and ammonium hypophosphite, continue heating to 110°C, and stir until completely dissolved at a stirring speed of 300 r / min;
[0035] (4) mixing the product obtained in step (2) with the product obtained in step (3), stirring the mixture at 90° C. for 3 h at a stirring speed of 180 r / min;
[0036] (5) mixing the product obtained in step (4) with fluoroethylene carbonate, ammonium dodecanedioate, lithium salt and diammonium phosphate, stirring and reacting at 90° C. for 0.4 h at a stirring speed of 700 r / min;
[0037] (6) Cool the product obtained in step (5) to 55° C., add o-nitroanisole, silicon-based additives, and mercaptobenzothiazole, and stir continuously until the product is completely clarified at a stirring speed of 900 r / min; cool naturally to obtain a high-voltage electrolyte containing silicon-based additives.
[0038] Embodiment 3: A high-voltage electrolyte containing a silicon-based additive, the high-voltage electrolyte comprising a solvent, a lithium salt and a silicon-based additive; the solvent comprises the following components in parts by weight: 30 parts of ethylene glycol, 10 parts of fluoroethylene carbonate, 10 parts of ammonium pentaborate, 10 parts of trifluoropropylene carbonate, 10 parts of polyvinyl alcohol, 10 parts of diethylene glycol, 10 parts of dodecanedionate ammonium, 10 parts of ammonium hypophosphite, 5 parts of o-nitroanisole, 5 parts of mercaptobenzothiazole, 30 parts of citric acid, 10 parts of diammonium phosphate, and 40 parts of deionized water; 30 parts of a silicon-based additive and 20 parts of a lithium salt; the silicon-based additive is one or more of silicon dioxide, silicon monoxide, silicon carbide and silicon element, and the amount of the silicon-based additive added is 10 mg / mL.
[0039] In this embodiment, a method for preparing a high-voltage electrolyte containing a silicon-based additive comprises the following steps:
[0040] (1) ethylene glycol, fluoroethylene carbonate, trifluoropropylene carbonate, ammonium pentaborate, polyvinyl alcohol, diethylene glycol, dodecanedioic acid, ammonium hypophosphite, citric acid, o-nitroanisole, mercaptobenzothiazole, diammonium phosphate and deionized water are weighed according to the above ratio and set aside;
[0041] (2) Heat ethylene glycol to 90°C, then add citric acid and trifluoropropylene carbonate, continue heating to 95°C, and stir until completely dissolved at a stirring speed of 200 r / min;
[0042] (3) Heat deionized water to 100°C, then add mannitol and ammonium hypophosphite, continue heating to 100-120°C, and stir until completely dissolved at a stirring speed of 400 r / min;
[0043] (4) mixing the product obtained in step (2) with the product obtained in step (3), stirring the mixture at 100° C. for 4 h at a stirring speed of 200 r / min;
[0044] (5) mixing the product obtained in step (4) with fluoroethylene carbonate, ammonium dodecanedioate, lithium salt and diammonium phosphate, stirring the mixture at 95° C. for 0.5 h at a stirring speed of 600-800 r / min;
[0045] (6) Cool the product obtained in step (5) to 60° C., add o-nitroanisole, silicon-based additives, and mercaptobenzothiazole, and stir continuously until the product is completely clarified at a stirring speed of 1000 r / min; cool naturally to obtain a high-voltage electrolyte containing silicon-based additives.
