Ferroelectric component or structure and method for producing ferroelectric component or structure
By using a diamond-like carbon layer as a hard mask on ferroelectric materials, the etching problem in the manufacturing of lithium niobate devices is solved, wafer-level manufacturing of high-performance, low-loss ferroelectric integrated photonics devices is achieved, and current problems are solved. There are manufacturing efficiency and performance deficiencies in the technology.
Patent Information
- Application Number
- CN202180105446.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-20
- Publication Date
- 2024-10-01
AI Technical Summary
Manufacturing high-performance ferroelectric devices or structures, especially lithium niobate, faces problems such as difficult etching of materials, high optical loss, insufficient structural aspect ratio, and long manufacturing time, and wafer-level manufacturing cannot be achieved.
Using a diamond-like carbon layer as a hard mask material, high-performance integrated photonic devices are designed and manufactured on ferroelectric materials through deposition and etching technologies, using the characteristics of low sputtering yield and resistance to ion bombardment etching to achieve smooth etching and high-fidelity Trueness.
It produces high-aspect ratio, low-loss ferroelectric integrated photonic devices that are compatible with DUV wafer-level processing, realizing wafer-level manufacturing of lithium niobate, and its performance is better than traditional etching mask methods.
Smart Images

Figure CN118742845A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to ferroelectric devices or structures and methods for producing or manufacturing at least one or more ferroelectric devices or structures. The ferroelectric devices or structures may, for example, include or consist of photonic devices, or include or consist of integrated photonic devices (such as but not limited to integrated photonic waveguides, resonators and electro-optical devices). Background Art
[0002] Ferroelectric materials such as lithium niobate are of particular importance, for example, for linear and nonlinear optical devices such as electro-optical devices, acousto-optical devices, optical waveguides, optical modulators, optical switches, frequency converters, and piezoelectric sensors.
[0003] However, it is challenging to fabricate ferroelectric devices or structures (such as lithium niobate structures or devices) with high performance properties. For example, lithium niobate is a hard and chemically inert material that is difficult to etch. Unlike, for example, silicon, it cannot be satisfactorily chemically etched to fabricate nanometer or high aspect ratio optical waveguides.
[0004] The produced devices have, for example, significant optical losses and / or insufficient structural aspect ratios, which prevents obtaining high performance optical devices. Furthermore, long manufacturing times are required and stitching methods are often used during manufacturing, which results in production misalignment at the stitching between regions. Wafer-scale manufacturing is currently not possible.
[0005] US11086048 discloses a method for manufacturing a lithium niobate device.
[0006] An alternative fabrication approach involves a hybrid method that involves bonding the lithium niobate material to a silicon substrate via flip-chip bonding and employing an adhesive bonding process (He et al., Nature Photonics, Vol. 13, May 2019, 359-364, https: / / doi.org / 10.1038 / s41566-019-0378-6).
[0007] The present invention solves the above mentioned inconveniences. The present invention also provides an alternative to the known manufacturing methods. Summary of the invention
[0008] The present invention solves the above limitations by providing a method for producing at least one or more ferroelectric devices or structures. The method comprises the following steps: providing at least one ferroelectric material or layer, or providing at least one ferroelectric material or layer to be patterned or structured; depositing at least one adhesion layer on a first side of the at least one ferroelectric material or layer; and depositing at least one diamond-like carbon layer or material on the at least one adhesion layer.
[0009] The present invention solves the above limitations by providing a ferroelectric device or structure, which includes at least one ferroelectric material or layer, at least one adhesion layer on a first side of the at least one ferroelectric material or layer; and at least one diamond-like carbon layer or material on the at least one adhesion layer.
[0010] The present invention addresses the above limitations by providing a ferroelectric device or structure, which includes at least one ferroelectric material or layer, at least one adhesion layer on a first side of the at least one ferroelectric material or layer; at least one diamond-like carbon layer or material on the at least one adhesion layer; at least one additional adhesion layer on a second side of the at least one ferroelectric material or layer and at least one diamond-like carbon layer or material on at least one additional adhesion layer on the second side of the at least one ferroelectric material or layer.
[0011] Further advantageous features can be found in the dependent claims.
[0012] The structures, devices and methods of the present disclosure allow for wafer-scale fabrication of superior integrated photonic devices, for example, on ferroelectric thin film platforms such as lithium niobate.
[0013] The use and accommodation of, for example, diamond-like carbon thin films as mask materials in etching processes is advantageous and allows the design and provision of structures and devices with high performance characteristics. Due to its very low sputtering yield, this material is highly resistant to physical etching, for example by ion bombardment. This enables the underlying ferroelectric material to be etched smoothly while maintaining good verticality and significant fidelity to the intended design or pattern. This innovative process can produce integrated photonic devices that produce performance that is superior to that achieved with known etching masks.
[0014] Known etch masks can experience mask erosion, limiting the height or profile of optical structures or devices such as waveguides.The disclosed methods and devices allow for the production of high quality and low loss ferroelectric (eg, lithium niobate) integrated photonics devices with high aspect ratios.
[0015] Another key advantage is that the disclosed hard mask fabrication process is compatible with DUV wafer level processing and enables the production of, for example, LNOI based integrated photonic waveguides.
[0016] The methods and devices of the present disclosure allow for DUV-compatible wafer-scale fabrication of high-quality and low-loss ferroelectric (eg, lithium niobate) integrated photonics devices with high aspect ratios.
[0017] The above and other objects, features and advantages of the present invention and the manner in which they are accomplished will become more apparent, and the invention itself will be best understood by studying the following description with reference to the accompanying drawings, which illustrate some preferred embodiments of the invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figures 1A to 1K An exemplary method for producing at least one or more ferroelectric devices or structures according to the present disclosure is shown. The method steps are not necessarily performed in the order shown, and not all steps are necessarily performed.
[0019] Figures 2A to 2N Another exemplary method for producing at least one or more ferroelectric devices or structures according to the present disclosure is shown. The method steps are not necessarily performed in the order shown, and not all steps are necessarily performed.
[0020] Figures 3A to 3D Different ferroelectric devices or structures are shown, which are produced as intermediate products by the method according to the present disclosure.
[0021] Figures 4 to 10 is a SEM image of a ferroelectric device or structure produced by the method of the present disclosure.
[0022] Figure 4 is a cross-sectional SEM image of a lithium niobate waveguide etched with a diamond-like carbon DLC etch mask after re-deposition cleaning and mask removal. The starting lithium niobate film thickness is 700nm, 620nm is etched, and 80nm remains. The sidewall angle is 77°.
[0023] Figure 5 is a tilted SEM image of the sidewall of a lithium niobate waveguide etched with a diamond-like carbon (DLC) etch mask after re-deposition cleaning and mask removal.
