Diaphragm-negative electrode composite sheet and preparation method thereof, lithium ion battery and vehicle
By using a solid electrolyte layer composed of Li5.3PS4.3ClBr0.7 and LiPON and a separator-negative electrode composite sheet of a conductive material negative electrode layer in a lithium-ion battery, the balance between volume utilization and fast charging capability of the lithium-ion battery is solved. problem, achieving high battery life and fast charging capabilities of lithium-ion batteries.
Patent Information
- Application Number
- CN202410959204.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing lithium iron phosphate power batteries are difficult to balance between volume utilization and fast charging capabilities, resulting in battery life anxiety and energy replenishment anxiety that have not been effectively resolved.
A separator-negative electrode composite sheet is used, including a base film and a solid electrolyte layer covering the surface of the base film. The solid electrolyte is composed of Li5.3PS4.3ClBr0.7 and LiPON. The negative electrode layer is a conductive material deposited by magnetic field sputtering technology. Form, optimize the thickness and porosity of the solid electrolyte layer and base film, and improve the energy density and fast charging capability of lithium-ion batteries.
By reducing the amount of electrolyte injection, reducing the weight of lithium-ion batteries and improving their energy density and fast-charging capabilities, the shortcomings of lithium-ion battery life and fast-charging capabilities are solved.
Smart Images

Figure CN118738769A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a diaphragm-negative electrode composite sheet and a preparation method thereof, a lithium ion battery and a vehicle. Background Art
[0002] At present, the new energy vehicle industry is still committed to solving the anxiety of battery life and energy replenishment. For example, the existing lithium iron phosphate power battery uses CTP module-free structure design, which greatly improves the volume utilization rate, thereby effectively improving its battery life. However, it is still difficult to balance the fast charging capacity of the battery. Therefore, the problems of battery life and energy replenishment are still urgent problems to be solved in the new energy vehicle industry. Summary of the invention
[0003] Based on this, it is necessary to provide a diaphragm-negative electrode composite sheet and its preparation method, a lithium-ion battery and a vehicle to address the above problems. The lithium-ion battery using the diaphragm-negative electrode composite sheet can simultaneously improve the endurance and fast charging capabilities.
[0004] A diaphragm-negative electrode composite sheet, the diaphragm-negative electrode composite sheet comprises a diaphragm and a negative electrode layer attached to one surface of the diaphragm, wherein the diaphragm comprises a base film and a solid electrolyte layer coated on the surface of the base film, and the solid electrolyte in the solid electrolyte layer comprises Li 5.3 PS 4.3 ClBr 0.7 and LiPON, wherein the material of the negative electrode layer is a conductive material.
[0005] In one embodiment, the solid electrolyte also satisfies at least one of the following conditions:
[0006] (1) Li in the solid electrolyte 5.3 PS 4.3 ClBr 0.7 The mass ratio with LiPON is 90:10-55:45;
[0007] (2) The mass fraction of the solid electrolyte in the solid electrolyte layer is 85%-98%.
[0008] In one embodiment, the solid electrolyte layer further satisfies at least one of the following conditions:
[0009] (1) The particle size of the solid electrolyte is 2 μm-15 μm;
[0010] (2) The thickness of the solid electrolyte layer is 1 μm-3 μm;
[0011] (3) The porosity of the solid electrolyte layer is 20%-60%.
[0012] In one embodiment, the base film satisfies at least one of the following conditions:
[0013] (1) The thickness of the base film is 2 μm-6 μm;
[0014] (2) The porosity of the base film is 30%-65%.
[0015] In one embodiment, the negative electrode layer satisfies at least one of the following conditions:
[0016] (1) The thickness of the negative electrode layer is 100 μm-200 μm;
[0017] (2) The conductive material is selected from carbon materials;
[0018] (3) The negative electrode layer has a mesoporous structure.
