A method for promoting metal dendrite reaction of lithium ion battery

By introducing resting, charging formation, and aging steps into the lithium-ion battery manufacturing process, the metal dendrite reaction is promoted, which solves the problem of difficulty in identifying dendrite short circuit hazards in lithium-ion batteries in the factory and improves battery safety and performance.

CN118738577BActive Publication Date: 2024-11-15UNION LITHPLUS ENERGY (LIAONING) CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411216132.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-15
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Currently, it is difficult to effectively identify and remove batteries with potential short circuits caused by metal dendrites within the manufacturing plant, resulting in safety hazards entering the market.

Method used

Specific charging, aging, and resting steps are used to promote the metal dendrite reaction in lithium-ion batteries, enabling them to fully exhibit abnormal voltage drops within the manufacturing plant. These steps include resting, charging formation, aging, and multiple charge-discharge cycles to ensure that the metal impurity reaction proceeds fully.

Benefits of technology

It improves the efficiency of identifying and eliminating lithium-ion batteries with potential dendrite short circuits before they leave the factory, reduces safety risks, and improves fast charging and low-temperature charging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738577B_ABST
    Figure CN118738577B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of manufacturing process of lithium ion batteries, and specifically relates to a method for promoting metal dendrite reaction of lithium ion batteries. The steps are: the lithium ion battery is left to stand after liquid injection; charging and formation are performed; then aging is performed; standing and cooling; charging to 100% SOC with 0.5C-1C constant current and constant voltage, cut-off current 0.02C, standing for 10min, discharging to 0% SOC with 0.2C-1C constant current; then charging to 100% SOC with constant current and constant voltage, discharging to 20%-60% SOC with constant current, repeating this step of charging and discharging 2-5 times; finally replenishing electricity to 30%-50% SOC. The present invention can make the metal impurities inside the positive electrode of the lithium ion battery react more fully before leaving the factory, so that the lithium ion battery with abnormally high metal impurity content shows a voltage drop exceeding the qualified range, so that it is discovered and removed in the production stage, preventing such batteries with large voltage drop hidden dangers from entering the market and causing safety risks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of manufacturing process of lithium ion batteries, and in particular relates to a method for promoting metal dendrite reaction of lithium ion batteries. Background Art

[0002] Lithium-ion batteries are a type of battery that is currently commonly used and are widely used in digital products, power tools, automobiles, energy storage and other fields. If the battery's voltage drops quickly due to rapid self-discharge, it will cause the electrical equipment to work for a short time, and in severe cases, it may cause the battery to burn and explode. Therefore, the batteries that enter the market for circulation and use must not have abnormally fast self-discharge and abnormally large voltage drop, and require strict voltage screening before the battery leaves the factory. Because there are metal impurities in the positive electrode material of the battery, the metal impurities will gradually transfer to the negative electrode after the battery is charged and form metal dendrites at the negative electrode. The dendrites will seriously penetrate the diaphragm and contact the positive electrode, causing a short circuit inside the battery. The existing lithium-ion battery charging and discharging method can only react some of the positive electrode metal impurities. In the manufacturing plant, the battery with the risk of dendrite short circuit cannot fully show low voltage and be eliminated, resulting in being misjudged as a qualified battery and flowing into the market, causing safety hazards. Summary of the invention

[0003] The purpose of the present invention is to provide a method for promoting the metal dendrite reaction of lithium-ion batteries, so that batteries with potential dendrite short circuit risks can be identified and removed within the manufacturing plant, thereby reducing the probability of entering the market and reducing safety risks.

[0004] The present invention adopts the following technical scheme to achieve the above-mentioned purpose, a method for promoting metal dendrite reaction of lithium ion battery, and the specific steps are as follows:

[0005] Step S1, after the lithium-ion battery is filled with liquid, it is left to stand;

[0006] Step S2, charging and forming the lithium-ion battery after standing in a charging cabinet;

[0007] Step S3, aging the charged lithium-ion battery;

[0008] Step S4, the aged lithium-ion battery is left to stand for cooling;

[0009] Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 0.5C-1C constant current and constant voltage, with a cut-off current of 0.02C, and allowed to stand for 10 minutes, and discharged to 0% SOC at 0.2C-1C constant current; then charged to 100% SOC at constant current and constant voltage, and discharged to 20%-60% SOC at constant current, and this charging and discharging step is repeated 2-5 times; finally, the battery is charged to 30%-50% SOC.

