Method for producing dispersion composition

By using a cooling liquid medium with high affinity to the raw material composition in the high-pressure pump, the problems of difficulty in reusing cooling water and deterioration of sealing members in non-aqueous dispersion compositions are solved, and the dispersibility and production of the dispersion composition are improved. sex.

CN118742379APending Publication Date: 2024-10-01아티엔스가부시키가이샤 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380017082.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-02
Filing Date
2023-02-01
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When producing a non-aqueous dispersion composition, mixing of cooling water from a high-pressure pump with the raw material composition makes it difficult to reuse the cooling water, and the high temperature causes deterioration of sealing members, reducing dispersion efficiency and productivity.

Method used

Use a liquid medium with 0 to 50 particles of 10 μm or more in the aggregation test as the cooling liquid medium to ensure high affinity between the raw material composition and the cooling liquid medium, prevent aggregation of the dispersoid and the dispersant, and extend the sealing member longevity and improved dispersion.

Benefits of technology

It effectively prevents the cooling efficiency from decreasing, prolongs the life of sealing components, improves the dispersibility and productivity of the dispersion composition, and reduces the leakage rate and pressure loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742379A_ABST
    Figure CN118742379A_ABST
Patent Text Reader

Abstract

Provided is a method for producing a dispersed composition using a dispersion device provided with: a dispersion mechanism for dispersing a raw material composition; a supply mechanism including a plunger part and supplying the raw material composition to the dispersion mechanism; and a cooling mechanism that cools the plunger section using a liquid medium for cooling, in which the raw material composition contains a non-aqueous dispersion medium and a dispersoid, and the liquid medium for cooling is a liquid medium in which the number of particles having a particle size of 10 [mu] m or more is 0-50 in the coagulation test described below. (Coagulation test): dispersing the same composition as the raw material composition using a bead mill or a high-pressure homogenizer, preparing a test dispersion having a particle size of less than 10 [mu] m using a grinding tester (0 [mu] m-100 [mu] m), mixing the test dispersion with a cooling liquid medium at 25 DEG C in a mass ratio of 1: 1 to prepare a test sample, and drying the test sample in a drying oven to obtain the test sample. And checking the number of particles of 10 [mu] m or more in the test sample using a grinding tester (0 [mu] m to 100 [mu] m).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a dispersion composition. Background Art

[0002] As a method for dispersing the dispersoid in a non-aqueous dispersion medium, there are stirrers, ball mill dispersers, bead mill dispersers, ultrasonic dispersers, uniaxial mixers, multiaxial mixers, roller mill dispersers, high-pressure homogenizers, etc. From the viewpoint of dispersion efficiency, bead mill dispersers are widely used. Although bead mills have the advantage of applying impact to the dispersoid to make the dispersoid micro-dispersed, they sometimes damage the dispersoid due to impact, thereby reducing the original characteristics of the dispersoid. The high-pressure homogenizer can utilize a method of spraying the treatment liquid from a nozzle or a method of passing the treatment liquid through a homogenizing valve, etc., to homogenize the treatment liquid. Since the treatment liquid is supplied with high pressure in order to improve the dispersion efficiency, the dispersoid can be micro-dispersed by the shear force and collision of the treatment liquids, the collision with the wall of the homogenizing valve, etc.

[0003] The valve-type high-pressure homogenizer can increase the flow rate of the treatment liquid, and thus does not require a nozzle that may cause clogging. Therefore, it is suitable for mass production and is used as a homogenizing device for water-based products such as dairy products and beverages. Since dairy products and the like have little solid content and are water-based, they have little effect on the components of the dispersion device. For example, they have the advantages of slow deterioration of gaskets of the high-pressure pump and a long replacement period. In addition, even if the gaskets of the high-pressure pump deteriorate and the treatment liquid leaks out, since it is a water-based treatment liquid, it can be recovered and easily processed. Since the high-pressure pump is loaded with high pressure and generates heat, there is a high-pressure pump that includes a cooling mechanism that utilizes cooling water. Even if the water-based treatment liquid leaks from the high-pressure pump, it will be recovered together with the cooling water, so there are fewer problems.

[0004] In recent years, high-pressure homogenizers have also been used as solvent-based dispersion devices for inks, etc., and in particular, as solvent-based dispersion devices for carbon materials including carbon nanotubes. Solvent-based processing liquids are prone to act on gaskets of high-pressure pumps, etc., and sometimes the gasket replacement period becomes shorter due to gasket deterioration, reducing operating efficiency. Furthermore, there is also a problem that the solvent leakage from the high-pressure pump is aggravated due to gasket deterioration.

[0005] Patent document 1 proposes the following: removing the organic solvent from a mixture of an organic solvent solution containing water and a polymer, dispersing the removed solvent, and producing an aqueous dispersion of pigment-containing polymer particles, thereby preventing the volatilization of the organic solvent during the decomposition and cleaning of the dispersion device while dispersing the solvent, thereby improving the operability and preventing the deterioration of the gasket of the dispersion device.

[0006] Patent document 2 proposes the following: in a method in which a coarse dispersion containing carbon nanotubes and a solvent is stored in a tank and transported to a disperser for dispersion treatment using a high-pressure pump, the high-temperature carbon nanotube dispersion discharged from the disperser is cooled to prevent the generation of bubbles in the dispersion, and the back pressure of the dispersion is reduced in multiple stages to prevent the generation of bubbles in the dispersion when it is released to atmospheric pressure, thereby improving the dispersibility of the carbon nanotubes.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2001-247810

[0010] Patent Document 2: International Publication No. 2015 / 015758 Summary of the invention

[0011] Problems to be solved by the invention

[0012] In the case of manufacturing a non-aqueous dispersion composition, if the cooling water for cooling the high-pressure pump is mixed with the raw material composition leaking from the high-pressure pump, the non-aqueous dispersion medium is mixed with the dispersoid into the discharge of the cooling water, and it is difficult to reuse the cooling water as water or to dispose of it as waste. If water is mixed into a system that maintains the dispersion stability of the dispersoid in the non-aqueous dispersion medium, the stability of the system sometimes collapses, and the dispersoid condenses to produce agglomerates. Since the dispersoid is also included in the leakage together with the non-aqueous dispersion medium, in order to reuse the cooling water, an additional process of removing the solid component by filtration or the like is set, but if agglomerates are produced, there is a problem that it is difficult to remove the solid component.

[0013] If the circulation efficiency of the recycled cooling water is reduced due to such an unfavorable situation, the cooling efficiency of the high-pressure pump may be reduced, and the components of the high-pressure pump may be exposed to high temperatures and deteriorate. For example, sealing components such as gaskets of the high-pressure pump may deteriorate due to high temperatures, causing pressure loss in the high-pressure pump. The deterioration of the gaskets may cause a decrease in operating efficiency, shorten replacement time, etc., and become the main cause of reduced productivity.

[0014] In Patent Document 1, the degradation of the gasket of the high-pressure homogenizer is prevented by removing the organic solvent contained in the aqueous dispersion of pigment-containing polymer particles in advance, but the problem of gasket degradation cannot be eliminated when the dispersion composition is a non-aqueous dispersion medium. In Patent Document 2, a coarse dispersion liquid is supplied to the high-pressure homogenizer by a high-pressure pump, but the focus is only on cooling the dispersion liquid after the dispersion treatment by the high-pressure homogenizer to prevent the generation of bubbles and improve the dispersibility, and the situation of reduced productivity due to the high temperature of the high-pressure pump is not studied.

[0015] The pressurizing mechanism of the high-pressure homogenizer uses a plunger to load pressure on the treatment liquid in the cylinder, and supplies the high-pressure treatment liquid to a dispersion part including a nozzle or a homogenizing valve, etc. Since friction heat is generated between the seal in the cylinder and the sliding surface of the plunger, there is a method of cooling the plunger to prevent the deterioration of the sealing member. Furthermore, since the plunger reciprocates in the cylinder, the treatment liquid is prone to leaking with the reciprocating movement of the plunger, and the above problem may occur when the treatment liquid is a non-aqueous dispersion medium.

[0016] An object of the present invention is to prevent a decrease in cooling efficiency of a plunger portion, to enhance dispersibility of a dispersion composition, and to improve productivity.

