High-activity positive electrode material for lithium carbon dioxide battery
By preparing highly active cathode materials, the problems of low overpotential and slow reaction kinetics of lithium carbon dioxide batteries are solved, the discharge platform and electric energy output of the battery are improved, and efficient catalytic conversion of carbon dioxide and cycle stability are achieved.
Patent Information
- Application Number
- CN202411048220.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-01
AI Technical Summary
Lithium carbon dioxide batteries face problems such as low overpotential, slow reaction kinetics and poor electrode activity, resulting in actual output voltage being much lower than the theoretical value, affecting the quality of electric energy and the utilization efficiency of carbon dioxide.
A method for preparing highly active cathode materials is adopted, by stirring a metal salt compound and polyvinylpyrrolidone in deionized water, adding a metal cyanide compound, and subjecting it to freeze-drying and high-temperature calcination to obtain a metal-containing highly active cathode material, which is combined with a conductive agent Mix it with the current collector and coat it on the electrode to improve the discharge platform and power output of lithium carbon dioxide batteries.
It improves the discharge platform of lithium carbon dioxide batteries to above 3.0V, improves electrical energy output, enhances carbon dioxide catalytic conversion activity and cycle stability, ensures the effective transmission of ions, electrons and CO2 molecules, and improves high-rate capacity and cycle stability. .
Smart Images

Figure CN118738683A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of novel battery energy storage technology, and more specifically, to a highly active positive electrode material for a lithium carbon dioxide battery that can be reversibly discharged and charged in a carbon dioxide environment and has a relatively small overpotential. Background Art
[0002] Carbon capture and utilization has received increasing attention in the fields of CO2 reduction, future Mars migration, mitigation of global warming, and reduction of automobile exhaust emissions. Various carbon capture and utilization technologies have been developed to convert CO2 into value-added chemicals for electrochemical reduction, such as methane dry gas reforming and photocatalytic reduction. In the past development history, researchers have proposed a lithium carbon dioxide battery energy storage device, which provides an attractive strategy for generating electricity from carbon dioxide. A typical lithium carbon dioxide battery consists of a lithium metal anode, a porous carbon dioxide cathode, and a non-protonic electrolyte. The typical reversible reaction that occurs in a lithium carbon dioxide battery is: 4Li+CO2→2Li2CO3+C. Calculations show that the thermodynamic equilibrium potential of this reaction is approximately 2.80V, and the specific energy density is 1876Wh kg -1 , far exceeding traditional lithium-ion battery technology.
[0003] However, the lithium carbon dioxide batteries used in practice face serious problems such as parasitic reactions, slow reaction kinetics, and poor electrode activity. Their discharge voltage is usually around 2.5V, and sometimes even lower than 2.0V in many experimental studies. In general, the quality of electric energy is determined by the supply voltage. An output voltage below 3.0V results in very low electric energy. Obviously, the actual output voltage of lithium carbon dioxide batteries is much lower than the theoretical value, and it is not high enough. In addition to the thermodynamic information of the reaction, the voltage that the battery can provide also depends on the catalytic activity of the catalyst and the transfer properties of charge and mass in the body and between the phase boundaries. The development of positive electrode materials with high catalytic activity has an important impact on improving the power output of lithium carbon dioxide and more carbon dioxide utilization technologies. Summary of the invention
[0004] The present invention provides a highly active positive electrode material for a lithium carbon dioxide battery. The high-quality and fast electron transmission capability of the catalyst positive electrode material itself increases the discharge platform of the lithium carbon dioxide battery to above 3.0V, thereby promoting its power supply and output.
[0005] The present invention firstly provides a method for preparing a highly active positive electrode material for a lithium carbon dioxide battery.
[0006] A second object of the present invention is to provide a highly active cathode material that provides superior electrochemical performance in a lithium carbon dioxide battery.