[0010] In the above-mentioned method for promoting metal dendrite reaction of lithium-ion batteries, in step S1, the standing is standing in an environment of 20-50° C. for 24-72 hours.

[0011] In the above-mentioned method for promoting metal dendrite reaction of lithium-ion batteries, in step S2, the battery is charged to 90%-100% SOC in a constant current and constant voltage manner, and the cut-off current is 0.02C-0.05C.

[0012] In the above-mentioned method for promoting metal dendrite reaction of lithium-ion batteries, in step S3, the aging is to transfer the charged and formed lithium-ion battery into a high temperature environment of 45±5°C for aging.

[0013] In the above-mentioned method for promoting metal dendrite reaction of lithium-ion batteries, the standing still is to place the sample in an environment of 25±5°C for 12-48 hours to cool the sample.

[0014] The symbol C above represents the current rate of the battery.

[0015] The beneficial effects of the present invention are as follows: the present invention can make the metal impurities in the positive electrode of the lithium-ion battery react more fully before leaving the factory, so that the lithium-ion battery with abnormally high metal impurity content exhibits a voltage drop exceeding the qualified range, so that it can be discovered and removed in the production stage, preventing such batteries with large voltage drop hidden dangers from entering the market and causing safety risks. After the formation charge is charged to 0%-100% SOC, aging is performed, and the cycle performance of the lithium-ion battery during fast charging and low-temperature charging can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a flow chart of the method of the present invention. DETAILED DESCRIPTION

[0017] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.

[0018] Example 1

[0019] The above contents of the present invention are further described in detail below in conjunction with the accompanying drawings. Figure 1 As shown, taking a 18650-2.0Ah nickel-cobalt-manganese ternary lithium-ion battery as an example, a method of promoting a metal dendrite reaction of a 18650 lithium-ion battery in this embodiment specifically comprises the following steps:

[0020] Step S1, after the lithium-ion battery is filled with liquid, it is placed in an environment of 25±5°C for 24-48 hours;

[0021] Step S2, the lithium-ion battery after standing is charged and formed in a charging cabinet, respectively, at 0.2A constant current charging for 30min, 0.4A constant current charging for 90min, 1A constant current charging for 60min, 1A constant current constant voltage charging to 4.2V, and the cut-off current is 0.04A;

[0022] Step S3, the charged lithium-ion battery is formed, and after measuring the voltage, it is transferred to a high temperature environment of 45±5° C. and stored for 3 days for aging;

[0023] Step S4, the aged lithium-ion battery is placed in an environment of 25±5°C for 24 hours to cool down;

[0024] Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 1A constant current and constant voltage, with a cut-off current of 0.04A, and allowed to stand for 10 minutes. It is then discharged to 2.5V at 1A constant current, allowed to stand for 5 minutes, and discharged to 2.5V at 0.4A constant current, and allowed to stand for 5 minutes. It is then charged to 4.2V at 2A constant current and constant voltage, with a cut-off current of 0.04A, and discharged to 3.5V at 2A constant current. This charging and discharging step is repeated twice. Finally, it is supplemented to 3.6V at 1A constant current and constant voltage, with a cut-off current of 0.04A.