[0017] Technical means of solving problems

[0018] The inventors and others have made great efforts to study in order to solve the above-mentioned problems. According to the results, in the process of applying a cooling liquid medium to the plunger, the cooling liquid medium is a liquid medium in which the number of particles above 10 μm in a prescribed coagulation test is 0 to 50. In the manufacturing method of a dispersion composition comprising a non-aqueous dispersion medium, a liquid medium with high affinity for the raw material composition is selected as the cooling liquid medium for cooling the plunger. Even if the raw material composition leaks from the cylinder body and contacts the cooling liquid medium, the generation of agglomerates caused by dispersed substances, dispersants, etc. can be suppressed. Thus, when the cooling liquid medium is reused and circulated, the cooling efficiency is prevented from being reduced, for example, the deterioration of sealing components such as gaskets is prevented, the life of the sealing components is extended, and long-term operation can be achieved. In addition, the replacement period of the sealing components becomes longer, which can improve the workability. In addition, the pressure loss caused by the deterioration of the sealing components can be suppressed, so that the treatment liquid is supplied to the dispersion mechanism from the high-pressure pump at high pressure, and the dispersibility of the dispersion composition can be improved.

[0019] That is, the present invention includes the following embodiments. The embodiments of the present invention are not limited to the following.

[0020] <1> A method for producing a dispersed composition, using a dispersing device, the dispersing device comprising: a dispersing mechanism for dispersing a raw material composition; a supply mechanism including a plunger portion and supplying the raw material composition to the dispersing mechanism; and a cooling mechanism for cooling the plunger portion using a cooling liquid medium, wherein the raw material composition comprises a non-aqueous dispersion medium and a dispersoid, and the cooling liquid medium is a liquid medium having a particle number of 0 to 50 particles of 10 μm or more in the following agglomeration test,

[0021] (Agglomeration test)

[0022] The method comprises dispersing a composition identical to the raw material composition using a bead mill or a high-pressure homogenizer, preparing a test dispersion having a particle size of less than 10 μm using a grinding tester (0 μm to 100 μm), mixing the test dispersion with the cooling liquid medium at a mass ratio of 1:1 at 25° C. to prepare a test sample, and confirming the number of particles of 10 μm or more in the test sample using a grinding tester (0 μm to 100 μm).

[0023] <2> The method for producing a dispersed composition according to <1>, wherein the nonaqueous dispersion medium of the raw material composition and the cooling liquid medium comprise the same liquid medium.

[0024] <3> The method for producing a dispersed composition according to <1> or <2>, wherein the leakage rate of the raw material composition represented by the following formula (1) from the supply mechanism is 0.2% or less per 100 hours of operation time,

[0025] Leakage rate (%) = (leakage amount of raw material composition from the supply mechanism (L) / supply amount of raw material composition (L)) × 100 (1).

[0026] <4> A method for producing a dispersed composition, using a dispersing device, the dispersing device comprising: a dispersing mechanism for dispersing a raw material composition; a supply mechanism comprising a plunger portion and supplying the raw material composition to the dispersing mechanism; and a cooling mechanism for cooling the plunger portion using a cooling liquid medium, wherein the raw material composition comprises a dispersoid, a non-aqueous dispersion medium and a dispersant, and the cooling liquid medium is a liquid medium that does not produce solid precipitates at 25°C in a state where a solution of the non-aqueous dispersion medium containing 5% by mass of the dispersant and the cooling liquid medium are mixed in a mass ratio of 1:1.

[0027] <5> A method for producing a dispersed composition, using a dispersing device, the dispersing device comprising: a dispersing mechanism for dispersing a raw material composition; a supply mechanism including a plunger portion and supplying the raw material composition to the dispersing mechanism; and a cooling mechanism for cooling the plunger portion using a cooling liquid medium, wherein the raw material composition comprises a dispersoid, a non-aqueous dispersion medium and a dispersant, and at 25°C, the cooling liquid medium is a liquid medium that dissolves 0.1% by mass or more of the dispersant contained in the raw material composition.

[0028] Effects of the Invention

[0029] According to one embodiment of the present invention, it is possible to prevent a decrease in the cooling efficiency of the plunger portion, enhance the dispersibility of the dispersion composition, and improve productivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] [Figure 1 ] is a schematic diagram showing an example of a dispersion device.

[0031] [ Figure 2 ] is a cross-sectional view schematically showing an example of a high-pressure pump and a cooling mechanism of a dispersion device.

[0032] [ Figure 3 ] is a cross-sectional view schematically showing a homogenizing valve in a dispersing portion of an example of a dispersing device. DETAILED DESCRIPTION

[0033] Hereinafter, a method for producing a dispersion composition which is an embodiment of the present invention will be described in detail. The present invention is not limited to the following embodiments, and the present invention also includes embodiments that can be implemented within the scope of the present invention.

[0034] <Dispersion device>

[0035] Hereinafter, a method for manufacturing a dispersion composition comprising a dispersant and a non-aqueous dispersion medium using a dispersion device is described. The non-aqueous dispersion medium may also contain a dispersant. The dispersion composition can be manufactured using a dispersion device, the dispersion device comprising: a dispersion mechanism for dispersing a raw material composition; a supply mechanism, comprising a plunger portion and supplying the raw material composition to the dispersion mechanism; and a cooling mechanism, using a cooling liquid medium to cool the plunger portion. The raw material composition is a composition in which raw materials containing the dispersion composition are mixed. The raw material composition may be a composition in a mixed state or a composition in a state of rough dispersion after mixing. As an example of such a dispersion device, a high-pressure homogenizer can be cited. The high-pressure homogenizer can supply the raw material composition from a high-pressure pump to the dispersion section at high pressure through the reciprocating movement of the plunger, and disperse the raw material composition in the dispersion section. In an example of the dispersion section, the raw material composition can be ejected at high pressure from a tiny opening at the front end of the nozzle, and the dispersant is dispersed in the non-aqueous dispersion medium through collision and shearing force between the raw material compositions. In other examples of the dispersion section, the raw material composition can be supplied to the homogenization valve at high pressure, so that the raw material composition collides with the wall of the homogenization valve and applies an impact, so that the dispersoid is dispersed in the non-aqueous dispersion medium. The method of using a homogenization valve for dispersion treatment can increase the flow rate of the raw material composition, avoid undesirable conditions such as nozzle clogging, and is suitable for mass production. The pressure of the raw material composition when supplied to the dispersion section is preferably 10MPa~150MPa. In the case where the dispersion section is a nozzle type, the pressure of the raw material composition when supplied to the dispersion section is preferably 60MPa~150MPa in the usual range, more preferably 80MPa~150MPa, and further preferably 100MPa~150MPa. In the case where the dispersion section is a valve type, the pressure of the raw material composition when supplied to the dispersion section is preferably 10MPa~150MPa in the usual range, more preferably 40MPa~150MPa, and further preferably 80MPa~150MPa. Furthermore, from the viewpoint of dispersion efficiency, a valve type homogenizer and a nozzle type homogenizer may be used together for dispersion, and from the viewpoint of adjustment of the dispersion state, a bead mill or a high shear mixer other than a high pressure homogenizer may be used together for dispersion.

[0036] Figure 1A schematic diagram showing an example of a dispersion device. The dispersion device 100 includes: a plunger 10, a high-pressure pump 20, a dispersion unit 30, and a cooling mechanism 40. The raw material composition tank 50 is a container for accommodating the raw material composition supplied to the high-pressure pump 20. The high-pressure pump 20 includes a supply port 22 for supplying the raw material composition from the raw material composition tank 50, and a discharge port 23 for discharging the raw material composition to the dispersion unit 30. The high-pressure pump 20 includes a cylinder body 21, which supports the plunger 10 so that it can reciprocate in the axial direction. In the cylinder body 21, a sealing mechanism can be provided to prevent the raw material composition and pressure from leaking out of the high-pressure pump 20 to the outside. The sealing mechanism can be listed as a sealing member configured throughout the entire circumference of the inner periphery of the cylinder body 21. A gland packing as an example of a sealing member is composed of polyaramid fiber, polytetrafluoroethylene (PTFE) fiber, organic fiber such as carbon fiber, inorganic fiber such as carbon fiber, metal fiber, natural fiber such as ramie fiber, or a combination thereof.