[0007] In order to achieve the above-mentioned invention object, a series of technical solutions are adopted for implementation:
[0008] A method for preparing a highly active positive electrode material for a lithium carbon dioxide battery comprises the following steps:
[0009] (1) adding a metal salt compound and polyvinyl pyrrolidone into deionized water and stirring to obtain a clear and uniform mixed solution;
[0010] (2) adding the metal cyanide compound into a deionized water solution and stirring to obtain a uniform and clear mixed solution;
[0011] (3) slowly and gradually dripping the solution obtained in step (1) into the solution obtained in step (2), and stirring continuously at room temperature for 24 hours to obtain a uniform mixture;
[0012] (4) washing the mixture obtained in step (3) with deionized water, centrifuging it 2 to 3 times, and then drying it in a freeze dryer to obtain a highly active positive electrode material precursor;
[0013] (5) The precursor material obtained in step (4) is subjected to high-temperature calcination treatment under an inert protective atmosphere to obtain a metal-containing high-activity positive electrode material; the temperature is initially raised to 500-800° C. and maintained for 1-3 hours to perform a carbonization treatment on the sample, and then the temperature is raised to 800-1000° C. and maintained for 1-3 hours to perform a metal reduction treatment to obtain a metal-containing high-activity positive electrode material.
[0014] The metal salt compound is one of a cobalt nitrate nonahydrate compound, a cobalt chloride nonahydrate compound, a cobalt nitrate hexahydrate compound, and a cobalt chloride hexahydrate compound.
[0015] The metal cyanide compound is potassium hexacyanocobaltate (III).
[0016] The molar ratio of the metal salt compound to the metal cyanide compound is 0.05 to 2:1.
[0017] The freeze-drying time is 15 to 24 hours.
[0018] The protective atmosphere is at least one of nitrogen and argon; the gas flow rate is 20-50 ml / min.
[0019] The temperature for starting the carbonization calcination process is 550° C., the heat preservation time is 1 hour, and the heating rate is 1-5° C. / min.
[0020] The temperature of the latter metal reduction calcination process is 900° C., the heat preservation time is 2 hours, and the heating rate is 1-3° C. / min.
[0021] The lithium carbon dioxide battery high-activity positive electrode material is used to prepare a lithium carbon dioxide electrode. The high-activity positive electrode material is mixed with a conductive agent and polyvinylidene fluoride in a mass ratio of 4:4:1 in N-methylpyrrolidone and coated on a current collector.
[0022] Wherein, the conductive agent is at least one of Super P, carbon nanotubes, Ketjen black, carbocarbon, acetylene black, carbon black, and graphene, and the current collector is at least one of carbon paper, carbon cloth, nickel mesh, stainless steel mesh, aluminum mesh, titanium mesh, and carbon mesh.
[0023] The beneficial effects of the present invention are as follows:
[0024] The high-activity positive electrode material provided by the present invention exhibits excellent carbon dioxide catalytic conversion activity in a lithium carbon dioxide battery, can withstand the material structure volume strain brought about during repeated cycles, ensure the effective transmission of ions, electrons, and CO2 molecules, increase the electrode-electrolyte contact area, and enhance the high-rate capacity and cycle stability; the high catalytic activity of the positive electrode material designed by the present invention enables the discharge platform of the lithium carbon dioxide battery to be above 3.0V, has extremely high electrical energy output, and has promoted gas reduction / oxidation reaction kinetics. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 This is a scanning electron microscope (SEM) image of the highly active positive electrode material obtained in Example 1 of the present invention;
[0027] Figure 2 The X-ray diffraction pattern (XRD pattern) of the high-activity positive electrode material obtained in Example 1 of the present invention;
[0028] Figure 3 The full discharge spectrum of the lithium carbon dioxide battery prepared with the high-activity positive electrode material obtained in Example 1 of the present invention at a current density of 200 mA / g;
[0029] Figure 4 The cyclic discharge spectrum of the lithium carbon dioxide battery prepared by the high-activity positive electrode material obtained in Example 1 of the present invention at a current density of 400 mA / g and a cut-off capacity of 1000 mAh / g;
[0030] Figure 5The rate performance spectrum of the lithium carbon dioxide battery prepared with the high-activity positive electrode material obtained in Example 1 of the present invention at a cut-off capacity of 1000 mAh / g at different current densities; DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0032] The experimental methods in the following examples are all conventional methods unless otherwise specified.
[0033] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0034] In the following embodiments:
[0035] (1) Scanning electron microscope test instrument model: SUPRA 55, Germany.
[0036] (2) X-ray diffraction test instrument model: Bruker D8, USA.