[0025] Comparative Example 1

[0026] Step S1, after the lithium-ion battery is filled with liquid, it is placed in an environment of 25±5°C for 24-48 hours;

[0027] Step S2, the lithium-ion battery after standing is charged and formed in a charging cabinet, respectively at a constant current of 0.2A for 30 minutes, a constant current of 0.4A for 90 minutes, and a constant current of 1A for 60 minutes;

[0028] Step S3, the charged lithium-ion battery is formed, and after measuring the voltage, it is transferred to a high temperature environment of 45±5° C. and stored for 3 days for aging;

[0029] Step S4, the aged lithium-ion battery is placed in an environment of 25±5°C for 24 hours to cool down;

[0030] Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 1A constant current and constant voltage, with a cut-off current of 0.04A, and allowed to stand for 10 minutes. It is then discharged to 2.5V at 1A constant current, allowed to stand for 5 minutes, and discharged to 2.5V at 0.4A constant current; finally, it is supplemented to 3.6V at 1A constant current and constant voltage, with a cut-off current of 0.04A.

[0031] Example 2

[0032] The above contents of the present invention are further described in detail below in conjunction with the accompanying drawings. Figure 1As shown, taking a 18650-3.0Ah nickel-cobalt-manganese ternary lithium-ion battery as an example, a method of promoting a metal dendrite reaction of a 18650 lithium-ion battery in this embodiment specifically comprises the following steps:

[0033] Step S1, after the lithium-ion battery is filled with liquid, it is placed in an environment of 25±5°C for 24-48 hours;

[0034] Step S2, the lithium-ion battery after standing is charged and formed in a charging cabinet, respectively, at 0.3A constant current charging for 30min, 0.6A constant current charging for 90min, 1.5A constant current charging for 60min, and 1.5A constant current constant voltage charging to 4.2V, with a cut-off current of 0.06A;

[0035] Step S3, the charged lithium-ion battery is formed, and after measuring the voltage, it is transferred to a high temperature environment of 45±5° C. and stored for 3 days for aging;

[0036] Step S4, the aged lithium-ion battery is placed in an environment of 25±5°C for 24 hours to cool down;

[0037] Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 1.5A constant current and constant voltage, with a cut-off current of 0.06A, and allowed to stand for 10 minutes. It is then discharged to 2.5V at 1.5A constant current, allowed to stand for 5 minutes, and discharged to 2.5V at 0.6A constant current, and allowed to stand for 5 minutes; then charged to 4.2V at 3A constant current and constant voltage, with a cut-off current of 0.06A, and discharged to 3.5V at 3A constant current, and this charging and discharging step is repeated twice; finally, it is supplemented to 3.6V at 1.5A constant current and constant voltage, with a cut-off current of 0.06A.

[0038] Comparative Example 2

[0039] Step S1, after the lithium-ion battery is filled with liquid, it is placed in an environment of 25±5°C for 24-48 hours;

[0040] Step S2, the lithium-ion battery after standing is charged and formed in a charging cabinet, respectively at a constant current of 0.3A for 30 minutes, a constant current of 0.6A for 90 minutes, and a constant current of 1.5A for 60 minutes;

[0041] Step S3, the charged lithium-ion battery is formed, and after measuring the voltage, it is transferred to a high temperature environment of 45±5° C. and stored for 3 days for aging;

[0042] Step S4, the aged lithium-ion battery is placed in an environment of 25±5°C for 24 hours to cool down;

[0043] Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 1.5A constant current and constant voltage, with a cut-off current of 0.06A, and allowed to stand for 10 minutes. It is then discharged to 2.5V at 1.5A constant current, allowed to stand for 5 minutes, and discharged to 2.5V at 0.6A constant current; finally, it is supplemented to 3.6V at 1.5A constant current and constant voltage, with a cut-off current of 0.06A.

[0044] Example 3

[0045] The above contents of the present invention are further described in detail below in conjunction with the accompanying drawings. Figure 1 As shown, taking a 14500-0.68Ah nickel-cobalt-manganese ternary lithium-ion battery as an example, a method of promoting a metal dendrite reaction of a 14500 lithium-ion battery in this embodiment specifically comprises the following steps:

[0046] Step S1, after the lithium-ion battery is filled with liquid, it is placed in an environment of 25±5°C for 24-48 hours;

[0047] Step S2, the lithium-ion battery after standing is charged and formed in a charging cabinet, respectively, at 0.068A constant current charging for 30min, 0.136A constant current charging for 90min, 0.34A constant current charging for 60min, and 0.34A constant current constant voltage charging to 4.2V, with a cut-off current of 0.013A;