[0024] Figures 6 to 10 is a tilted SEM image showing an example of an integrated lithium niobate photonic device after lithium niobate etching, redeposition cleaning, and mask removal. Figures 6 to 10 A 100 GHz FSR ring resonator, coupled ring resonators, very thin tapered waveguide, 2-2 splitter and Y splitter are shown respectively.
[0025] The material shown in the figures is provided by way of example, and the methods, devices, and structures of the present disclosure are not limited to the specific details shown in the figures.
[0026] Herein, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. DETAILED DESCRIPTION
[0027] Figures 1A to 1K Exemplary steps of an exemplary embodiment of a manufacturing method according to the present disclosure are shown. The method steps are not necessarily performed in the order shown, and not all steps are necessarily performed.
[0028] The method produces a ferroelectric device or a ferroelectric structure FD. The ferroelectric device or structure FD may include, for example, Figures 3A to 3D The ferroelectric layer or material 3 shown may alternatively include, for example, Figure 1K and 2N The patterned or structured ferroelectric layer or material 3 shown may be formed by, for example, Figure 1K and 2N The patterned or structured ferroelectric layer or material 3 is shown.
[0029] The ferroelectric device or structure FD may include further materials or layers provided above and / or below the ferroelectric layer or material 3 .
[0030] The patterned or structured ferroelectric layer or material 3 comprises or defines one or more elements EL, which may define features or components of a device, such as features or components of an optical or optoelectronic device.
[0031] These elements EL may include, for example, protrusions EL1, recesses EL2 or openings EL3 extending partially or completely through the ferroelectric layer or material 3. These elements may extend across the ferroelectric layer or material 3 to define an elongated device or structure. For example, the device or structure may include or consist of a protrusion EL1 defined by a first and a second recess EL2 (or a recess EL2 and an opening EL3), the first and the second recess EL2 defining a first side wall SW1 and a second side wall SW2 of the device or structure.
[0032] The structured or patterned ferroelectric layer or material 3 may be part of a device that includes other materials or elements located above and / or below the ferroelectric layer or material 3. For example, where the ferroelectric layer or material 3 is included in or as part of a ferroelectric-on-insulator wafer (e.g., a lithium niobate-on-insulator (LNOI) wafer), a silicon electronic device may be used to electronically or electrically control the structured or patterned ferroelectric layer or material 3, which may also, for example, include electrodes in contact therewith.
[0033] The structured or patterned ferroelectric layer or material 3 may, for example, comprise, define or be part of a plurality of interconnect devices, such as interconnects or integrated photonic devices. Figures 6 to 10 Exemplary devices are shown, but other devices and device configurations are possible.
[0034] As described above, the ferroelectric device or structure FD may include, for example, an unpatterned or unstructured ferroelectric layer or material 3, such as Figures 3A to 3D As shown. These ferroelectric devices or structures FD are, for example, (DUV) lithography-ready intermediate products. This facilitates large-scale and high-frequency production of ferroelectric devices, for example, to produce lithium niobate integrated photonics devices.
[0035] The method of the present disclosure is a wafer-less bonding method or an adhesive-free wafer bonding method.
[0036] The method for producing a ferroelectric device or structure FD comprises providing at least one ferroelectric material or layer 3 or providing at least one ferroelectric material or layer 3 to be patterned or structured.
[0037] The provided ferroelectric material or layer 3 may be, for example, a carrier or support consisting only of ferroelectric material.
[0038] Alternatively, the ferroelectric material or layer 3 may be provided, for example, as part of a carrier, a wafer or a support comprising the ferroelectric material or layer 3 and also comprising other layers or materials (e.g., included as an underlying layer below the ferroelectric material or layer 3). The ferroelectric material or layer 3 may, for example, be provided on a substrate consisting of a material different from the material of the ferroelectric material or layer 3. The ferroelectric material or layer 3 may be provided directly or indirectly on a substrate layer.
[0039] For example, the ferroelectric material or layer 3 may be included in or as part of a ferroelectric-on-insulator wafer or carrier 5 (see, e.g. Figure 1A ). The ferroelectric on insulator wafer or carrier 5 may comprise or consist of a substrate 5A, at least one oxide layer 5B provided on the substrate 5A and at least one ferroelectric material or layer 3 provided on the oxide layer 5B. An additional oxide layer 5C may also be provided between the ferroelectric material 3 and the substrate 5A, the additional oxide layer 5C being provided on an opposite substrate side S2 opposite to the side S1 where the oxide layer 5B is located.
[0040] The ferroelectric material or layer 3 may, for example, be part of or comprised in a lithium niobate on insulator (LNOI) wafer or carrier 5, as shown in the exemplary and non-limiting embodiments of the accompanying drawings (see, for example, Figure 1A and 2A ). The lithium niobate on insulator wafer 5 comprises or consists of a substrate 5A, at least one oxide layer 5B provided (e.g. directly) on the substrate 5A, and at least one lithium niobate (LiNbO3) layer or material 3 provided (e.g. directly) on the oxide layer 5B. The lithium niobate on insulator wafer 5 may further comprise at least one additional oxide layer 5C provided on the substrate 5A on a side S2 of the substrate 5A opposite to the at least one oxide layer 5B.
[0041] The substrate 5A may, for example, include or consist of silicon. The oxide layers 5B, 5C may include or consist of thermal oxide layers. The oxide layers 5B, 5C may include or consist of silicon oxide (SiO 2 ).
[0042] The ferroelectric material or layer 3 may, for example, be a doped or undoped and / or single-crystalline material.
[0043] The ferroelectric material or layer 3 may, for example, comprise lithium niobate (LiNbO3) or single-crystalline lithium niobate (LiNbO3) or consist only of lithium niobate (LiNbO3) or single-crystalline lithium niobate (LiNbO3). The ferroelectric material or layer 3 may comprise doped or undoped lithium niobate (LiNbO3) or doped or undoped single-crystalline lithium niobate (LiNbO3) or consist only of doped or undoped lithium niobate (LiNbO3) or doped or undoped single-crystalline lithium niobate (LiNbO3).
[0044] The ferroelectric material or layer 3 may, for example, comprise or consist exclusively of lithium tantalate (LiTaO 3 ) or barium titanate BTO or gallium phosphide GaP.
[0045] The ferroelectric material or layer 3 may be provided, for example, with a thickness t between 100 nm and 10 μm, or between 250 nm and 1 μm, for example 500 nm or 700 nm. FM (Before etching).
[0046] For example, a lithium niobate on insulator (LNOI) wafer or carrier 5 may include a thickness t FM A lithium niobate layer of 500nm or 700nm, a substrate 5A with a thickness between 500μm and 1000μm (e.g. 500μm or 700μm), a first or upper oxide layer 5B with a thickness between 3μm and 7μm (e.g. 4.7μm), and a second or lower oxide layer 5C with a thickness between 3μm and 7μm (e.g. 4.7μm).