[0037] One end of the plunger 10 is inserted into the high-pressure pump 20, and the other end extends to the outside of the high-pressure pump 20 and is supported by the cylinder 21. The sliding surface between the plunger 10 and the cylinder 21 is preferably sealed so as to prevent the raw material composition from leaking from the high-pressure pump 20, and preferably does not cause pressure loss due to the outflow of air from the high-pressure pump 20 to the outside. The plunger 10 changes the volume of the pressure chamber of the high-pressure pump 20 by reciprocating in the axial direction. When the plunger 10 is pulled out of the high-pressure pump 20 and the volume of the pressure chamber increases, the raw material composition is sucked from the supply port 22 of the high-pressure pump 20. When the plunger 10 is pushed out of the high-pressure pump 20 and the volume of the pressure chamber decreases, the raw material composition is ejected from the discharge port 23 of the high-pressure pump 20. In order to prevent the backflow of the raw material composition, valves may be provided at the supply port 22 and the discharge port 23 of the high-pressure pump 20, respectively.

[0038] The raw material composition discharged from the high-pressure pump 20 is supplied to the dispersion unit 30 at high pressure. The dispersion unit 30 may be a nozzle type or a valve type. Since a large amount of raw material composition can be supplied to the dispersion unit 30 at high pressure using the plunger 10, the dispersion unit 30 is preferably a valve type, and more specifically, a homogenizing valve. After the dispersion treatment, a dispersion composition in which a dispersoid is dispersed in a non-aqueous dispersion medium is obtained. Although not shown in the figure, the dispersion composition after the dispersion treatment can be recovered from the discharge port of the dispersion unit 30 through a pipe to the dispersion composition tank.

[0039] The cooling mechanism 40 includes a cooling liquid medium tank 41 and a cooling part 42. The cooling mechanism 40 includes a pipe 40a for supplying a liquid medium from the cooling liquid medium tank 41 to the cooling part 42, and a pipe 40b for discharging the liquid medium from the cooling part 42. The pipe 40b is connected to the recovery container 43, and the used liquid medium can be recovered in the recovery container 43. In other examples, the liquid medium recovered to the recovery container 43 can also be filtered, and the liquid medium from which the solid components are removed can be recycled to the cooling liquid medium tank 41 through the pipe 40c for reuse. The cooling part 42 is a member for cooling the plunger 10 extending from the high-pressure pump 20 to the outside. The cooling part 42 is, for example, a member that surrounds the outer periphery of the plunger 10 extending to the outside of the high-pressure pump 20 and covers the opening of the cylinder part 21 in a liquid-tight manner. By filling the cooling liquid medium inside the cooling part 42, the cooling liquid medium is directly in contact with the plunger 10 and the opening of the cylinder part 21 to cool. The outer peripheral surface of the plunger 10 is cooled, and the plunger 10 continues to reciprocate, so that the outer peripheral surface of the plunger 10 that is cooled enters the interior of the cylinder body 21 of the high-pressure pump 20, and can be cooled to the interior of the cylinder body 21. In this way, the sealing components such as the gland gasket arranged on the inner peripheral surface of the cylinder body 21 can be cooled. The cooling liquid medium is supplied from the cooling liquid medium tank 41 to the cooling part 42 through the pipe 40a, and the cooling liquid medium is discharged from the cooling part 42 to the recovery container 43 through the pipe 40b. Although not shown in the figure, the pipe 40b from the cooling part 42 to the recovery container 43 may not be provided, and the cooling liquid medium discharged from the cooling part 42 may be directly dropped into the recovery container 43 or a tray, etc. for recovery. In addition, the recovery container 43 may not be provided, and the cooling liquid medium discharged from the cooling part 42 may be directly returned to the cooling liquid medium tank 41.

[0040] As another example of the cooling mechanism, although not shown in the figure, a supply port for the cooling liquid medium may be provided on the upper part of the plunger extending from the high-pressure pump, and the cooling liquid medium may be directly dripped onto the plunger for cooling. In the above case, the cooling liquid medium that falls after being dripped onto the plunger may be recovered by a recovery container or a tray.

[0041] As another example of the cooling mechanism, although not shown in the figure, a cooling pipe for a cooling liquid medium may also be arranged inside the cylinder body. The cooling liquid medium is supplied to the cooling pipe, and the inside of the cylinder body is cooled by the cooling pipe, so that the sealing member arranged on the inner peripheral surface of the cylinder body and the plunger that slides relatively therewith can be cooled. The cooling liquid medium of the cooling pipe supplied to the inside of the cylinder body is discharged from the opening of the cylinder body. For example, the cooling liquid medium discharged from the cooling pipe can be discharged to the cooling part 42, or it can be recovered to the recovery container 43 through another pipe, or it can be directly dropped into the recovery container 43 or the tray and recovered. In the method of any cooling mechanism, since the cooling liquid medium is in direct contact with the plunger, if the raw material composition leaks from the high-pressure pump via the cylinder body, the raw material composition may also be in contact with the cooling liquid medium.

[0042] use Figure 2 and Figure 3 A specific example of a dispersing device is described below. Figure 1 The same symbols are given to the common components, and the parts not specially described are as described Figure 1 As described in . Figure 2 FIG. 2 is a cross-sectional view schematically showing the high-pressure pump 20 and the cooling mechanism 40 of the dispersion device. Figure 2 In the figure, the high-pressure pump 20 includes a cylinder body 21, a gland gasket 24 arranged on the inner circumferential surface of the cylinder body 21, and a ball valve 22' and a ball valve 23' respectively arranged at the supply port 22 and the discharge port 23. The cooling mechanism 40 includes a cooling liquid medium tank 41, a cooling part 42, a pump 44 and a heat exchanger 45. The plunger 10 can move back and forth and is supported by the gland gasket 24 in a liquid-tight manner in the cylinder body 21 so as to be able to slide. Through the reciprocating movement of the plunger 10, the raw material composition is supplied to the high-pressure pump 20 in the direction of the arrow in the figure and discharged. In the cooling mechanism 40, the cooling liquid medium is fed from the cooling liquid medium tank 41 through the pump 44 in the direction of the arrow in the figure and filled into the cooling part 42, and then the cooled and heated cooling liquid medium is discharged from the upper part of the cooling part 42, fed and circulated to the cooling liquid medium tank 41. A heat exchanger 45 may be provided between the pipes from the cooling unit 42 to the cooling liquid medium tank 41 to cool the heated cooling liquid medium and then circulate it.

[0043] Figure 3 FIG. 3 is a cross-sectional view schematically showing a homogenizing valve of the dispersion unit 30. Figure 3 In the figure, the homogenizing valve of the dispersion part 30 includes a valve seat 31, an impact ring 32 and a homogenizing valve 33. The raw material composition supplied from the high-pressure pump 20 is supplied to the homogenizing valve at high pressure in the direction of the arrow in the figure and is finely dispersed, and then discharged from the discharge port, although not shown.

[0044] As an example of a dispersing device, a valve-type high-pressure homogenizer can use the "HC3 Series" manufactured by Sanmaru Machinery Industry, the "HV-H Series" manufactured by Izumi Food Machinery, and the "R-Model" manufactured by SPX flow. As another example of a dispersing device, a nozzle-type high-pressure homogenizer can be used. As a nozzle-type high-pressure homogenizer, the "Genus PY" manufactured by Genus, the "Star Burst" manufactured by Sugino Machine, and the "Nanomizer" manufactured by Nanomizer can be used, but it is not limited to these. The nozzle-type high-pressure homogenizer includes a pump and one or more nozzles, and there are many shapes of nozzles used for dispersing treatment. For example, there are types in which raw materials are made to collide with each other under high pressure, types in which high-pressure raw materials are made to collide with ceramic balls or pass through slits and are processed using their shearing force, types in which cavitation caused by the jet flow of high-pressure raw materials is used, etc., but the present invention is not limited to these.

[0045] <Agglomeration test>

[0046] In the manufacture of a dispersion composition containing a non-aqueous dispersion medium, if leakage of the raw material composition occurs when the cooling liquid medium is water, the stability of the system of the dispersed substance of the raw material composition and the non-aqueous dispersion medium sometimes collapses due to mixing with water, and the dispersed substance condenses to produce condensates. Furthermore, when the dispersed substance and the dispersant are included in the raw material composition, the stability of the system is easily collapsed by water, and condensates are more likely to be produced. The condensates are accumulated and blocked in the pipe or tank for discharging the cooling liquid medium, so the cooling efficiency of the plunger is reduced, and the plunger and the components around it are exposed to high temperatures, especially sometimes causing the deterioration of sealing components such as gland gaskets. Sometimes pressure loss is generated due to the deterioration of the sealing component, and the pressure load based on the plunger is reduced, the pressure of the raw material composition supplied to the dispersion part is reduced, and the dispersibility is reduced. In addition, the replacement operation of the sealing component is carried out after stopping the operation of the dispersion device and discharging the raw material composition, so the operation time becomes longer, which becomes the main reason for the reduction in productivity. In particular, the gland gasket is expensive, so if it is replaced frequently, it will lead to a reduction in production efficiency.