[0019] A method for preparing the separator-negative electrode composite sheet comprises the following steps:
[0020] preparing a solid electrolyte into a slurry;
[0021] Placing the slurry on the surface of the base film and drying to obtain a diaphragm;
[0022] A negative electrode layer is formed on one surface of the separator.
[0023] In one of the embodiments, the negative electrode layer is deposited on one surface of the diaphragm by means of magnetic field sputtering.
[0024] A lithium ion battery comprises a positive electrode sheet, the separator-negative electrode composite sheet and an electrolyte.
[0025] In one embodiment, the lithium-ion battery is a lithium iron phosphate battery or a ternary lithium battery.
[0026] A vehicle using the lithium-ion battery.
[0027] In the present invention, Li 5.3 PS 4.3 ClBr 0.7 The solid electrolyte layer obtained by cooperating with LiPON has a large amount of active lithium, which can reduce the injection amount of electrolyte from about 3g / Ah to less than 1g / Ah, reduce the weight of lithium-ion batteries, and thus improve the energy density of lithium-ion batteries. 5.3 PS 4.3 ClBr 0.7The solid electrolyte layer obtained by cooperating with LiPON has excellent ion conductivity and stability, thereby improving the fast charging capability of lithium-ion batteries; in addition, the present invention directly attaches the conductive material to the diaphragm as the negative electrode, which fits more closely, and the electron and ion transmission is smoother, which can avoid the use of current collectors, and is conducive to further improving the energy density of lithium-ion batteries. Therefore, the lithium-ion battery using the diaphragm-negative electrode composite sheet of the present invention can simultaneously improve the endurance and fast charging capabilities. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 It is a schematic diagram of the structure of the separator-negative electrode composite sheet of the present invention.
[0030] In the figure: 10, separator; 20, negative electrode layer; 101, base film; 102, solid electrolyte layer. DETAILED DESCRIPTION
[0031] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.
[0033] like Figure 1 As shown, the separator-negative electrode composite sheet provided by the present invention includes a separator 10 and a negative electrode layer 20 attached to one surface of the separator 10, wherein the separator 10 includes a base film 101 and a solid electrolyte layer 102 coated on the surface of the base film 101, and the solid electrolyte in the solid electrolyte layer 102 includes Li 5.3PS 4.3 ClBr 0.7 and LiPON, the material of the negative electrode layer 20 is a conductive material.
[0034] In the separator-negative electrode composite sheet of the present invention, Li 5.3 PS 4.3 ClBr 0.7 The solid electrolyte layer 102 obtained by cooperating with LiPON has a large amount of active lithium, so that the injection amount of the electrolyte can be reduced from about 3g / Ah to less than 1g / Ah, reducing the weight of the lithium-ion battery, and then the energy density of the lithium-ion battery can be increased, that is, the endurance of the lithium-ion battery is improved. At the same time, the use of Li 5.3 PS 4.3 ClBr 0.7 The solid electrolyte layer 102 obtained in cooperation with LiPON has excellent ion conductivity and stability, thereby improving the fast charging capability of the lithium-ion battery.
[0035] Moreover, using Li 5.3 PS 4.3 ClBr 0.7 It can also exhibit excellent processing performance when used in conjunction with LiPON, making it more suitable for large-scale mass production.
[0036] In the separator-negative electrode composite sheet of the present invention, the conductive material is directly attached to the separator 10 as the negative electrode, which fits more closely, and the electron and ion transmission is smoother, and the use of a current collector can be avoided, which is conducive to further improving the energy density of the lithium-ion battery. Therefore, the lithium-ion battery using the separator-negative electrode composite sheet of the present invention can simultaneously improve the endurance and fast charging capabilities.
[0037] It is understood that the solid electrolyte layer 102 of the present invention also includes auxiliary components such as binders, and the binders include but are not limited to polyvinylidene fluoride (PVDF), acrylates, acrylonitriles, etc. Preferably, the mass fraction of the solid electrolyte in the solid electrolyte layer 102 is 85%-98%.