[0047] For example, Figure 1B As shown, at least one adhesion layer 7 may be deposited or provided on the first side SD1 of the ferroelectric material or layer 3. At least one diamond-like carbon layer or material (DLC) 9 may be provided or deposited on the adhesion layer 7. Figure 1C ).
[0048] The adhesion layer 7 is configured to ensure adhesion of the diamond-like carbon layer or material (DLC) 9 to the ferroelectric material or layer 3, in particular during processing of the device or structure.
[0049] The adhesion layer 7 is configured to prevent delamination of the diamond-like carbon layer or material 9 from the ferroelectric material or layer 3 .
[0050] The adhesion layer 7 is, for example, deposited directly on the first side SD1 of the ferroelectric material or layer 3 or is in direct contact with the first side SD1 of the ferroelectric material or layer 3 .
[0051] The adhesion layer 7 may, for example, include or consist of silicon nitride (Si 3 N 4 ), silicon oxide (SiO 2 ) or sapphire (Al 2 O 3 ).
[0052] The adhesion layer 7 can be deposited, for example, by chemical vapor deposition, such as plasma enhanced chemical vapor deposition (PECVD). For example, an adhesion layer 7 with a thickness between 20 and 60 nm can be deposited. For example, 30 nm of silicon nitride (Si3N4) can be deposited by PECVD as the adhesion layer 7. For example, a standard recipe for Si3N4 can be used, for example, the deposition is performed with an Oxford Instruments PlasmaPro 100PECVD tool. For example, the following deposition parameters can be used: chamber pressure = 800 mTorr, RF power = 40 W, SiH4 / N4 (2%) gas flow rate: 1000 sccm, NH3 gas flow rate = 15 sccm, bottom electrode temperature = 300°C, deposition time = 1 min.
[0053] As mentioned above, in a preferred embodiment, a diamond-like carbon layer or material (DLC) 9 ( Figure 1C ). The diamond-like carbon layer or material (DLC) 9 defines the hard mask layer and acts as a hard mask.
[0054] The diamond-like carbon layer or material 9 is, for example, deposited directly on the adhesion layer 7 which is deposited on the first side SD1 of the ferroelectric material or layer 3 .
[0055] The diamond-like carbon layer or material 9 may be deposited on the adhesion layer 7, for example, by a chemical vapor deposition (CVD) process. The thickness of the diamond-like carbon layer or material 9 may be, for example, between 200 nm and 1000 nm, for example, 500 nm. The deposition may be performed in a reactive ion etching chamber, for example, an Oxford Instruments PlasmaPro 80. For example, the following deposition parameters may be used: chamber pressure = 30 mTorr, 200 W DC bias, 50 sccm CH4 gas flow. Prior to deposition, a surface cleaning step may be performed, for example, cleaning for 2 minutes at a pressure of 40 mTorr, 150 W DC bias power and 50 sccm argon gas flow.
[0056] The diamond-like carbon layer or material 9 may alternatively be deposited on the adhesion layer 7 , for example by a physical vapor deposition process.
[0057] The inventors have found that the diamond-like carbon layer or material is resistant to etching, especially physical etching by ion bombardment, and has a very low sputtering yield. The diamond-like carbon layer or material determines the selectivity of the etching rate compared to the etching rate of the ferroelectric material and allows the underlying ferroelectric material to be smoothly etched while maintaining excellent verticality and excellent fidelity to the intended design or pattern to be transferred to the ferroelectric material. Therefore, integrated photonic devices can be produced that produce performance superior to that achieved with prior art etching masks.
[0058] The diamond-like carbon layer or material (DLC) 9 may, for example, comprise or consist of an amorphous material or an amorphous carbon layer / film or a carbon material.
[0059] The diamond-like carbon layer or material (DLC) 9 may, for example, include an amorphous carbon film and sp 3 hybridized carbon atoms and hydrogen, or amorphous carbon film and sp 3 Hybridized carbon atoms and hydrogen.
[0060] The layer or material may for example have no long range crystalline order.The diamond-like carbon layer or material (DLC) 9 may for example comprise or consist of micro- or nano-crystalline diamond and graphite.
[0061] It exhibits typical properties of diamond, such as great hardness. The diamond-like carbon layer or material (DLC) 9 is a material different from natural diamond or synthetic diamond and does not include or consist of natural diamond or synthetic diamond.
[0062] For example, detailed information on diamond-like carbon layers or materials (DLC) 9 can be found in Carbon Alloys, Novel Concepts to Develop Carbon Science and Technology (2003), pp. 545-558, Chapter 34 - Super Hard Materials (by Osamu Takai), https: / / doi.org / 10.1016 / B978-008044163-4 / 50034-6, and Properties and Classification of Diamond-Like Carbon Films (by Naoto Ohtake et al., Materials 2021, 14(2), 315, https: / / doi.org / 10.3390 / ma14020315), the entire contents of which are incorporated herein.
[0063] The diamond-like carbon layer or material 9 may, for example, be an internal or intrinsic stress compensating layer or a compressive stress compensating layer.
[0064] Although the preferred embodiment uses a diamond-like carbon layer or material (DLC) 9 as a hard mask, it should be noted that alternative hard mask layers may, for example, comprise or consist of at least one silicon carbide (SiC) layer or material.
[0065] For example, Figure 1D As shown, a capping layer 11 may be provided or deposited on the diamond-like carbon layer or material 9. It is (indirectly) deposited on the first side SD1 of the ferroelectric material or layer 3. The capping layer 11 may be provided or deposited directly on the diamond-like carbon layer or material 9 and in direct contact with the diamond-like carbon layer or material 9.
[0066] The provision or deposition of the cover layer 11 further ensures a reliable and reproducible deposition of a stable diamond-like carbon layer or material 9 that does not delaminate. The inventors have found that the diamond-like carbon layer or material 9 does not delaminate even after storage in air for weeks or even months.
[0067] The capping layer 11 may be or act as a masking layer. The layer 11 may be a capping layer and / or a masking layer. The layer 11 may be a masking layer or a hard mask layer for etching the diamond-like carbon layer or material 9 or transferring a pattern or structure into the diamond-like carbon layer or material 9 during etching the diamond-like carbon layer or material 9. The layer 11 may be partially removed during etching of the ferroelectric material or layer 3.
[0068] The thickness t of the cover layer 11 is cl For example, less than the thickness t of at least one diamond-like carbon layer or material DLC The thickness t of the diamond-like carbon layer or material 9 is DLC The thickness t of the cover layer 11 is ml For example, 5 to 10 times larger.
[0069] The cover layer or mask layer 11 may include or consist of the same material as the adhesion layer 7 .
[0070] The cover layer or mask layer 11 may, for example, include or consist of silicon nitride (Si 3 N 4 ) or sapphire or amorphous silicon.