[0047] Therefore, the cooling liquid medium is preferably a liquid medium in which the number of particles of 10 μm or more is 0 to 50 in the following aggregation test.

[0048] (Agglomeration test)

[0049] The method comprises dispersing a composition identical to the raw material composition using a bead mill or a high-pressure homogenizer, preparing a test dispersion having a particle size of less than 10 μm using a grinding tester (0 μm to 100 μm), mixing the test dispersion with the cooling liquid medium at a mass ratio of 1:1 at 25° C. to prepare a test sample, and confirming the number of particles of 10 μm or more in the test sample using a grinding tester (0 μm to 100 μm).

[0050] The number of particles of 10 μm or more in the cooling liquid medium in the condensation test is preferably 50 or less, more preferably 30 or less, further preferably 10 or less, further more preferably 3 or less. More preferably, the number of particles of 10 μm or more in the cooling liquid medium in the condensation test is preferably 0, that is, no particles of 10 μm or more are observed. By satisfying the above conditions, even if the raw material composition leaks from the supply mechanism during the operation of the dispersion device and the raw material composition contacts the cooling liquid medium, the generation of condensates in the discharge piping, recovery container, etc. of the cooling liquid medium can be prevented.

[0051] Regarding the test dispersion, a composition identical to the raw material composition is dispersed and dispersed using a grinding tester (0 μm to 100 μm) until the particle size is less than 10 μm. The conditions for the dispersion vary depending on the type of the raw material composition, but by dispersing the raw material composition, as a result, it is sufficient to disperse the composition using a grinding tester until the particle size is less than 10 μm. For example, for a raw material composition with low cohesion, it can be prepared by coarse dispersion using a bead mill, and for a raw material composition with high cohesion, a high-pressure homogenizer can be used for fine dispersion. The particle size of the test dispersion is measured using a grinding tester with a groove depth of 0 μm to 100 μm and a scale interval of 10 μm.

[0052] The test sample is prepared by mixing the test sample with the cooling liquid medium at a mass ratio of 1:1 at 25°C. As for the mixing method, it is sufficient to mix the test sample with the cooling liquid medium as a whole, and a stirring device can be used for mixing. As for the stirring device, a self-rotating revolution stirring device can be used in terms of being able to degas the bubbles generated during mixing. For example, a self-rotating revolution stirring device can be used to stir at 2000 rpm for 30 seconds. The number of particles larger than 10 μm of the obtained test sample is confirmed using a grinding tester (0 μm to 100 μm) at 25°C. When confirming the number of particles larger than 10 μm of the test sample, a grinding tester with a groove depth of 0 μm to 100 μm and a scale interval of 10 μm is used. After the test sample is prepared, the number of particles larger than 10 μm is measured using a grinding tester within 60 seconds. The coagulation test is performed under the conditions of 25°C and 1 atmosphere.

[0053] The cooling liquid medium may be a single-component liquid or a cooling liquid medium composed of two or more liquids. In the case of a cooling liquid medium composed of two or more liquids, a cooling liquid medium in which two or more liquids are mixed at the same mass ratio as the cooling liquid medium used in the dispersion device is used as the cooling liquid medium used in the coagulation test.

[0054] As long as the cooling liquid medium satisfies the coagulation test, its type is not particularly limited, and is preferably a non-aqueous liquid medium, and more preferably an organic solvent. Specifically, it can be selected from the organic solvent used for the raw material composition described below for use. The cooling liquid medium is preferably a liquid medium that is not based on water as the main component, and specifically, it is preferably a ratio of water less than 50% by mass. The cooling liquid medium is more preferably a ratio of water of 10% by mass or less, and further preferably 1% by mass or less, and further more preferably substantially free of water. By selecting a non-aqueous liquid medium with high affinity for the raw material composition instead of previously widely used water as the cooling liquid medium for cooling the plunger portion, even if the raw material composition leaks from the cylinder portion and contacts with the cooling liquid medium, the generation of condensates caused by dispersed substances, dispersants, etc. can also be suppressed.

[0055] The cooling liquid medium only needs to satisfy the coagulation test, and preferably satisfies the following conditions on the basis of satisfying the coagulation test. The cooling liquid medium is preferably the same as the non-aqueous dispersion medium of the raw material composition. For example, in the case where the raw material composition comprises a single-component non-aqueous dispersion medium, it is preferred to use the non-aqueous dispersion medium as the cooling liquid medium. In the case where the raw material composition comprises a plurality of non-aqueous dispersion media, as the cooling liquid medium, a single component of the plurality of non-aqueous media of the raw material composition can be used, or two or more components can be used in combination, or all components can be used in combination. In the case of using all components, the blending ratio of each component may be the same as or different from the non-aqueous dispersion medium of the raw material composition. Preferably, in the case where the raw material composition comprises a plurality of non-aqueous dispersion media, the cooling liquid medium is a liquid medium comprising a plurality of non-aqueous dispersion media of the raw material composition in the same blending ratio.

[0056] In the method of one embodiment, it is preferred that the leakage rate of the raw material composition represented by the following formula (1) from the supply mechanism is 0.2% or less per 100 hours of operation time.

[0057] Leakage rate (%) = (amount of raw material composition leaking from the supply mechanism (L) / amount of raw material composition supplied (L)) × 100 (1)

[0058] In formula (1), the leakage amount of the raw material composition from the supply mechanism is the amount of the raw material composition leaking from the supply mechanism to the cooling mechanism during the 100-hour operation period, and the supply amount of the raw material composition is the total amount discharged from the dispersion unit during the 100-hour operation period. The leakage amount of the raw material composition from the supply mechanism is calculated according to the following procedure.

[0059] (1) When replacing the gland gasket, the cooling liquid medium is also replaced. The cooling liquid medium at this time is referred to as X(L).

[0060] (2) The liquid recovered in the cooling liquid medium tank when the total operation time reaches 100 hours is defined as Y(L). The leakage amount of the raw material composition from the supply mechanism is calculated according to the following formula.

[0061] The amount of raw material composition leaking from the supply mechanism (L) = Y (L) - X (L)

[0062] From the viewpoint of the production efficiency of the dispersed composition using the dispersing device, the replacement frequency of the gland gasket of the dispersing device is preferably once per month or less. As the operating time of the dispersing device, the life of the gland gasket is expected to be more than several hundred hours, and the leakage of the raw material composition from the supply mechanism in the initial to middle stage of the replacement interval, that is, every 100 hours of operating time, is an important indicator in estimating the life of the gland gasket. By not confirming that the sealing component begins to deteriorate during the 100-hour operating time, it can be predicted that the raw material composition will be prevented from leaking from the supply mechanism during the subsequent operation. Therefore, by the leakage rate of less than 0.2% per 100 hours of operating time, it can be confirmed that the cooling efficiency of the plunger part is well performed, and it can be predicted that the degradation of the gland gasket will be further prevented in the subsequent operation.

[0063] The leakage rate represented by formula (1) is preferably 0.2% or less, more preferably 0.1% or less, and further preferably 0.05% or less. If the deterioration of the sealing member is prevented and the airtightness of the sliding surface between the cylinder portion and the plunger of the high-pressure pump is further ensured, the leakage rate represented by formula (1) is preferably close to 0%.

[0064] <Raw material composition>

[0065] The raw material composition supplied to the dispersing device is not particularly limited as long as it includes a dispersoid and a non-aqueous dispersion medium. In order to obtain the dispersion stability of the dispersoid, the raw material composition may also include a dispersant. The raw material composition may also include any components such as a resin emulsion, a surfactant, an adhesive resin, a wetting agent, a wetting penetrant, and a leveling agent as needed.