[0038] Preferably, the particle size of the solid electrolyte is 2 μm-15 μm, so that there is more active lithium per unit volume.
[0039] Preferably, Li in the solid electrolyte 5.3 PS 4.3 ClBr 0.7 The mass fraction of LiPON is greater than that of LiPON. 5.3 PS 4.3 ClBr 0.7The mass ratio with LiPON is 90:10-55:45, which can show higher battery life and fast charging capabilities.
[0040] Preferably, the solid electrolyte layer 102 has a thickness of 1 μm-3 μm and a porosity of 20%-60%, which can better balance the ion conductivity and stability.
[0041] The present invention does not limit the selection of the base film 101, including but not limited to polyamide film, polypropylene film and polyester film. In the present invention, the thickness of the base film is preferably 2μm-6μm, and the porosity is preferably 30%-65%, so that the base film 101 has better ion conductivity and electronic insulation ability, and cooperates with the solid electrolyte layer 102 of the present invention, so that the lithium-ion battery can better improve the endurance and fast charging ability.
[0042] The thickness of the negative electrode layer 20 in the present invention is preferably 100 μm-200 μm, which can improve the electron and ion transmission capabilities.
[0043] Preferably, the conductive material is selected from carbon materials, which can have higher active sites and fast charging capabilities.
[0044] Preferably, the negative electrode layer 20 has a mesoporous structure, more preferably 5 μm-20 μm, so that even if metallic lithium is deposited in the negative electrode layer 20, it will be deposited uniformly without forming lithium dendrites, thereby not affecting the performance and life of the lithium-ion battery.
[0045] The present invention also provides a method for preparing a separator-negative electrode composite sheet, comprising the following steps:
[0046] preparing a solid electrolyte into a slurry;
[0047] The slurry is placed on the surface of the base film 101 and dried to obtain the separator 10;
[0048] The negative electrode layer 20 is formed on one surface of the separator 10 .
[0049] When the solid electrolyte is prepared into a slurry, the present invention preferably comprises Li 5.3 PS 4.3 ClBr 0.7 , LiPON and a binder are dispersed in a solvent such as N-methylpyrrolidone (NMP) to obtain a slurry. The slurry can be placed on the surface of the base film 101 by coating, such as gravure coating, and the solid electrolyte layer 102 is obtained after drying.
[0050] The negative electrode layer 20 can also be prepared by coating, etc., but the present invention further prefers magnetron sputtering, which can obtain a more uniform negative electrode layer 20. During preparation, the conductive material is first made into a thin sheet by casting, vapor deposition, etc., with a thickness of 5μm-3000μm, and then used as a cathode, and the diaphragm 10 to be sputtered is the anode. The equipment is first evacuated to a vacuum, and then 0.2Pa-5Pa of argon or other inert gas is introduced. The cathode generates glow discharge under the action of 1.5KV-2.5KV DC negative high voltage or 12MHz radio frequency voltage, and multiple magnetron sputtering is performed to deposit the negative electrode layer 20 on one surface of the diaphragm 10.
[0051] The present invention also provides a lithium ion battery, comprising a positive electrode sheet, the separator-negative electrode composite sheet and an electrolyte. In the lithium ion battery of the present invention, the separator-negative electrode composite sheet is used to replace the traditional separator and negative electrode sheet, and the injection amount of the electrolyte is reduced from about 3g / Ah to less than 1g / Ah, and the injection amount is preferably 0.1g / Ah-1g / Ah.
[0052] Optionally, the lithium-ion battery of the present invention is a lithium iron phosphate battery or a ternary lithium battery.
[0053] The present invention also provides a vehicle using the lithium-ion battery, which can better solve the problems of endurance and energy replenishment anxiety.
[0054] Hereinafter, the separator-negative electrode composite sheet and its preparation method, lithium-ion battery and vehicle will be further described through the following specific examples.