[0071] The thickness t of the cover layer or mask layer 11 is cl It may for example be between 20 and 100 nm, for example 60 nm.
[0072] The capping layer or masking layer 11 can be deposited by chemical vapor deposition, such as plasma enhanced chemical vapor deposition (PECVD). For example, a layer with a thickness between 20 and 100 nm can be deposited. For example, 60 nm of silicon nitride (Si3N4) can be deposited by PECVD. For example, a standard recipe for Si3N4 can be used, and the deposition can be performed using, for example, an Oxford Instruments PlasmaPro 100PECVD tool. For example, the following deposition parameters can be used: chamber pressure = 800 mTorr, RF power = 40 W, SiH4 / N4 (2%) gas flow: 1000 sccm, NH3 gas flow = 15 sccm, bottom electrode temperature = 300°C, deposition time = 1 min.
[0073] For example, Figure 1E As shown, the method of the present disclosure may further include performing a photolithography process to provide at least one patterned or structured photoresist layer 15 on the cover layer or mask layer 11 (or directly on the cover layer or mask layer 11 ).
[0074] The patterned or structured photoresist layer 15 exposes one or more portions or surfaces P1 of the cover layer or mask layer 11, for example Figure 1E shown.
[0075] The patterned or structured photoresist layer 15 exposes one or more portions or surfaces P2 of the at least one diamond-like carbon layer or material 9 in the (partial) absence of the capping or masking layer 11 .
[0076] The photolithography process comprises or consists of an ultraviolet or deep ultraviolet (DUV) photolithography process. The photolithography process may be performed, for example, using stepper photolithography or step-and-repeat camera photolithography.
[0077] The process may include the following steps: A photoresist layer 15 may be coated or deposited (eg, directly coated or deposited) on the capping layer or mask layer 11 .
[0078] Photolithography or UV lithography is used to transfer (geometric) patterns or structures from a photomask or optical mask to a light-sensitive photoresist. Deep ultraviolet (DUV) lithography uses light with a wavelength of, for example, <400 nm (e.g., in the range of 193 nm-254 nm) to illuminate a photomask to define an exposure pattern on and in the photoresist so that the resulting polymer pattern can be transferred to an underlying layer or material by etching.
[0079] The exposure UV or DUV light passes through, for example, a chrome photomask on quartz, whose opaque areas serve as a template for the desired pattern. The photoresist layer 15 can be baked before and / or after exposure. Then, the exposed photoresist area is chemically developed to remove unwanted photoresist areas (the photoresist remains in the area where the photomask blocks exposure) and produce an area P1 of uncovered or exposed material or layer (e.g., layer or material 11) below, which can then be processed.
[0080] For example, the ASML PAS 5500 / 350C deep-UV stepper tool is used to expose and produce Figures 6 to 10 The device shown in . For example, the photoresist coating and development are performed using a TEL Clean Track ACT-8 tool connected in sequence. The photoresist can be, for example, a 400nm thick M108Y (6cP) DUV photoresist from JSR Micro NV, located on top of a 60nm DUV42P as an anti-reflective coating (BARC) below. For example, coating / exposure / development can be performed using a standard recipe provided by a supplier.
[0081] The above method is a positive photoresist exposure method. Alternatively, a negative photoresist exposure method using a negative photoresist may also be used.
[0082] Optionally, and before depositing the photoresist layer 15, a bottom anti-reflection coating may be deposited, for example with a thickness of 60 nm. This allows the reflection of light emanating from layers or materials below the photoresist layer 15 to be reduced.
[0083] The result of the photolithography process is a patterned or structured photoresist layer 15. The pattern or structure of the photoresist layer 15 will be transferred to the underlying layers or materials, including to the diamond-like carbon layer or material 9 and to the ferroelectric layer or material 3 to define the element EL ( Figure 1K ), element EL defines the features or components of the device.
[0084] The photolithography process completely removes portions through the thickness of the photoresist material to expose one or more portions P1 of the capping or masking layer 11, such as Figure 1E As shown, one or more portions P2 of a diamond-like carbon layer or material 9.
[0085] like Figure 1F As shown, etching may be performed to etch the capping or masking layer 11. Etching is performed to etch exposed portions P1 of the capping or masking layer 11 to remove the exposed capping or masking layer / material 11 (and underlying materials) and expose one or more portions P2 of the diamond-like carbon layer or material 9 located beneath the capping or masking layer 11. The pattern of the photoresist layer 15 is transferred to the capping or masking layer or material 11.
[0086] The etching of the mask material 11 is performed by plasma etching, for example, using an SPTS advanced plasma system with an ICP-based high-density plasma source. For example, the following etching parameters can be used: chamber pressure = 15mTorr, 50sccm CHF3 and 10sccm SF6 gas flow, 13.56MHz coil power = 950W, 13.56MHz platen power = 50W, platen temperature = 10°C. Before etching the cap layer or mask layer 11, a BARC opening step can be performed, for example, with the same tool using the following parameters: chamber pressure = 15mTorr, 10sccm O2 and 10sccm CHF3 gas flow, 13.56MHz coil power = 950W, 13.56MHz platen power = 50W, platen temperature = 10°C.
[0087] like Figure 1G As shown, etching may be performed to etch the diamond-like carbon layer or material 9. Etching is performed to etch the exposed portion or portions P2 of the diamond-like carbon layer or material 9 to remove the exposed diamond-like carbon layer or material 9 (and the underlying material) and expose one or more portions P3 of the adhesion layer 7 located below the diamond-like carbon layer or material 3. The pattern of the photoresist layer 15 is transferred to the hard mask DLC layer 9.
[0088] The etching of the hard mask DLC layer 9 is performed by plasma etching with O2, for example, using an SPTS advanced plasma system with an ICP-based high-density plasma source. For example, the following etching parameters can be used: chamber pressure = 50mTorr, 100sccm O2 gas flow, 13.56MHz coil power = 2000W, 13.56MHz platen power = 200W, platen temperature = 10°C.
[0089] Etching of the patterned or structured photoresist layer or material 15 may be performed to remove or completely remove the patterned or structured photoresist layer or material 15 (remaining top portion TP2). This may be done using the same plasma etch as used to etch the diamond-like carbon layer or material 9. The etching of the patterned or structured photoresist layer or material 15 and the diamond-like carbon layer or material 9 may be performed simultaneously.
[0090] like Figure 1H As shown, for example, etching can be performed to etch the adhesion layer or material 7. Etching is performed to etch the exposed portion or portions P3 of the adhesion layer or material 7 to remove the exposed adhesion layer or material 7 (and the underlying material) and expose one or more portions P4 of the ferroelectric material or layer 3 located below the adhesion layer 7 ( Figure 1G ). The pattern of the photoresist layer 15 is transferred to the adhesion layer or material 7.