[0066] The dispersoid may be a combination of inorganic particles, organic particles, inorganic-organic composite particles, etc., preferably particles that can be dispersed in a non-aqueous dispersion medium, preferably a substance that is insoluble in a non-aqueous dispersion medium. As inorganic particles, for example, carbon materials, ceramics, metals, etc. may be mentioned. As carbon materials, carbon materials such as carbon black, carbon nanotubes, fullerenes, graphene, multilayer graphene, and graphite may be mentioned. As carbon black, for example, acetylene black, furnace black, hollow carbon black, Ketjen black, etc. may be mentioned. These carbon materials may be any one of neutral, acidic, and alkaline, and may also be oxidized or graphitized. Examples of ceramics include metal oxides, carbonates, nitrides, phosphates, carbides, and the like, such as calcium oxide, calcium carbonate, magnesium oxide, magnesium carbonate, magnesium phosphate, aluminum oxide, aluminum nitride, aluminum phosphate, boron nitride, silicon oxide, silicon nitride, silicon carbide, zirconium oxide, titanium oxide, kaolin clay, indium tin oxide (ITO), and the like. Examples of metals include zinc, lead, titanium, cadmium, iron, copper, cobalt, and the like, or alloys thereof.

[0067] As the organic particles, resin particles are preferred, and examples thereof include polystyrene, polyurethane, polyester, polyamide, vinyl polymers, acrylic polymers, and composite polymers thereof; cellulose, pulp fibers, and the like.

[0068] As the dispersant, an inorganic pigment or an organic pigment may also be used. Examples of organic pigments include azo, phthalocyanine, anthraquinone, perylene, perinone, quinacridone, thioindigo, dioxazine, isoindolinone, quinophthalone, azomethine azo, diketopyrrolopyrrole, and isoindolinone pigments. More specifically, examples include carmine 6B, lake red C, permanent red 2B, disazoyellow, pyrazolone orange, carmine FB, cromophtal yellow, cromophtal red, phthalocyanine blue, phthalocyanine green, dioxazine violet, quinacridone magenta, quinacridone red, indanthrone blue, pyrimidine yellow, thioindigo bordeaux, thioindigo magenta, perylene red, perinone orange, isoindolinone yellow, diketopyrrolopyrrole red, aniline black, and daylight fluorescent pigments. Furthermore, examples of organic pigments include CI pigment black, CI pigment blue, CI pigment green, CI pigment red, CI pigment violet, CI pigment yellow, CI pigment orange, CI pigment brown, etc., which are organic compounds or organometallic complexes among colorants listed in the Pigment Index (Colour Index International, abbreviated as CI).

[0069] Examples of the inorganic pigment include white pigments such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, and silicon dioxide; and pigments other than white pigments such as aluminum powder, mica, bronze powder, chrome vermilion, chrome yellow, cadmium yellow, cadmium red, aluminum hydroxide, ultramarine, dark blue, iron oxide (bengala), yellow iron oxide, black iron, titanium oxide, and zinc oxide.

[0070] The dispersoid may also be surface treated. The dispersoid may be used alone or in combination of two or more. The content of the dispersoid in the raw material composition is not particularly limited as long as it is appropriately adjusted according to the materials of the non-aqueous dispersion medium and the dispersoid within the range in which the dispersoid can be dispersed in the non-aqueous dispersion medium after the dispersion treatment.

[0071] As the non-aqueous dispersion medium, as long as a solvent capable of dispersing the dispersoid is used according to the type of the dispersoid, an organic solvent is preferred. As the organic solvent, any one of a non-polar solvent and a polar solvent may be used, and these combinations may also be used within the range that they can be mixed. As the non-polar solvent, aliphatic hydrocarbon solvents such as hexane, cyclohexane, and paraffin, aromatic hydrocarbon solvents such as benzene, toluene, and xylene, and other petroleum hydrocarbon solvents may be listed. As the polar solvent, ester solvents, ether solvents, alcohol solvents, ketone solvents, amide solvents, heterocyclic solvents, sulfoxide solvents, sulfone solvents, carbonate solvents, etc. may be listed.

[0072] More specifically, as the non-aqueous dispersion medium, amides (N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone (NEP), N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N-methylcaprolactam, etc.), heterocyclics (cyclohexylpyrrolidone, 2-oxazolidinone, 1,3-dimethyl-2-imidazolidinone, γ-butyrolactone, etc.), sulfoxides (dimethyl sulfoxide, etc.), sulfones (hexamethylphosphonic triamide, cyclopentane sulfone, etc.), lower ketones (acetone, methyl ethyl ketone, etc.), carbonates (diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, fluoroethylene carbonate, propylene carbonate, ethylene carbonate), tetrahydrofuran, acetonitrile, etc. can be used.

[0073] Examples of the non-aqueous dispersion medium include formic acid, acetic acid, methanol, ethanol, propanol, methyl acetate, ethyl acetate, diethyl ether, α-terpineol, etc. The non-aqueous dispersion medium may be used alone or in combination of two or more.

[0074] As the dispersant, any of a resin-type dispersant and a surfactant may be used, and a preferred type of dispersant may be appropriately used in a preferred blending amount according to the properties required for the dispersion of the dispersoid.

[0075] As the resin type dispersant, (meth) acrylic acid polymers, polymers derived from ethylenically unsaturated hydrocarbons, cellulose derivatives, copolymers thereof, etc. can be used. As polymers derived from ethylenically unsaturated hydrocarbons, polyvinyl alcohol resins, polyvinyl pyrrolidone resins, polyacrylonitrile resins, nitrile rubbers, etc. can be cited. As the polyvinyl alcohol resins, polyvinyl alcohol, modified polyvinyl alcohol having functional groups other than hydroxyl groups (e.g., acetyl, sulfonic, carboxyl, carbonyl, amino), polyvinyl alcohol modified with various salts, polyvinyl alcohol modified with other anions or cations, polyvinyl alcohol acetals modified with aldehydes (acetal modified or butyral modified, etc.) (polyvinyl alcohol acetoacetal, polyvinyl alcohol butyral, etc.) can be cited. As polyacrylonitrile resin, it can be a homopolymer of polyacrylonitrile, a copolymer of polyacrylonitrile, a modified body thereof, etc., preferably a polyacrylonitrile resin having at least one selected from the group consisting of hydroxyl, carboxyl, primary amino, secondary amino, and mercapto groups, basic groups, (meth) acrylic acid alkyl esters or α-olefins, etc. and introduced alkyl groups, etc. For example, the acrylonitrile copolymers described in Japanese Patent Laid-Open No. 2020-163362 can be used. As nitrile rubbers, acrylonitrile butadiene rubber, hydrogenated acrylonitrile butadiene rubber, etc. can be listed. As cellulose derivatives, cellulose acetate, cellulose acetate butyrate, cellulose butyrate, cyanoethyl cellulose, ethyl hydroxyethyl cellulose, nitrocellulose, methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, etc., or copolymers thereof, etc. In addition, the dispersants recorded in International Publication No. 2008 / 108360 Handbook, Japanese Patent Unexamined Publication No. 2018-192379, Japanese Patent Unexamined Publication No. 2019-087304, Japanese Patent No. 6524479, and Japanese Patent Unexamined Publication No. 2009-026744 can also be used, but are not limited to these dispersants. Particularly preferably, methylcellulose, ethylcellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, homopolymers of polyacrylonitrile, copolymers of polyacrylonitrile, hydrogenated acrylonitrile butadiene rubber are preferred. Polymers into which other substituents are introduced in a part of these polymers, modified polymers, etc. can also be used.

[0076] The surfactant may be any of anionic, cationic, amphoteric ionic surfactants and nonionic surfactants. The dispersant is preferably 5 to 300 parts by mass, more preferably 10 to 200 parts by mass, and further preferably 15 to 100 parts by mass, relative to 100 parts by mass of the dispersed substance.

[0077] The content of the dispersoid relative to the total amount of the raw material composition varies depending on the specific gravity of the dispersoid, but is preferably 0.1% to 80% by mass, more preferably 0.5% to 60% by mass, and further preferably 0.7% to 50% by mass. The solid content of the raw material composition is preferably 0.5% to 80% by mass, more preferably 0.7% to 60% by mass, and further preferably 1% to 50% by mass.

[0078] <Raw material composition containing carbon nanotubes>

[0079] The dispersing device of one embodiment can be dispersed by high pressure treatment without applying mechanical impact to the particles, and is therefore suitable for maintaining the shape of the particles for dispersion. Furthermore, it is suitable for improving the dispersibility of bulk materials by defibration as fibrous particles. For example, it can be preferably used in a method for producing a carbon nanotube dispersion. Hereinafter, carbon nanotubes are also recorded as CNTs.