[0055] Example 1
[0056] 6 kg of Li 5.3 PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0057] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0058] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0059] Example 2
[0060] 7 kg of Li 5.3 PS 4.3 ClBr 0.7 , 3 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0061] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0062] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0063] Example 3
[0064] 7.5 kg of Li 5.3 PS 4.3 ClBr 0.7 , 2.5 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0065] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0066] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0067] Example 4
[0068] 8 kg of Li 5.3 PS 4.3 ClBr 0.7 , 2 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0069] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0070] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0071] Example 5
[0072] 8.5 kg of Li 5.3 PS 4.3 ClBr 0.7 , 1.5 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0073] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0074] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0075] Example 6
[0076] 5 kg of Li 5.3 PS 4.3 ClBr 0.7 , 5 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0077] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0078] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0079] Example 7
[0080] 4 kg of Li 5.3 PS 4.3 ClBr 0.7 , 6 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain slurry.
[0081] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0082] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0083] Example 8
[0084] 6 kg of Li 5.3 PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0085] A polypropylene film with a thickness of 6 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0086] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0087] Example 9
[0088] 6 kg of Li 5.3PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0089] A polypropylene film with a thickness of 8 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0090] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0091] Example 10
[0092] 6 kg of Li 5.3 PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0093] A polypropylene film with a thickness of 10 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0094] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0095] Embodiment 11
[0096] 6 kg of Li 5.3 PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0097] A polypropylene film with a thickness of 6 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 3 μm and the porosity is 50%.
[0098] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0099] Example 12
[0100] 6 kg of Li 5.3 PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0101] A polypropylene film with a thickness of 6 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 4 μm and the porosity is 50%.
[0102] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0103] Example 13
[0104] 6 kg of Li 5.3 PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0105] A polypropylene film with a thickness of 6 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 5 μm and the porosity is 50%.
[0106] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0107] Embodiment 14
[0108] 6 kg of Li 5.3PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0109] A polypropylene film with a thickness of 6 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0110] The carbon material is made into a thin sheet with a thickness of 10μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 150μm and a pore size of 10nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0111] Embodiment 15
[0112] 6 kg of Li 5.3 PS 4.3 ClBr 0.7 , 4 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0113] A polypropylene film with a thickness of 6 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0114] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates a glow discharge under the action of a 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 120 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0115] Comparative Example 1
[0116] 10 kg of Li 5.3 PS 4.3 ClBr 0.7 , 0.3 kg of polyvinylidene fluoride was dispersed in N-methylpyrrolidone to obtain a slurry.
[0117] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0118] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0119] Comparative Example 2
[0120] 10 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain slurry.
[0121] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0122] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0123] Comparative Example 3
[0124] 7 kg of Li 5.3 PS 4.3 ClBr 0.7 , 3kg of Li 1.2 Al 0.2 Ti 1.8 (PO4)3 and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain slurry.
[0125] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0126] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0127] Comparative Example 4
[0128] 7 kg of Li 5.3 PS4.3 ClBr 0.7 , 3 kg of Li2S and 0.3 kg of polyvinylidene fluoride are dispersed in N-methylpyrrolidone to obtain a slurry.
[0129] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0130] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0131] Comparative Example 5
[0132] 7 kg of Li 1.2 Al 0.2 Ti 1.8 (PO4)3, 3 kg of LiPON and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain slurry.
[0133] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0134] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0135] Comparative Example 6
[0136] 7 kg of Li2S, 3 kg of LiPON, and 0.3 kg of polyvinylidene fluoride were dispersed in N-methylpyrrolidone to obtain a slurry.
[0137] A polypropylene film with a thickness of 4 μm and a porosity of 45% is provided, and then the above slurry is coated on both sides of the polypropylene film. After drying, a diaphragm is obtained. In the diaphragm, the thickness of the single-sided solid electrolyte layer is 2 μm and the porosity is 50%.