[0091] like Figure 1H As shown, for example, etching may be performed to etch the ferroelectric material or layer 3. This may be performed, for example, by continuing with a continuous etch after completely etching through the exposed portion of the adhesion layer or material 7.
[0092] The etching is performed to etch the exposed portion or portions P4 of the ferroelectric material or layer 3 to remove the exposed ferroelectric material or layer 3 and the (immediately) underlying material.
[0093] After having been transferred to the overlying layer or material, the pattern of the photoresist layer 15 is transferred to the ferroelectric material or layer 3 material.
[0094] The ferroelectric material or layer 3 may be partially etched (eg Figure 1H ). This may allow, for example, the creation of an underlying support layer. The ferroelectric material or layer 3 may be etched completely through to expose one or more portions of P5 of any underlying layers or materials 5B, 5A.
[0095] The pattern of the photoresist layer 15 is transferred to the ferroelectric material or layer 3 to define the element EL ( Figure 1K ), the element EL defines a feature or component of a device of the ferroelectric device or structure FD.
[0096] The etching is performed to at least partially produce one or more ferroelectric devices or structures or photonic devices or integrated photonic devices, which may include or be defined by elements EL transferred to the ferroelectric material or layer 3 material.
[0097] The etching of the ferroelectric material or layer 3 and the adhesion layer or material 7 is performed, for example, by ion beam etching. The etching is performed by ion beam etching, including, for example, using a Nexus IBE350 tool from Veeco. The tool uses an argon ion source with a 1.8 MHz RF plasma generator with a power of up to 2000 W. The ions are accelerated and collimated by 3-grid optics.
[0098] The ion beam may be incident at an angle relative to the surface or intermediate ferroelectric device or structure to be etched, for example at an angle of 10° or 30°, and generated at a power of up to 2000 W, or in alternating steps of different angles and powers.
[0099] For example, the etching may be performed in such a way that a thin plate or substrate BS of 50 nm to 100 nm of the ferroelectric material or layer 3 is left, thus not etching completely through the ferroelectric material or layer 3 .
[0100] For example, in Figures 6 to 10 In the case of the device shown, an etching depth of 620 nm was achieved in the ferroelectric material 3 of lithium niobate.
[0101] The structured or patterned ferroelectric material or layer 3 produced by ion beam etching may then be cleaned to remove any redeposition of ferroelectric material that may have occurred during the ion beam etching ( Fig. 1I ). For example, this cleaning step can be performed using a solution of ammonia (NH3 28-30%), hydrogen peroxide (H2O2 3%) and deionized water heated to 85°C (concentrated RCA1 solution) in a 2:2:1 ratio (by weight) for 4 minutes.
[0102] This same ion beam etch may also be used to remove any remaining top portion TP1 of the mask or capping layer or material 11 located on top of the diamond-like carbon layer or material 9 ( Figure 1G )( Fig. 1I ). For example, during etching of the adhesion layer 7 and / or the ferroelectric material 3, a top portion TP of the mask or cover layer 11 is removed simultaneously.
[0103] For example, Figure 1J As shown, the remaining portion or top portion TP1 of the diamond-like carbon layer or material 9 located on top of the adhesion layer or material 7 and / or the ferroelectric material or layer 3 is removed ( Fig. 1I ).
[0104] For example, the remaining or top portion TP1 ( TP2 ) of the diamond-like carbon layer or material 9 may be etched by plasma etching with O 2 . Fig. 1I ). For example, this can be done using an SPTS advanced plasma system with an ICP-based high-density plasma source. For example, the following etching parameters can be used: chamber pressure = 50 mTorr, 100 sccm O2 gas flow, 13.56 MHz coil power = 2000 W, 13.56 MHz platen power = 200 W, platen temperature = 10°C.
[0105] For example, Figure 1K As shown, the remaining portion or top portion TP3 (TP3) of the adhesion layer or material 7 located on top of the ferroelectric material or layer 3 Figure 1J ) is removed.
[0106] The etching is performed by wet etching, for example, using a buffered HF (hydrofluoric acid) solution.
[0107] One or more electrodes may be provided or deposited on the ferroelectric material or layer 3 to electrically address the device or component formed by the above etching process. At least one cladding material may also be provided or deposited on the ferroelectric material or layer 3.
[0108] The ferroelectric device or structure may include or consist of a photonic device or an integrated photonic device.
[0109] Ferroelectric material or layer 3 or device or structure (e.g. Figure 1KThe device or structure in the ferroelectric structure can be divided or cut into multiple ferroelectric chips or subdivided bodies.
[0110] Figures 2A to 2N Another exemplary method for producing at least one or more ferroelectric devices or structures according to the present disclosure is shown. The method steps are not necessarily performed in the order shown, and not all steps are necessarily performed.
[0111] Apart from Figure 2B , 2F In addition to the additional steps shown in 2K and 2M / 2N, Figures 2A to 2N An exemplary method and Figures 1A to 1K The exemplary method is the same as that of .
[0112] For example, Figure 2B As shown, at least one further adhesion layer 17 is provided or deposited on a second side SD2 of the ferroelectric material or layer 3. The second side SD2 is located opposite the first side SD1. The second side SD2 is for example a lower side, whereas the first side SD1 is an upper side.
[0113] For example, Figure 2F As shown, at least one further diamond-like carbon layer or material 19 is provided or deposited on the further adhesion layer 17 located or deposited on the second side SD2 of the ferroelectric material or layer 3 .
[0114] The further adhesion layer 17 is, for example, deposited directly on the second side SD2 of the ferroelectric material or layer 3 , or is directly in contact with the ferroelectric material or layer 3 .
[0115] Alternatively, if Figure 2B As shown, the further adhesion layer 17 is indirectly deposited on or in contact with the second side SD2 of the ferroelectric material or layer 3. Between the further adhesion layer 17 and the ferroelectric material or layer 3 there are one or more underlying layers.
[0116] The further adhesion layer 17 is, for example, identical to the adhesion layer 7 and is deposited in the same way.
[0117] The thickness of the further adhesion layer 17 may be greater than the thickness of the adhesion layer 7, for example 4 to 10 times greater. The thickness of the further adhesion layer 17 may be, for example, between 120 nm and 200 nm, for example 150 nm.
[0118] The adhesion layer 7 and the further adhesion layer 17 may comprise or consist of the same material. The adhesion layer and / or the further adhesion layer may comprise or consist of, for example, silicon nitride (Si3N4), silicon oxide (SiO2) or sapphire (Al2O3).
[0119] The adhesion layer 7 and the further adhesion layer 17 may be deposited in any order, not necessarily in the order Figure 2B and 2C The sequence of deposition shown in Figure 2B and 2C A further adhesion layer 17 is deposited before the adhesion layer 7 .