[0080] In the raw material composition containing carbon nanotubes, the non-aqueous dispersion medium can use the non-aqueous dispersion medium. In the raw material composition containing carbon nanotubes, the non-aqueous dispersion medium preferably contains an aprotic solvent and a non-polar solvent, more preferably contains an aprotic solvent, and further preferably contains an aprotic polar solvent. The aprotic polar solvent can further prevent the aggregation of carbon nanotubes, and the solubility of the resin-type dispersant suitable for the dispersion of carbon nanotubes is also excellent. Among them, it is preferred to contain an amide solvent, specifically, it is more preferred to contain at least one selected from the group consisting of N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone and 1-n-octyl-2-pyrrolidone.

[0081] In the state before being dispersed in the raw material composition, the carbon nanotube preferably has the following characteristics. CNT is a shape in which planar graphite is wound into a cylindrical shape, and includes single-layer CNT and multi-layer CNT, which can be mixed. Single-layer CNT has a structure in which a layer of graphite is wound. Multi-layer CNT has a structure in which two or more layers of graphite are wound. In addition, the side wall of CNT may not be a graphite structure. In addition, for example, CNT including a side wall having an amorphous structure is also CNT in this specification.

[0082] The shape of CNT is not limited. As the shape, various shapes including needle-shaped, cylindrical tube-shaped, herringbone-shaped (fishbone type or cup stacking type), playing card-shaped (platelet) and coil-shaped can be listed. Among them, the shape of CNT is preferably needle-shaped or cylindrical tube-shaped. CNT can be a single shape or a combination of two or more shapes.

[0083] Examples of CNT forms include graphite whiskers, filamentous carbon, graphite fibers, ultrafine carbon tubes, carbon tubes, carbon fibrils, carbon microtubes, and carbon nanofibers. Carbon nanotubes may have any of these forms alone or in combination of two or more.

[0084] The average outer diameter of CNT is preferably 1 nm or more, more preferably 1.2 nm or more. In addition, it is preferably 30 nm or less, more preferably 20 nm or less, and further preferably 15 nm or less. In addition, the average outer diameter of CNT can be calculated as follows: First, the CNT is observed and photographed using a transmission electron microscope, and in the observation photograph, 300 CNTs are randomly selected and their outer diameters are measured and averaged.

[0085] The average fiber length of CNT is preferably 0.5 μm or more, more preferably 0.8 μm or more, and further preferably 1.0 μm or more. In addition, it is preferably 20 μm or less, and more preferably 10 μm or less. In addition, the average fiber length of CNT can be calculated as follows: First, the CNT is observed and photographed using a scanning electron microscope, and in the observation photograph, 300 CNTs are selected at random and their fiber lengths are measured and averaged.

[0086] The value obtained by dividing the fiber length of CNT by the outer diameter is the aspect ratio. Using the value of the average fiber length and the average outer diameter, a representative aspect ratio can be obtained. The higher the aspect ratio of the conductive material, the higher the conductivity can be obtained when forming an electrode. The aspect ratio of CNT is preferably 30 or more, more preferably 50 or more, and more preferably 80 or more. In addition, it is preferably 100,000 or less, more preferably 30,000 or less, and more preferably 10,000 or less.

[0087] The specific surface area of ​​CNT is preferably 100 m 2 / g or more, more preferably 150m 2 / g or more, more preferably 200m 2 / g or more. In addition, preferably 1200m 2 / g or less, more preferably 1000m 2 The specific surface area of ​​CNT is calculated by the Brunauer-Emmett-Teller (BET) method based on nitrogen adsorption measurement.

[0088] The carbon nanotubes may be surface-treated carbon nanotubes, carbon nanotube derivatives to which functional groups represented by carboxyl groups are added, or carbon nanotubes containing organic compounds, metal atoms, or substances represented by fullerenes may be used.

[0089] The raw material composition containing carbon nanotubes may contain a dispersant, and as the dispersant, the above-mentioned dispersant may be used. In order to further improve the dispersion stability of the carbon nanotubes in the non-aqueous dispersion medium, it is preferred to use a resin-type dispersant. Particularly preferred are methyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, homopolymers of polyacrylonitrile, copolymers of polyacrylonitrile, and hydrogenated acrylonitrile butadiene rubber. The raw material composition containing carbon nanotubes may also contain any component such as the above-mentioned binder resin.

[0090] The content of carbon nanotubes is preferably 0.1% to 20% by mass, more preferably 0.5% to 15% by mass, and further preferably 0.7% to 10% by mass, relative to the total amount of the raw material composition. The dispersant is preferably 5.0 parts by mass to 300 parts by mass in terms of mass ratio relative to the carbon nanotubes. The solid content of the raw material composition containing carbon nanotubes is preferably 0.5% to 50% by mass, more preferably 0.7% to 30% by mass, and further preferably 1% to 20% by mass.

[0091] <Other embodiments>

[0092] Hereinafter, another embodiment of the method for producing a dispersion composition comprising a dispersoid, a non-aqueous dispersion medium and a dispersant using a dispersing device is described. In the method, the raw material composition comprises a dispersoid, a non-aqueous dispersion medium and a dispersant, and the dispersion composition can be obtained by supplying the raw material composition from a supply mechanism to a dispersing mechanism and performing a dispersion treatment. The dispersing device for producing the dispersion composition can use the device.

[0093] In the dispersion composition in which the dispersant is dispersed in the non-aqueous dispersion medium, the dispersant preferably shows solubility in the non-aqueous dispersion medium and has the characteristic of being adsorbed on the dispersant in the non-aqueous dispersion medium. In such a dispersion composition, for the purpose of dispersion stability, the respective types of the non-aqueous dispersion medium, the dispersant, and the dispersant are appropriately selected. On the other hand, when the dispersion composition is added to other solvents such as water, due to factors such as the low solubility of the dispersant in other solvents, the dispersant sometimes detaches from the dispersant, and the dispersion stability is reduced and the dispersant is easily condensed.

[0094] Therefore, the cooling liquid medium is preferably a liquid medium that does not produce solid precipitates at 25°C in a state where a solution of a non-aqueous dispersion medium containing 5% by mass of a dispersant and a cooling liquid medium are mixed in a mass ratio of 1:1. As a specific judgment criterion, at 25°C and 1 atmosphere, a solution of a non-aqueous dispersion medium containing 5% by mass of a dispersant contained in the raw material composition is mixed with a cooling liquid medium in a mass ratio of 1:1, stirred at 2000 rpm for 30 seconds using a self-rotating revolution stirring device, filtered with a filter with a 30 μm mesh, and the solid content (X mass%) of the filtrate is measured. When the solid content of the filtrate is reduced by more than 5% compared to the theoretical solid content (2.5 mass%), it can be judged that precipitation has occurred. Specifically, when the formula "((2.5 mass%-X mass%) / 2.5 mass%)×100" is satisfied and is less than 5%, it is judged that no solid precipitates are produced. When the dispersant was not dissolved at 5% by mass in the non-aqueous dispersion medium, the test was carried out at the maximum soluble concentration, and similarly, precipitation was determined to have occurred when the solid content decreased by 5% or more from the theoretical solid content.

[0095] In another embodiment, at 25°C, the cooling liquid medium is preferably a liquid medium that dissolves 0.1% by mass or more of the dispersant contained in the raw material composition. The cooling liquid medium is a liquid medium for evaluating the solubility of the dispersant at 25°C and 1 atmosphere. The solubility of the dispersant relative to the cooling liquid medium is expressed by the percentage of the mass of the dispersant relative to the total mass of the dispersant and the cooling liquid medium. The solubility of the dispersant relative to the cooling liquid medium is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and further preferably 1.0% by mass or more. By dissolving the dispersant of the raw material composition by the cooling liquid medium, even if the raw material composition leaking from the supply mechanism comes into contact with the cooling liquid medium, the reduction of the function of the dispersant can be suppressed, the stability of the system is maintained, and the aggregation of the dispersed substance is prevented.

[0096] Specifically, the solubility of the dispersant in the cooling liquid medium can be determined according to the following procedure.

[0097] (1) A liquid medium containing a dispersant in a predetermined amount (Y mass %) relative to the total amount of the cooling liquid medium and the dispersant is prepared, and the liquid medium is mixed by stirring at 1500 rpm for 24 hours using a high-speed disperser homogenizer. In addition, if the dispersant lumps are large, they are cut into 1 cm square or less before use.