[0037] (2) Full discharge performance test: The instrument model used is: Land, Wuhan; test parameters: current density 0.2 mA / g.
[0038] (3) Cyclic performance test: The instrument model used is: Land, Wuhan; test parameters: current density 0.4 mA / g.
[0039] Lithium Carbon Dioxide Battery Cathode Preparation:
[0040] The high-activity positive electrode material prepared by the present invention: Super P conductive agent: polyvinylidene fluoride = 4:4:1 mass ratio is ground in a mortar, and then an appropriate amount of N-methylpyrrolidone is dropped into it and fully ground to a dispersed viscous state to obtain an active slurry, and the slurry is evenly coated on a porous carbon paper current collector with a coating scraper, and placed in a vacuum drying oven and heated to 100° C. under vacuum state, and kept warm for 24 hours to obtain a dried lithium carbon dioxide battery positive electrode plate, and the plate is cut into a circular plate with a diameter of 11 mm by a plate cutting machine, and the loading amount of a single active material is 0.20 mg, which is convenient for assembling a lithium carbon dioxide battery.
[0041] Preparation of metal-air battery:
[0042] Assemble a lithium carbon dioxide battery in an argon atmosphere with a water and oxygen content of <0.01ppm, place the shrapnel, gasket, lithium sheet, and diaphragm into the negative electrode shell in order, drop 150μL of battery electrolyte, then put the above-cut positive electrode sheet and positive electrode shell, and press the battery with a sealing machine to obtain a button battery.
[0043] The diaphragm is a glass fiber diaphragm, model GF / D;
[0044] The lithium carbon dioxide battery electrolyte is 1M LiTFSI / DMSO;
[0045] The button battery model size is CR 2032.
[0046] Example 1
[0047] (1) Weigh 0.1 mol of cobalt nitrate nonahydrate and 1 g of polyvinyl pyrrolidone, add them into 100 mL of deionized water, and stir them thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform yellow clear liquid;
[0048] (2) Weigh 0.05 mol of potassium hexacyanocobaltate (III) and add it to 100 mL of deionized water. Stir the mixture thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid.
[0049] (3) The yellow clear liquid was slowly dripped into the colorless clear liquid, and the liquid was observed to gradually turn into a pink turbid state. The mixed liquid was continuously stirred at room temperature at a stirring speed of 200 rpm for 24 h, and then centrifuged and washed with deionized water for 3 times. The product was transferred to a freeze dryer and dried for 24 h;
[0050] (4) The dried sample is placed in a crucible and transferred to a tube furnace for high-temperature annealing. The annealing procedure is as follows: under argon protection, the temperature is increased from room temperature to 550°C at a rate of 2°C / min and kept at that temperature for 1 hour; then the temperature is increased from 550°C to 900°C at a rate of 2°C / min and kept at that temperature for 2 hours. The black positive electrode material product is obtained by naturally cooling to room temperature.
[0051] The SEM spectrum of the cathode catalyst obtained in this example is as follows Figure 1 As shown, it is composed of dispersed nanoparticles;
[0052] The XRD pattern of the cathode catalyst obtained in this example is as follows Figure 2 As shown, its characteristic peaks correspond to the multiphase compounds of Co;
[0053] The lithium carbon dioxide battery obtained in this embodiment has an initial discharge capacity of 2.392645 mAh at a current density of 100 mA / g, which is converted into a mass discharge capacity of 23926.45 mAh / g. Figure 3 As shown;
[0054] The lithium carbon dioxide battery obtained in this embodiment can stably cycle 150 times when the cut-off capacity is 500 mAh / g at 200 mA / g. The test results are as follows: Figure 4 shown.
[0055] The lithium carbon dioxide battery obtained in this example is subjected to different current densities (100-1000 mA g -1 ) When the cut-off capacity is 500mAh / g, its rate performance is very stable and the overpotential is small. The test results are as follows Figure 5 shown.
[0056] Example 2
[0057] (1) Weighing 0.05 mol of cobalt nitrate nonahydrate and 1 g of polyvinyl pyrrolidone, adding them to 100 mL of deionized water, stirring them at room temperature at a stirring speed of 200 rpm to obtain a uniform yellow clear liquid;
[0058] (2) Weigh 0.05 mol of potassium hexacyanocobaltate (III) and add it to 100 mL of deionized water. Stir the mixture thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid.