[0120] The further adhesion layer 17 is configured to ensure adhesion of the diamond-like carbon layer or material (DLC) 19 to the ferroelectric material or layer 3 or to the layer(s) underneath the ferroelectric material or layer 3, in particular during processing of the device or structure.
[0121] The further adhesion layer 17 is configured to prevent delamination of the diamond-like carbon layer or material 19 .
[0122] The adhesive layer 7 and / or the further adhesive layer 17 and the cover layer 11 may comprise the same material or consist of the same material.
[0123] As described above, the further diamond-like carbon layer or material 19 is provided or deposited on the further adhesion layer 17, for example directly on the further adhesion layer 17. The further diamond-like carbon layer or material 19 is similar to the one previously described with respect to Figures 1A to 1K The diamond-like carbon layer or material 9 is the same as that described in the previous embodiments and can be deposited in the same manner.
[0124] The further diamond-like carbon layer or material 19 may for example have a thickness between 200 nm and 1000 nm. The further diamond-like carbon layer or material 19 may have the same thickness as the diamond-like carbon layer or material 9 deposited on the first side SD1, or a thickness that is less than or greater than that thickness. The further diamond-like carbon layer or material 19 may for example have a thickness of 300 nm. The thickness is selected to optimize the bending compensation.
[0125] The further diamond-like carbon layer or material 19 allows compensating for any bending that may be present or caused by the diamond-like carbon layer or material 9 on the first side S1 of the ferroelectric layer or material 3. The further diamond-like carbon layer or material 19 reduces, minimizes or eliminates the bending.
[0126] This ensures compatibility with the processing stages of micro-machining equipment, including DUV stepper lithography tools. Even in the case of single-side polished wafers with very high backside roughness, a stable film can be successfully obtained on the back side of the wafer. The further adhesion layer 17 provides adhesion stability for the further diamond-like carbon layer or material 19, even in the case of single-side polished wafers.
[0127] For example, Figure 2KAs shown, the further diamond-like carbon layer or material 19 is removed by etching the diamond-like carbon layer or material 19 deposited on the second side SD2 of the ferroelectric material or layer 3 to remove or completely remove the diamond-like carbon layer or material 19 (see, for example, Figure 2J ).
[0128] The etching is performed in the same manner as etching the diamond-like carbon layer or material 9 deposited on the first side SD1 of the ferroelectric material or layer 3, as previously described with respect to Figures 1A to 1K As described in the embodiments.
[0129] It is worth noting that the etching of the diamond-like carbon layer or material 9 deposited on the first side SD1 of the ferroelectric material or layer 3 can be performed after the etching of the diamond-like carbon layer or material 19 deposited on the second side SD2 of the ferroelectric material or layer 3, as shown in the figure, however, the etching can also be performed in the opposite order.
[0130] For example, Figure 2M and 2N As shown, the additional diamond-like carbon layer or material 19 is removed in the same manner as the adhesion layer 7 (see, for example, Figure 2J ) and the further adhesive layer 17. The removal can be performed simultaneously.
[0131] This other embodiment (such as Figures 2A to 2N The other steps are similar to those in Figures 1A to 1K As described above, the order of some steps may be changed, and some steps may not need to be performed.
[0132] Removing the adhesion layer 7 and / or the further adhesion layer 17 at least partially provides a freestanding ferroelectric device or structure.
[0133] The present disclosure also relates to ferroelectric devices or structures FD, such as Figures 3A to 3D These devices or structures FD are advantageously lithography-ready or stepper-lithography-ready.
[0134] like Figure 3A As shown, the ferroelectric device or structure FD includes a ferroelectric material or layer 3, an adhesion layer 7 on (eg, directly on) a first side SD1 of the ferroelectric material or layer 3, and a diamond-like carbon layer or material 9 on (eg, directly on) the adhesion layer 7.
[0135] The ferroelectric device or structure may further comprise an additional adhesion layer 17 ( Figure 3D ), and a further diamond-like carbon layer or material 19 on a further adhesion layer 17 on the second side SD2 of the ferroelectric material or layer 3.
[0136] The adhesion layer 7 is, for example, in direct contact with the ferroelectric material or layer 3. The diamond-like carbon layer or material 9 is, for example, in direct contact with the adhesion layer 7.
[0137] The further adhesion layer 17 may be in indirect contact with the ferroelectric material or layer 3, for example via the bottom layer(s). Figure 3D ), or alternatively, in direct contact with the ferroelectric material or layer 3 ( Figure 3C ).
[0138] The further diamond-like carbon layer or material 19 is, for example, in direct contact with the further adhesion layer 17 .
[0139] The ferroelectric device or structure may further comprise a capping or masking layer 11 (not shown) provided on the (upper) diamond-like carbon layer or material 9 provided on the adhesion layer 7 on the first side SD1 of the ferroelectric layer or material 3 .
[0140] As mentioned above, the ferroelectric material or layer 3 may include lithium niobate (LiNbO3), single-crystal lithium niobate (LiNbO3), doped lithium niobate (LiNbO3) or doped single-crystal lithium niobate (LiNbO3), or only consist of lithium niobate (LiNbO3), single-crystal lithium niobate (LiNbO3), doped lithium niobate (LiNbO3) or doped single-crystal lithium niobate (LiNbO3). The ferroelectric material or layer 3 may include lithium tantalate (LiTaO3) or only consist of lithium tantalate (LiTaO3).
[0141] The ferroelectric material or layer 3 may include or consist of lithium niobate contained in or as part of a lithium niobate-on-insulator (LNOI) wafer 5 ( Figure 3B , 3D ). The lithium niobate on insulator (LNOI) wafer 5 may include a substrate 5A, an oxide layer 5B provided on the substrate 5A, and a lithium niobate (LiNbO3) layer 3 provided on the oxide layer 5B, or may consist of the substrate 5A, the oxide layer 5B provided on the substrate 5A, and the lithium niobate (LiNbO3) layer 3 provided on the oxide layer 5B. The lithium niobate on insulator (LNOI) wafer 5 may further include an additional oxide layer 5C provided on the substrate 5A opposite to the first oxide layer 5B. The substrate may, for example, include silicon, or consist of silicon. The oxide layers 5B, 5C may include silicon oxide, or consist of, for example, silicon oxide.
[0142] The adhesion layer 7 and the further adhesion layer 17 may, for example, comprise the same material, or consist of the same material.The one adhesion layer and the cover layer or mask layer may, for example, comprise the same material, or consist of the same material.
[0143] The adhesion layer 7 and / or the further adhesion layer 17 may, for example, comprise or consist of silicon nitride (Si3N4), silicon oxide (SiO2) or sapphire (Al2O3). The cover layer or mask layer may, for example, comprise or consist of silicon nitride (Si3N4).