[0098] (2) After filtering using a filter with a mesh size of 30 μm, the solid content (X mass %) of the filtrate is measured. When the ratio of the solid content (X mass %) of the filtrate to the theoretical solid content (Y mass %) is less than 20% ((Y mass % - X mass %) / Y mass %) × 100), it is judged to be dissolved.

[0099] <Another embodiment>

[0100] Hereinafter, another embodiment of the method for producing a dispersed composition using a dispersion device will be described. The dispersion device for producing the dispersed composition can use the above-mentioned device.

[0101] According to the embodiment, a method for producing a dispersed composition is provided, which uses a dispersing device, wherein the dispersing device includes: a dispersing mechanism for dispersing a raw material composition; a supply mechanism including a plunger portion and supplying the raw material composition to the dispersing mechanism; and a cooling mechanism for cooling the plunger portion using a cooling liquid medium, wherein the method for producing a dispersed composition satisfies at least one of the following (i), (ii) and (iii).

[0102] (i) The raw material composition contains a non-aqueous dispersion medium and a dispersoid, and the cooling liquid medium is a liquid medium in which the number of particles of 10 μm or more is 0 to 50 in the following aggregation test.

[0103] (Agglomeration test)

[0104] The method comprises dispersing a composition identical to the raw material composition using a bead mill or a high-pressure homogenizer, preparing a test dispersion having a particle size of less than 10 μm using a grinding tester (0 μm to 100 μm), mixing the test dispersion with a cooling liquid medium at a mass ratio of 1:1 at 25° C. to prepare a test sample, and confirming the number of particles of 10 μm or more in the test sample using a grinding tester (0 μm to 100 μm).

[0105] (ii) The raw material composition comprises a dispersoid, a non-aqueous dispersion medium and a dispersant, and the cooling liquid medium is a liquid medium that does not produce solid precipitates at 25° C. in a state where a solution of a non-aqueous dispersion medium containing 5% by mass of the dispersant and the cooling liquid medium are mixed in a mass ratio of 1:1.

[0106] (iii) The raw material composition comprises a dispersoid, a non-aqueous dispersion medium and a dispersant, and the cooling liquid medium is a liquid medium in which 0.1 mass % or more of the dispersant contained in the raw material composition is dissolved at 25°C.

[0107] In the above embodiment, at least one of (i), (ii) and (iii) is sufficient. Preferably, (i) is satisfied. When the raw material composition contains a dispersant, it is more preferable to satisfy (i) and (ii) or (iii) at the same time, and it is more preferable to satisfy (i), (ii) and (iii) at the same time.

[0108] Example

[0109] The present invention is described in more detail below with reference to the following examples. The present invention is not limited to the following examples unless it exceeds the gist of the invention. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0110] (Dispersion device)

[0111] In Example 1, a valve-type high-pressure homogenizer of "HC3-5" (trade name) manufactured by Sanmaru Machinery Co., Ltd. was used for dispersion. In Example 2, a valve-type high-pressure homogenizer of "HC3-5" (trade name) manufactured by Sanmaru Machinery Co., Ltd. was used to disperse the dispersed composition after one pass dispersion using a nozzle-type high-pressure homogenizer of "Star Burst 100" (trade name) manufactured by Sugino Machine Co., Ltd. under the operating condition of 100 MPa in a single nozzle chamber. The dispersion conditions are as shown in Table 1. In the table, Ex. indicates the example number, and No. indicates the recipe number. The cooling mechanism is as shown in Table 1. Figure 2 The cooling liquid medium is supplied to the cooling liquid medium tank of the cooling mechanism, and the cooling liquid medium is circulated at a flow rate of 2 L / H during the operation of the dispersion device.

[0112] (Raw Material Composition)

[0113] As a raw material composition, each component was mixed according to the following formulation.

[0114] Prescription 1:

[0115] Carbon nanotube ("100P" manufactured by Kumho Corporation) 3 mass%

[0116] N-methyl-2-pyrrolidone (NMP) 96 mass%

[0117] Dispersant ("Zetpol 2010L" manufactured by ZEON Co., Ltd., Japan) 1 mass%

[0118] Prescription 2:

[0119] Carbon nanotube ("trade name: 100P" manufactured by Kumho Corporation) 2 mass%

[0120] Butyl acetate 90 mass%

[0121] Dispersant ("DISPERBYK 111" manufactured by BYK, solid content 95%) 8 mass%

[0122] Prescription 3:

[0123] Carbon black ("Denka black granules" manufactured by Denka Corporation) 20% by mass

[0124] N-methyl-2-pyrrolidone (NMP) 78.95 mass%

[0125] Dispersant ("Trade name: polyacrylonitrile Mw 150,000" manufactured by Sigma-Aldrich) 1 mass%

[0126] pH adjuster ("Sodium hydroxide", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.05 mass%

[0127] Prescription 4:

[0128] Titanium oxide ("CR-95" manufactured by Ishihara Sangyo Co., Ltd.) 50 mass%

[0129] Methyl ethyl ketone 44.0 mass%

[0130] Dispersant ("DISPERBYK 182" manufactured by Lubrizol Japan, solid content 43%) 6.0 mass%

[0131] Prescription 5:

[0132] ITO ("E-ITO", manufactured by Mitsubishi Materials Corporation) 9 mass%

[0133] α-Terpineol 87% by mass

[0134] Dispersant ("DISPERBYK 111" manufactured by BYK, solid content 95%) 1 mass%

[0135] Prescription 6:

[0136] Carbon nanotube ("trade name: 100P" manufactured by Kumho Corporation) 1 mass%

[0137] Methyl Ethyl Ketone (MEK) 89 mass%

[0138] Dispersant ("EFKA PX4320" manufactured by BASF, solid content 50%) 10 mass%

[0139] (Cooling liquid medium)

[0140] The cooling liquid media shown in Table 1 were prepared.

[0141] (Agglomeration test)

[0142] The coagulation test was performed in the following procedure for the combinations of the raw material composition and the cooling liquid medium shown in Table 1. The coagulation test was performed in an environment of 25°C.

[0143] (1) The same composition as the raw material composition was dispersed using a bead mill, and a test dispersion having a particle size of less than 10 μm was prepared using a grinding tester (0 μm to 100 μm). The dispersion device used was "Starmill LMZ2" manufactured by Ashizawa Finetech. Regarding the dispersion conditions, the dispersion was performed at a peripheral speed of 12 m / s until the particle size was less than 10 μm.

[0144] (2) 10 g of the test dispersion and 10 g of the cooling liquid medium were weighed in a stirring container ("001 stirring container" manufactured by Kinki Kaiji Co., Ltd.), and stirred at 2000 rpm for 30 seconds using a Thinky mixer to prepare a test sample.

[0145] (3) After the test sample was prepared, the number of particles of 10 μm or larger in the test sample was checked using a polishing tester (0 μm to 100 μm) within 60 seconds.

[0146] <Grinding tester>

[0147] The grinding tester used in (1) and (3) of the aggregation test is as follows.

[0148] Gauge model: "GS0-100" manufactured by Taiyou Machinery Co., Ltd.

[0149] Groove depth: 0μm~100μm, scale interval: 10μm

[0150] <Judgment Criteria>

[0151] The results of the aggregation test were evaluated according to the number of particles of 10 μm or more confirmed in the test sample in accordance with the following criteria.

[0152] ○: No particles larger than 10 μm (no aggregation)

[0153] △: The number of particles with a size of 10 μm or more is 1 or more and 50 or less (some aggregation occurs)

[0154] ×: There are 51 or more particles with a size of 10 μm or larger (agglomeration occurs)

[0155] (Life evaluation of gland gasket)

[0156] The dispersion device was operated for 100 hours using the combination of the raw material composition and the cooling liquid medium shown in Table 1. The leakage amount of the raw material composition from the supply mechanism (plunger part) and the supply amount of the raw material composition were measured every 100 hours of operation, and the leakage rate (%) was calculated according to the following formula (1).

[0157] Leakage rate (%) = (amount of raw material composition leaking from the supply mechanism (L) / amount of raw material composition processed (L)) × 100 (1)

[0158] The leakage amount of the raw material composition from the supply mechanism is obtained according to the following procedure.

[0159] (1) When replacing the gland gasket, the cooling liquid medium is also replaced. The cooling liquid medium at this time is referred to as X(L).

[0160] (2) The liquid recovered in the cooling liquid medium tank when the total operation time reaches 100 hours is defined as Y(L). The leakage amount of the raw material composition from the supply mechanism is calculated according to the following formula.