[0138] The carbon material is made into a thin sheet with a thickness of 10 μm and used as the cathode. The above-obtained diaphragm is used as the anode. The system is evacuated and then 1 Pa of argon gas is introduced. The cathode generates glow discharge under the action of 2 KV DC negative high voltage. After multiple magnetron sputtering, a negative electrode layer with a thickness of 170 μm and a pore size of 10 nm is deposited on one surface of the diaphragm to obtain a diaphragm-negative electrode composite sheet.
[0139] The separator-negative electrode composite sheets obtained in Examples 1-15 and Comparative Examples 1-6 were assembled into power lithium-ion batteries, wherein the electrolyte injection amount was 0.5 g / Ah, and then performance tests were performed. The results are shown in Table 1.
[0140] Table 1
[0141]
[0142] As can be seen from Table 1, the lithium-ion battery using the separator-negative electrode composite sheet of the present invention can simultaneously improve the capacity density and the fast charging capacity, that is, it can simultaneously improve the endurance and the fast charging capacity. And from the comparison of Comparative Examples 1-6, it can be seen that only when Li 5.3 PS 4.3 ClBr 0.7 The solid electrolyte layer obtained in conjunction with LiPON can simultaneously improve the energy density and fast charging capability of lithium-ion batteries.
[0143] In addition, it can be seen from the comparison between Example 1 and Examples 6-7, Example 1 and Examples 9-10, and Example 1 and Examples 12-13 that the solid electrolyte Li 5.3 PS 4.3 ClBr 0.7 Optimizing the mass ratio with LiPON, the thickness of the solid electrolyte layer and the thickness of the base film can further improve both the battery life and the fast charging capability.
[0144] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0145] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A separator-negative electrode composite sheet, characterized in that: The separator-negative electrode composite sheet includes a separator and a negative electrode layer attached to one surface of the separator, wherein the separator includes a base film and a solid electrolyte layer coated on the surface of the base film, and the solid electrolyte in the solid electrolyte layer includes Li 5.3 PS 4.3 ClBr 0.7 and LiPON, wherein the material of the negative electrode layer is a conductive material.
2. The separator-negative electrode composite sheet according to claim 1, characterized in that: The solid electrolyte also satisfies at least one of the following conditions: (1) Li in the solid electrolyte 5.3 PS 4.3 ClBr 0.7 The mass ratio with LiPON is 90:10-55:45; (2) The mass fraction of the solid electrolyte in the solid electrolyte layer is 85%-98%.
3. The separator-negative electrode composite sheet according to claim 1, characterized in that: The solid electrolyte layer also satisfies at least one of the following conditions: (1) The particle size of the solid electrolyte is 2 μm-15 μm; (2) The thickness of the solid electrolyte layer is 1 μm-3 μm; (3) The porosity of the solid electrolyte layer is 20%-60%.
4. The separator-negative electrode composite sheet according to any one of claims 1 to 3, characterized in that: The base film satisfies at least one of the following conditions: (1) The thickness of the base film is 2 μm-6 μm; (2) The porosity of the base film is 30%-65%.
5. The separator-negative electrode composite sheet according to any one of claims 1 to 3, characterized in that: The negative electrode layer satisfies at least one of the following conditions: (1) The thickness of the negative electrode layer is 100 μm-200 μm; (2) The conductive material is selected from carbon materials; (3) The negative electrode layer has a mesoporous structure.
6. A method for preparing a separator-negative electrode composite sheet according to any one of claims 1 to 5, characterized in that: The following steps are involved: preparing a solid electrolyte into a slurry; Placing the slurry on the surface of the base film and drying to obtain a diaphragm; A negative electrode layer is formed on one surface of the separator.
7. The method for preparing a separator-negative electrode composite sheet according to claim 6, characterized in that: The negative electrode layer is deposited on one surface of the diaphragm by means of magnetic field sputtering.
8. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode sheet, a separator-negative electrode composite sheet as claimed in any one of claims 1 to 5, and an electrolyte.
9. The lithium-ion battery according to claim 8, characterized in that: The lithium-ion battery is a lithium iron phosphate battery or a ternary lithium battery.