[0059] (3) The yellow clear liquid was slowly dripped into the colorless clear liquid, and the liquid was observed to gradually turn into a pink turbid state. The mixed liquid was continuously stirred at room temperature at a stirring speed of 200 rpm for 24 h, and then centrifuged and washed with deionized water for 3 times. The product was transferred to a freeze dryer and dried for 24 h;
[0060] (4) The dried sample is placed in a crucible and transferred to a tube furnace for high-temperature annealing. The annealing procedure is as follows: under argon protection, the temperature is increased from room temperature to 550°C at a rate of 5°C / min and kept at that temperature for 1 hour; then the temperature is increased from 550°C to 900°C at a rate of 5°C / min and kept at that temperature for 2 hours. The black positive electrode material product is obtained by naturally cooling to room temperature.
[0061] Example 3
[0062] (1) Weigh 0.1 mol of cobalt nitrate nonahydrate and 1 g of polyvinyl pyrrolidone, add them into 100 mL of deionized water, and stir them thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform yellow clear liquid;
[0063] (2) Weigh 0.05 mol of potassium hexacyanocobaltate (III) and add it to 100 mL of deionized water. Stir the mixture thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid.
[0064] (3) The yellow clear liquid was slowly dripped into the colorless clear liquid, and the liquid was observed to gradually turn into a pink turbid state. The mixed liquid was continuously stirred at room temperature at a stirring speed of 200 rpm for 24 h, and then centrifuged and washed with deionized water for 3 times. The product was transferred to a freeze dryer and dried for 24 h;
[0065] (4) The dried sample is placed in a crucible and transferred to a tube furnace for high-temperature annealing. The annealing procedure is as follows: under argon protection, the temperature is raised from room temperature to 900°C at a rate of 5°C / min, kept at this temperature for 3 hours, and naturally cooled to room temperature to obtain a black positive electrode material product.
[0066] Example 4
[0067] (1) Weigh 0.1 mol of cobalt nitrate nonahydrate and 1 g of polyvinyl pyrrolidone, add them into 100 mL of deionized water, and stir them thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform yellow clear liquid;
[0068] (2) Weigh 0.05 mol of potassium hexacyanocobaltate (III) and add it to 100 mL of deionized water. Stir the mixture thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid.
[0069] (3) The yellow clear liquid was slowly dripped into the colorless clear liquid, and the liquid was observed to gradually turn into a pink turbid state. The mixed liquid was continuously stirred at room temperature at a stirring speed of 200 rpm for 24 h, and then centrifuged and washed with deionized water for 3 times. The product was transferred to a freeze dryer and dried for 24 h;
[0070] (4) The dried sample is placed in a crucible and transferred to a tube furnace for high-temperature annealing. The annealing procedure is as follows: under argon protection, the temperature is raised from room temperature to 900°C at a rate of 2°C / min, kept at this temperature for 3 h, and naturally cooled to room temperature to obtain a black positive electrode material product.
[0071] Example 5
[0072] (1) Weighing 0.05 mol of cobalt nitrate nonahydrate and 1 g of polyvinyl pyrrolidone, adding them to 100 mL of deionized water, stirring them at room temperature at a stirring speed of 200 rpm to obtain a uniform yellow clear liquid;
[0073] (2) Weigh 0.05 mol of potassium hexacyanocobaltate (III) and add it to 100 mL of deionized water. Stir the mixture thoroughly at room temperature at a stirring speed of 200 rpm to obtain a uniform colorless clear liquid.
[0074] (3) The yellow clear liquid was slowly dripped into the colorless clear liquid, and the liquid was observed to gradually turn into a pink turbid state. The mixed liquid was continuously stirred at room temperature at a stirring speed of 200 rpm for 24 h, and then centrifuged and washed with deionized water for 3 times. The product was transferred to a freeze dryer and dried for 24 h;
[0075] (4) The dried sample is placed in a crucible and transferred to a tube furnace for high-temperature annealing. The annealing procedure is as follows: under argon protection, the temperature is raised from room temperature to 900°C at a rate of 2°C / min, kept at this temperature for 3 h, and naturally cooled to room temperature to obtain a black positive electrode material product.