[0144] Although the present invention has been disclosed with reference to certain preferred embodiments, various modifications, variations and changes may be made to the described embodiments and their equivalents without departing from the scope of the present invention. Therefore, the present invention is not limited to the described embodiments, but is given the broadest reasonable interpretation according to the language of the appended claims. The features of any one of the above embodiments may be included in any other embodiment described herein.
Claims
1. A method for producing at least one ferroelectric device or structure (FD), the method comprising the following steps: - providing at least one ferroelectric material or layer (3), or providing at least one ferroelectric material or layer (3) to be patterned or structured; - depositing at least one adhesion layer (7) on the first side (SD1) of the at least one ferroelectric material or layer (3); and - depositing at least one diamond-like carbon layer or material (9) on said at least one adhesion layer (7).
2. The method according to the preceding claim, further comprising the following steps: - depositing at least one further adhesion layer (17) on the second side (SD2) of the at least one ferroelectric material or layer (3); and - depositing at least one diamond-like carbon layer or material (19) on said at least one further adhesion layer (17) deposited on the second side (SD2) of said at least one ferroelectric material or layer (3).
3. The method according to the preceding claim, wherein: The second side (SD2) is located opposite to the first side (SD1).
4. A method according to any one of the preceding claims, wherein: The at least one adhesion layer (7) is deposited directly on the first side (SD1) of the at least one ferroelectric material or layer (3), or is deposited directly in contact with the first side (SD1) of the at least one ferroelectric material or layer (3).
5. A method according to any one of the preceding claims, wherein: The at least one diamond-like carbon layer or material (9) is deposited directly on the at least one adhesion layer (7) deposited on the first side (SD1) of the at least one ferroelectric material or layer (3).
6. A method according to any one of the preceding claims, wherein: The diamond-like carbon layer or material (9) is deposited by physical vapor deposition or chemical vapor deposition on the at least one adhesion layer (7) deposited on the first side (SD1) of the at least one ferroelectric material or layer (3).
7. The method according to any one of the preceding claims 2 to 6, wherein: The at least one further adhesion layer (17) is indirectly deposited on or is indirectly in contact with the second side (SD2) of the at least one ferroelectric material or layer (3).
8. The method according to any of the preceding claims, further comprising the step of depositing a capping layer (11) on the at least one diamond-like carbon layer or material (3) deposited on the first side (SD1) of the at least one ferroelectric material or layer (3).
9. The method according to the preceding claim, wherein: The thickness (t cl ) is less than the thickness (t DLC ).
10. The method according to the preceding claim, wherein: The thickness (t DLC ) is greater than the thickness (t cl ) is 5 to 10 times larger.
11. The method according to any of the preceding claims, further comprising the step of performing a photolithography process to provide at least one patterned or structured photoresist layer (15) on the cover layer (11), wherein the at least one patterned or structured photoresist layer (15) exposes at least one or more portions (P1) of the cover layer (11).
12. The method according to the preceding claim, wherein: The at least one patterned or structured photoresist layer or material (15) is provided directly on the cover layer (11).
13. A method according to claim 11 or 12, wherein: The photolithography process includes a deep ultraviolet (DUV) photolithography process, or consists of a deep ultraviolet photolithography process.
14. The method according to any of the preceding claims, further comprising etching at least one or more exposed portions (P1) of the cover layer (11) to remove the exposed cover layer (11) to expose at least one or more portions (P2) of the at least one diamond-like carbon layer or material (9).
15. The method according to the preceding claim, wherein: The etching is performed by plasma etching.
16. The method according to any one of the preceding claims 11 to 15, further comprising etching the exposed at least one or more portions (P2) of the at least one diamond-like carbon layer or material (9) to expose at least one or more portions (P3) of the at least one adhesion layer (7).
17. The method according to the preceding claim, wherein: The etching is performed by plasma etching.
18. The method according to claim 16 or 17, further comprising etching the at least one patterned or structured photoresist layer or material (15) to remove or completely remove the at least one patterned or structured photoresist layer or material (15).
19. The method according to the preceding claim, wherein: The at least one patterned or structured photoresist layer or material (15) and the at least one diamond-like carbon layer or material (9) are etched simultaneously.
20. The method according to any one of the preceding claims 15 to 17, further comprising etching at least one or more exposed portions (P3) of the at least one adhesion layer (7) to expose at least one or more portions (P4) of the at least one ferroelectric material or layer (3).
21. The method according to the preceding claim, further comprising etching at least one or more exposed portions (P4) of the at least one ferroelectric material or layer (3).
22. The method according to claim 20 or 21, wherein: The etching is performed by ion beam etching.
23. A method according to claim 21 or 22, wherein: The etching is performed to at least partially produce one or more ferroelectric devices or structures, or photonic devices, or integrated photonic devices.
24. The method according to any one of the preceding claims 2 to 23 further comprises etching the at least one diamond-like carbon layer or material (19) deposited on the second side (SD2) of the at least one ferroelectric material or layer (3) to remove or completely remove the at least one diamond-like carbon layer or material (19).
25. The method according to any of the preceding claims, further comprising etching the at least one diamond-like carbon layer or material (9) to remove or completely remove the at least one diamond-like carbon layer or material (9) from the first side (SD1) of the at least one ferroelectric material or layer (3).
26. A method according to claim 24 or 25, wherein: The etching is performed by plasma etching.
27. The method according to the preceding claim, further comprising the step of removing the at least one adhesive layer (7) and / or the at least one further adhesive layer (17).
28. The method according to the preceding claim, wherein: The step of removing the at least one adhesion layer (7) and / or the at least one further adhesion layer (17) at least partially provides a freestanding ferroelectric device or structure (FD).
29. A method according to any one of the preceding claims, wherein: The at least one ferroelectric material or layer (3) comprises lithium niobate (LiNbO3) or single-crystalline lithium niobate (LiNbO3), or consists only of lithium niobate or single-crystalline lithium niobate.
30. The method according to the preceding claim, wherein: The at least one ferroelectric material or layer (3) comprises doped lithium niobate (LiNbO3) or doped single-crystalline lithium niobate (LiNbO3), or consists only of doped lithium niobate or doped single-crystalline lithium niobate.
31. A method according to any one of the preceding claims, wherein: The at least one ferroelectric material or layer (3) comprises lithium tantalate (LiTaO3), or consists only of lithium tantalate.
32. A method according to any one of the preceding claims, wherein: Providing the at least one ferroelectric material or layer (3) comprises providing the ferroelectric material or layer 3 as a wafer or a wafer comprising the ferroelectric material or layer 3, or as a lithium niobate on insulator (LNOI) wafer (5).
33. The method according to the preceding claim, wherein: The lithium niobate on insulator (LNOI) wafer (5) comprises a substrate (5A), at least one oxide layer (5B) provided on the substrate (5A) and at least one lithium niobate (LiNbO3) layer (3) provided on the oxide layer (5B), or consists of a substrate (5A), at least one oxide layer (5B) provided on the substrate (5A) and at least one lithium niobate layer (3) provided on the oxide layer (5B).