[0161] The amount of raw material composition leaking from the supply mechanism (L) = Y (L) - X (L)

[0162] Based on the leakage rate obtained above, the results of the coagulation test were evaluated according to the following criteria.

[0163] <Judgment Criteria>

[0164] ○: Leakage rate is 0.10% or less

[0165] △: Leakage rate exceeds 0.10% and is less than 0.20%

[0166] ×: Leakage rate exceeds 0.20%

[0167] (Precipitation test)

[0168] The precipitation test was performed in the following procedure for the combinations of the dispersant and the cooling liquid medium shown in Table 1. The precipitation test was performed in an environment of 25°C.

[0169] (1) The dispersant contained in the raw material composition is dissolved in a non-aqueous dispersion medium at a concentration of 5% by mass.

[0170] (2) 30 g of a non-aqueous dispersion medium solution containing a dispersant dissolved at a concentration of 5% by mass and 30 g of a cooling liquid medium were weighed in a stirring container ("001 stirring container" manufactured by Kinki Kaiji Co., Ltd.), and stirred at 2000 rpm for 30 seconds using a Thinky mixer.

[0171] (3) After filtering using a filter with a mesh size of 30 μm, the solid content of the filtrate is measured. When the solid content of the filtrate (X mass %) is reduced by 5% or more compared to the theoretical solid content (2.5 mass %), specifically, when the formula "((2.5 mass % - X mass %) / 2.5 mass %) × 100" is satisfied and is 5% or more, it is judged that precipitation has occurred. In addition, the solid content of the filtrate is measured by measuring 5 g of the filtrate in an aluminum pan, using the mass before and after drying in an oven at 200°C for 2 hours, and calculating according to the following formula.

[0172] Solid content (mass %) = ((mass of aluminum pan + filtrate after 2 hours at 200°C) / (mass of aluminum pan + filtrate)) × 100

[0173] <Judgment Criteria>

[0174] The results of the precipitation test were evaluated according to the following criteria. The results are shown in Table 1.

[0175] ○: The solid content of the filtrate decreases by less than 5% from the theoretical solid content (2.5 mass%), or does not decrease (no precipitation occurs)

[0176] ×: The solid content of the filtrate is reduced by 5% or more from the theoretical solid content (2.5% by mass) (precipitation occurs)

[0177] (Dissolution test)

[0178] The dissolution test was conducted in the following procedure for the combinations of the dispersant and the cooling liquid medium shown in Table 1. The dissolution test was conducted in an environment of 25°C.

[0179] (1) 499.5 g of a cooling liquid medium and 0.5 g of a dispersant contained in the raw material composition were weighed in a 1 L container and stirred at 1500 rpm for 24 hours using a high-speed disperser homogenizer to prepare a cooling liquid medium containing 0.1 mass % of the dispersant.

[0180] (2) After filtering using a filter with a mesh size of 30 μm, the solid content of the filtrate is measured. When the solid content of the filtrate (X mass %) is reduced by 20% or more compared to the theoretical solid content (0.1 mass %), specifically, when the formula "((0.1 mass % - X mass %) / 0.1 mass %) × 100" is satisfied and is 20% or more, it is judged that there is no dissolution. In addition, the solid content of the filtrate is measured by measuring 5 g of the filtrate in an aluminum pan, using the mass before and after drying in an oven at 200°C for 2 hours, and calculating according to the following formula.

[0181] Solid content (mass %) = ((mass of aluminum pan + filtrate after 2 hours at 200°C) / (mass of aluminum pan + filtrate)) × 100

[0182] <Judgment Criteria>

[0183] The results of the dissolution test were evaluated according to the following criteria. The results are shown in Table 1.

[0184] ○: The solid content of the filtrate decreases by less than 20% compared to the theoretical solid content (0.1 mass%), or does not decrease (dissolve)

[0185] ×: The solid content of the filtrate is reduced by 20% or more compared to the theoretical solid content (0.1 mass%) (no dissolution)

[0186]

[0187]

[0188] According to the table, through the results of the condensation test, it is known that in the example where no condensate is generated, the leakage rate of the cooling liquid medium from the plunger portion is reduced, and the life of the gland gasket is prolonged. In addition, it is known that even in the example where the number of condensates generated is small, the leakage rate of the cooling liquid medium from the plunger portion is reduced, and the life of the gland gasket is also prolonged. Through the results of the condensation test, it is known that in the example where a large amount of condensates are generated, the leakage rate of the cooling liquid medium from the plunger portion is increased, and the life of the gland gasket is shortened.

[0189] According to the precipitation test, it is known that in the case where the non-aqueous dispersion medium containing 5 mass % of the dispersant and the cooling liquid medium are mixed at a mass ratio of 1:1 without generating solid precipitates, the life of the gland gasket is prolonged. According to the coagulation test, in the case where the cooling liquid medium containing 0.1 mass % of the dispersant is evaluated to have dissolved the dispersant, the life of the gland gasket is prolonged.

[0190] Although the present invention has been described with reference to the above-described embodiments, the present invention is not limited to the above-described embodiments. Various changes can be made to the structure and details of the present invention within the scope of the present invention.

[0191] The disclosure of the present application is related to the subject matter described in Japanese Patent Application No. 2022-014907 filed on February 2, 2022, and all the disclosed contents are incorporated herein by reference.

[0192] Explanation of symbols

[0193] 10: Plunger

[0194] 20: High pressure pump

[0195] 21: Cylinder body

[0196] 24: Gland gasket

[0197] 30: Dispersed Department

[0198] 31: Valve seat

[0199] 32: Impact Ring

[0200] 33: Homogenizing valve

[0201] 40: Cooling mechanism

[0202] 41: Cooling liquid medium tank

[0203] 42: Cooling unit

[0204] 43: Recycling Container

[0205] 50: Raw material composition tank

[0206] 100: Dispersion device

Claims

1. A method for producing a dispersed composition, using a dispersing device, the dispersing device comprising: A dispersing mechanism for dispersing the raw material composition; a supply mechanism including a plunger portion and supplying the raw material composition to the dispersion mechanism; as well as A cooling mechanism cools the plunger portion using a cooling liquid medium, wherein The raw material composition comprises a non-aqueous dispersion medium and a dispersant, The cooling liquid medium is a liquid medium in which the number of particles larger than 10 μm is 0 to 50 in the following agglomeration test. (Agglomeration test) The same composition as the raw material composition is dispersed by a bead mill or a high-pressure homogenizer, and a test dispersion having a particle size of less than 10 μm is prepared by a grinding tester (0 μm to 100 μm). The test dispersion and the cooling liquid medium are mixed at a mass ratio of 1:1 at 25° C. to prepare a test sample, and the number of particles of 10 μm or more in the test sample is confirmed using a grinding tester (0 μm to 100 μm). 2 . The method for producing a dispersed composition according to claim 1 , wherein the nonaqueous dispersion medium of the raw material composition and the cooling liquid medium comprise the same liquid medium.

3. The method for producing a dispersed composition according to claim 1 or 2, wherein the leakage rate of the raw material composition represented by the following formula (1) from the supply mechanism is 0.2% or less per 100 hours of operation time, Leakage rate (%) = (leakage amount of raw material composition from the supply mechanism (L) / supply amount of raw material composition (L)) × 100 (1).

4. A method for producing a dispersed composition, using a dispersing device, the dispersing device comprising: A dispersing mechanism for dispersing the raw material composition; a supply mechanism including a plunger portion and supplying the raw material composition to the dispersion mechanism; as well as A cooling mechanism cools the plunger portion using a cooling liquid medium, wherein The raw material composition includes a dispersoid, a non-aqueous dispersion medium, and a dispersant, and the cooling liquid medium is a liquid medium that does not produce solid precipitates at 25° C. in a state where a solution of the non-aqueous dispersion medium containing 5% by mass of the dispersant and the cooling liquid medium are mixed at a mass ratio of 1:

1.

5. A method for producing a dispersed composition, using a dispersing device, the dispersing device comprising: A dispersing mechanism for dispersing the raw material composition; a supply mechanism including a plunger portion and supplying the raw material composition to the dispersion mechanism; as well as A cooling mechanism cools the plunger portion using a cooling liquid medium, wherein The raw material composition comprises a dispersoid, a non-aqueous dispersion medium and a dispersant. The cooling liquid medium is a liquid medium in which 0.1 mass % or more of the dispersant contained in the raw material composition is dissolved at 25° C.