[0048] Step S3, the charged lithium-ion battery is formed, and after measuring the voltage, it is transferred to a high temperature environment of 45±5° C. and stored for 3 days for aging;

[0049] Step S4, the aged lithium-ion battery is placed in an environment of 25±5°C for 24 hours to cool down;

[0050] Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 0.34A constant current and constant voltage, with a cut-off current of 0.013A, and allowed to stand for 10 minutes. It is then discharged to 2.5V at 0.34A constant current, allowed to stand for 5 minutes, and discharged to 2.5V at 0.136A constant current, and allowed to stand for 5 minutes; then charged to 4.2V at 0.68A constant current and constant voltage, with a cut-off current of 0.013A, and discharged to 3.5V at 0.68A constant current and constant voltage, and this charging and discharging step is repeated twice; finally, it is supplemented to 3.7V at 1A constant current and constant voltage, with a cut-off current of 0.013A.

[0051] Comparative Example 3

[0052] Step S1, after the lithium-ion battery is filled with liquid, it is placed in an environment of 25±5°C for 24-48 hours;

[0053] Step S2, the lithium-ion battery after standing is charged and formed in a charging cabinet, respectively, at a constant current of 0.068A for 30 minutes, at a constant current of 0.136A for 90 minutes, and at a constant current of 0.34A for 60 minutes;

[0054] Step S3, the charged lithium-ion battery is formed, and after measuring the voltage, it is transferred to a high temperature environment of 45±5° C. and stored for 3 days for aging;

[0055] Step S4, the aged lithium-ion battery is placed in an environment of 25±5°C for 24 hours to cool down;

[0056] Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 0.34A constant current and constant voltage, with a cut-off current of 0.013A, and allowed to stand for 10 minutes. It is then discharged to 2.5V at 0.34A constant current, allowed to stand for 5 minutes, and discharged to 2.5V at 0.013A constant current; finally, it is supplemented to 3.7V at 0.34A constant current and constant voltage, with a cut-off current of 0.013A.

[0057] Example 4 Experimental Verification

[0058] Test plan:

[0059] 1. Take the positive electrode material with excessive magnetic material to make battery A.

[0060] 2. Take half of the battery A1 and perform the process according to the embodiment, and the other half of the battery A2 and perform the process according to the corresponding comparative example.

[0061] Test results:

[0062] For battery A1 implemented in the embodiment, the low voltage defective rates of embodiments 1-3 are 14.5%, 14.1%, and 15.5%, respectively; for battery A2 implemented in the comparative example, the low voltage defective rates of comparative examples 1-3 are 0.86%, 0.91%, and 0.74%, respectively. This shows that the embodiment method has a significant effect on promoting the reaction of magnetic substances in the positive electrode material, and can make the low voltage of the battery caused by the metal dendrites generated by the magnetic substance appear, so that it can be identified and removed in the production process to avoid entering the market and causing safety risks.

Claims

1. A method for promoting metal dendrite reaction in lithium ion batteries, characterized in that: The specific steps are: Step S1, after the lithium-ion battery is filled with liquid, it is placed in an environment of 20-50°C for 24-72 hours; Step S2, the lithium-ion battery after standing is charged and formed in a charging cabinet, and the formation is charged to 90%-100% SOC in a constant current and constant voltage mode, and the cut-off current is 0.02C-0.05C; Step S3, the charged and formed lithium-ion battery is placed in a high temperature environment of 45±5°C for aging; Step S4, the aged lithium-ion battery is placed in an environment of 25±5°C for 12-48 hours to cool down; Step S5, the lithium-ion battery cooled to 25±5°C is charged to 100% SOC at 0.5C-1C constant current and constant voltage, with a cut-off current of 0.02C, and allowed to stand for 10 minutes, and discharged to 0% SOC at 0.2C-1C constant current; then charged to 100% SOC at constant current and constant voltage, and discharged to 20%-60% SOC at constant current, and this charging and discharging step is repeated 2-5 times; finally, the battery is charged to 30%-50% SOC.