34. The method according to the preceding claim, wherein: The lithium niobate on insulator (LNOI) wafer (5) further comprises at least one further oxide layer (5C) provided on the substrate (5A) opposite to the at least one oxide layer (5B).
35. A method according to any one of the preceding claims 31 to 32, wherein: The substrate (5A) includes silicon or consists of silicon.
36. A method according to any one of the preceding claims, wherein: The at least one adhesive layer (7) and the at least one further adhesive layer (17) comprise the same material, or consist of the same material.
37. A method according to any one of the preceding claims, wherein: The at least one adhesion layer (7) and / or the at least one further adhesion layer (17) are configured to prevent delamination of the at least one diamond-like carbon layer or material (9, 19).
38. A method according to any one of the preceding claims, wherein: The at least one adhesive layer (7) and the cover layer (11) comprise the same material, or consist of the same material.
39. A method according to any one of the preceding claims, wherein: The at least one adhesion layer (7) and / or the at least one further adhesion layer (17) comprises or consists of the following material: silicon nitride (Si3N4), silicon oxide (SiO2) or sapphire (Al2O3).
40. A method according to any one of the preceding claims, wherein: The cover layer (11) comprises or consists of the following materials: silicon nitride (Si3N4) or amorphous silicon.
41. A method according to any preceding claim, further comprising the step of providing at least one or more electrodes on said at least one ferroelectric material or layer (3).
42. A method according to any one of the preceding claims, wherein: It also comprises the step of depositing at least one cladding material on said at least one ferroelectric material or layer (3).
43. A method according to any one of the preceding claims, wherein: The method also includes dividing the ferroelectric device or structure (FD) into a plurality of ferroelectric chips or subdivided bodies.
44. A method according to any one of the preceding claims, wherein: The at least one or more ferroelectric devices or structures (FD) include or consist of at least one or more photonic devices or integrated photonic devices.
45. A method according to any one of the preceding claims, wherein: The method is a wafer-free bonding method or an adhesive-free wafer bonding method.
46. A method for producing at least one ferroelectric device or structure (FD), the method comprising the steps of: - providing at least one ferroelectric material or layer (3), or providing at least one ferroelectric material or layer (3) to be patterned or structured; - depositing at least one adhesion layer (7) on the first side (SD1) of the at least one ferroelectric material or layer (3); and - depositing at least one silicon carbon layer or material (9) on said at least one adhesion layer (7).
47. A ferroelectric device or structure (FD), comprising: - at least one ferroelectric material or layer (3), - at least one adhesion layer (7) on the first side (SD1) of the at least one ferroelectric material or layer (3); and - at least one diamond-like carbon layer or material (9) on said at least one adhesion layer (7).
48. The ferroelectric device or structure (FD) according to the preceding claim further comprises at least one additional adhesion layer (17) on the second side (SD2) of the at least one ferroelectric material or layer (3), and at least one diamond-like carbon layer or material (19) on the at least one additional adhesion layer (17) on the second side (SD2) of the at least one ferroelectric material or layer (3).
49. A ferroelectric device or structure according to claim 47 or 48, wherein At least one adhesion layer (7) is in direct contact with at least one ferroelectric material or layer (3).
50. A ferroelectric device or structure according to any one of claims 47 to 49, wherein The at least one diamond-like carbon layer or diamond-like carbon material (9) is in direct contact with the at least one adhesion layer (7).
51. A ferroelectric device or structure according to any preceding claim 47 to 50, wherein: The at least one further adhesion layer (17) is in indirect contact with the at least one ferroelectric material or layer (3).
52. A ferroelectric device or structure according to any one of claims 47 to 50, wherein: The at least one diamond-like carbon layer or diamond-like carbon material (19) is in direct contact with the at least one further adhesion layer (17).
53. A ferroelectric device or structure according to any one of the preceding claims 47 to 52, further comprising at least one covering layer (11) provided on the at least one diamond-like carbon layer or material (9), wherein the at least one diamond-like carbon layer or material (9) is provided on the at least one adhesion layer (7).
54. A ferroelectric device or structure according to any one of claims 47 to 53, wherein: The at least one ferroelectric material or layer (3) comprises lithium niobate (LiNbO3) or single-crystalline lithium niobate (LiNbO3), or consists only of lithium niobate or single-crystalline lithium niobate.
55. A ferroelectric device or structure according to any one of claims 47 to 54, wherein The at least one ferroelectric material or layer (3) comprises doped lithium niobate (LiNbO3) or doped single-crystalline lithium niobate (LiNbO3), or consists only of doped lithium niobate or doped single-crystalline lithium niobate.
56. A ferroelectric device or structure according to any one of claims 47 to 55, wherein The at least one ferroelectric material or layer (3) comprises lithium tantalate (LiTaO3) or consists exclusively of lithium tantalate.
57. A ferroelectric device or structure according to any one of claims 47 to 56, wherein The at least one ferroelectric material or layer (3) comprises or consists of lithium niobate contained in or as part of a lithium niobate on insulator (LNOI) wafer (5).
58. A ferroelectric device or structure according to the preceding claim, wherein The lithium niobate on insulator (LNOI) wafer (5) comprises a substrate (5A), at least one oxide layer (5B) provided on the substrate (5A) and at least one lithium niobate (LiNbO3) layer (3) provided on the oxide layer (5B), or consists of a substrate (5A), at least one oxide layer (5B) provided on the substrate (5A) and at least one lithium niobate layer (3) provided on the oxide layer (5B).
59. A ferroelectric device or structure according to the preceding claim, wherein: The lithium niobate on insulator (LNOI) wafer (5) further comprises at least one further oxide layer (17) provided on the substrate (5A) opposite to the at least one oxide layer (5B).
60. A ferroelectric device or structure according to claim 58 or 59, wherein The substrate (5A) includes silicon or consists of silicon.
61. A ferroelectric device or structure according to any one of claims 47 to 60, wherein: The at least one adhesive layer (7) and the at least one further adhesive layer (17) comprise the same material, or consist of the same material.
62. A ferroelectric device or structure according to any preceding claim 53 to 61, wherein: The at least one adhesive layer (7) and the at least one covering layer (11) comprise the same material, or consist of the same material.
63. A ferroelectric device or structure according to any preceding claim 47 to 62, wherein: The at least one adhesion layer (7) and / or the at least one further adhesion layer (17) comprises or consists of the following material: silicon nitride (Si3N4), silicon oxide (SiO2) or sapphire (Al2O3).
64. A ferroelectric device or structure according to any preceding claim 47 to 63, wherein: The at least one covering layer (11) comprises silicon nitride (Si3N4) or amorphous silicon, or consists of silicon nitride or amorphous silicon.