[0046] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0047] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A high-voltage electrolyte containing a silicon-based additive, characterized in that: The high-voltage electrolyte comprises a solvent, a lithium salt and a silicon-based additive; the solvent comprises the following components in parts by weight: 20-30 parts of ethylene glycol, 5-10 parts of fluoroethylene carbonate, 5-10 parts of ammonium pentaborate, 5-10 parts of trifluoropropylene carbonate, 5-10 parts of polyvinyl alcohol, 5-10 parts of diethylene glycol, 5-10 parts of dodecanedionate ammonium, 5-10 parts of ammonium hypophosphite, 2-5 parts of o-nitroanisole, 2-5 parts of mercaptobenzothiazole, 20-30 parts of citric acid, 5-10 parts of diammonium phosphate, and 30-40 parts of deionized water; 20-30 parts of silicon-based additives, 10-20 parts of lithium salt; The silicon-based additive is one or more of silicon dioxide, silicon monoxide, silicon carbide and silicon alone, and the added amount of the silicon-based additive is 5-10 mg / mL.
2. The high-voltage electrolyte containing a silicon-based additive according to claim 1, characterized in that: The lithium salt is one or a combination of two or more of lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium difluorophosphate, and lithium trifluoromethanesulfonate.
3. The high-voltage electrolyte containing a silicon-based additive according to claim 1, characterized in that: The concentration of the lithium salt is 0.8 mol / L-1.5 mol / L.
4. A method for preparing a high-voltage electrolyte containing a silicon-based additive, characterized in that: The following steps are involved: (1) ethylene glycol, fluoroethylene carbonate, trifluoropropylene carbonate, ammonium pentaborate, polyvinyl alcohol, diethylene glycol, dodecanedioic acid, ammonium hypophosphite, citric acid, o-nitroanisole, mercaptobenzothiazole, diammonium phosphate and deionized water are weighed according to the above ratio and set aside; (2) heating ethylene glycol to 80-90°C, then adding citric acid and trifluoropropylene carbonate, continuing to heat to 90-95°C, stirring until completely dissolved, at a stirring speed of 100-200 r / min; (3) Heat deionized water to 90-100° C., then add mannitol and ammonium hypophosphite, continue heating to 100-120° C., and stir until completely dissolved at a stirring speed of 200-400 r / min; (4) mixing the product obtained in step (2) with the product obtained in step (3), stirring and reacting at 85-100° C. for 2-4 h at a stirring speed of 150-200 r / min; (5) mixing the product obtained in step (4) with fluoroethylene carbonate, ammonium dodecanedioate, lithium salt and diammonium phosphate, stirring and reacting at 85-95° C. for 0.3-0.5 h at a stirring speed of 600-800 r / min; (6) Cooling the product obtained in step (5) to 50-60° C., adding o-nitroanisole, silicon-based additives, and mercaptobenzothiazole, stirring continuously until completely clarified, the stirring speed being 800-1000 r / min; cooling naturally to obtain a high-voltage electrolyte containing silicon-based additives.
5. The method for preparing a high-voltage electrolyte containing a silicon-based additive according to claim 4, characterized in that: Step (3) Heat the deionized water to 88° C., then add mannitol, silicon-based additive, sodium borate and citric acid, continue heating to 97° C., and stir until completely dissolved at a stirring speed of 300 r / min.
6. The method for preparing a high-voltage electrolyte containing a silicon-based additive according to claim 1, characterized in that: Step (4) The product obtained in step (2) is mixed with the product obtained in step (3), and the mixture is stirred at 90° C. for 5 h at a stirring speed of 200 r / min.
7. The method for preparing a high-voltage electrolyte containing a silicon-based additive according to claim 1, characterized in that: Step (5) The product obtained in step (4) is mixed with fluoroethylene carbonate, ammonium dodecanedioate, lithium salt and ammonium dihydrogen phosphate, and the mixture is stirred at 90° C. for 0.5 h at a stirring speed of 800 r / min.
8. The method for preparing a high-voltage electrolyte containing a silicon-based additive according to claim 1, characterized in that: Step (6) Cool the product obtained in step (5) to 55° C., add o-nitroanisole, silicon-based additives, and mercaptobenzothiazole, and stir continuously until it is completely clarified at a stirring speed of 800 r / min; cool naturally to obtain a high-voltage electrolyte containing a silicon-based additive.
Citation Information