[0076] The above-described embodiments of the present invention do not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A highly active positive electrode material for a lithium carbon dioxide battery, characterized in that: The following steps are involved: (1) adding a metal salt compound and polyvinyl pyrrolidone into deionized water and stirring to obtain a clear and uniform mixed solution; (2) adding the metal cyanide compound into the deionized water solution and stirring to obtain a uniform and clear mixed solution; (3) slowly and gradually dripping the solution obtained in step (1) into the solution obtained in step (2), and stirring continuously at room temperature for 24 hours to obtain a uniform mixture; (4) washing the mixture obtained in step (3) with deionized water, centrifuging it 2 to 3 times, and then drying it in a freeze dryer to obtain a highly active positive electrode material precursor; (5) The precursor material obtained in step (4) is subjected to high-temperature calcination treatment under an inert protective atmosphere to obtain a metal-containing high-activity positive electrode material; the temperature is initially raised to 500-800° C. and maintained for 1-3 hours to perform a carbonization treatment on the sample, and then the temperature is raised to 800-1000° C. and maintained for 1-3 hours to perform a metal reduction treatment to obtain a metal-containing high-activity positive electrode material.
2. The highly active positive electrode material for a lithium carbon dioxide battery according to claim 1, characterized in that: The metal salt compound in step (1) is one of a cobalt nitrate nonahydrate compound, a cobalt chloride nonahydrate compound, a cobalt nitrate hexahydrate compound, and a cobalt chloride hexahydrate compound.
3. The highly active positive electrode material for a lithium carbon dioxide battery according to claim 1, characterized in that: The metal cyanide compound in step (2) is potassium hexacyanocobaltate (III).
4. The molar ratio of the metal salt compound to the metal cyanide compound as claimed in claim 1 is 0.05 to 2:
1.
5. The highly active positive electrode material for a lithium carbon dioxide battery according to claim 1, characterized in that: The freeze-drying time in step (4) is 15 to 24 hours.
6. The highly active positive electrode material for a lithium carbon dioxide battery according to claim 1, characterized in that: The protective atmosphere in step (5) is at least one of nitrogen and argon; and the gas flow rate is 20 to 50 ml / min.
7. The highly active positive electrode material for a lithium carbon dioxide battery according to claim 1, characterized in that: In step (5), the temperature at which the carbonization calcination process of the high-activity positive electrode material for lithium carbon dioxide batteries begins is 550° C., the holding time is 1 hour, and the heating rate is 1 to 5° C. / min.
8. The highly active positive electrode material for a lithium carbon dioxide battery according to claim 1, characterized in that: In step (5), the temperature of the rear-stage metal reduction calcination process of the high-activity positive electrode material for lithium carbon dioxide batteries is 900° C., the holding time is 2 hours, and the heating rate is 1 to 3° C. / min.
9. The highly active positive electrode material for a lithium carbon dioxide battery according to claim 1, characterized in that: The lithium carbon dioxide battery electrode is prepared by mixing the high-activity positive electrode material, the conductive agent and polyvinylidene fluoride in N-methylpyrrolidone at a mass ratio of 4:4:1 and coating the mixture on the current collector.
10. The lithium carbon dioxide battery electrode according to claim 9, characterized in that: The conductive agent is at least one of Super P, carbon nanotubes, Ketjen black, carbocarbon, acetylene black, carbon black, and graphene, and the current collector is at least one of carbon paper, carbon cloth, nickel mesh, stainless steel mesh, aluminum mesh, titanium mesh, and carbon mesh.
Citation Information
Patent Citations
Anode material used for lithium-carbon dioxide battery, preparation method and application thereof
CN109830678A
Preparation method and application of composite material with elemental cobalt coated with carbon nanotubes
CN110571439A
Carbon coating method of Prussian blue material for sodium ion battery
CN114725383A
Lithium-carbon dioxide battery positive electrode material and preparation method and application thereof
CN117525454A
Method of synthesizing porous composite including single atom metal catalysts and nitrogen atoms in hierarchical carbon material from carbon dioxide containing gas
US20230055011A1