Display device

By using a resin composition cured film and a through opening pattern structure in an LED display, the problem of insufficient wiring concealment is solved, higher design and visibility are achieved, and problems such as wiring short circuits are avoided.

CN118742939APending Publication Date: 2024-10-01TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380019102.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-04-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing LED display devices have deficiencies in wiring concealment and design. The wiring concealment is insufficient and the design is reduced.

Method used

A cured film containing a resin composition is used. The cured film has a light transmittance of 0.1% or more and 95% or less at a wavelength of 450 nm based on a thickness of 1 μm. It is used to hide wiring and provide an opening pattern penetrating in the thickness direction in the display device. Configure the wiring to ensure the electrical insulation and concealment of the wiring.

Benefits of technology

The wiring concealment and design of the display device are improved, the glare of the wiring is reduced, the visibility and contrast are enhanced, and the problems of wiring short circuit and low back are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742939A_ABST
    Figure CN118742939A_ABST
Patent Text Reader

Abstract

[Problem] To solve the problem that in an LED display device, wiring hiding is not sufficient and the designability is reduced by means of an insulating film or a protective film for insulating peripheral wiring, a partition wall, or the like. [Solution] A display device having at least wiring lines, a cured film, and a plurality of light-emitting elements, in which the light-emitting elements each include electrodes on two different surfaces, at least one of the electrodes is connected to a plurality of the wiring lines extending in the cured film, and at least one of the electrodes is connected to a plurality of the wiring lines extending in the cured film. The plurality of wirings are configured so as to maintain electrical insulation properties by means of the cured film, the cured film is a film obtained by curing a resin composition containing (A) a resin, and the transmittance of light having a wavelength of 450 nm at a thickness reference of 5 [mu] m is 0.1% to 95% (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a display device such as an LED display. Background Art

[0002] In recent years, from the perspective of further improving the performance of displays, as a new display technology following liquid crystal, plasma display, and organic electroluminescence (EL) display, LED displays that form displays by arranging the same number of light emitting diodes (hereinafter referred to as LEDs) as the number of pixels, especially mini LED displays that set the size of LEDs as light sources from the existing 1mm to 100μm to 700μm, and micro LED displays that are miniaturized to less than 100μm have attracted much attention and are being actively researched and developed. The main features of mini LED displays and micro LED displays include high contrast, high-speed responsiveness, low power consumption, and wide viewing angle. They are not only used in existing TVs or smartphones, but also in wearable displays represented by smart watches. It is also expected to be widely used in signage or augmented reality (AR), virtual reality (VR), and transparent displays that can display spatial images.

[0003] Regarding LED display devices, various methods have been proposed for practical application or high performance, including a method of configuring micro LEDs on a multilayer flexible circuit substrate (see Patent Document 1), a method of providing a dam layer and a tracer line on a display substrate and configuring micro LEDs and a micro driver chip thereon (see Patent Document 2). In addition, the following methods have been proposed: forming a planarization film on a growth substrate integrally formed with a light-emitting element body including an electrode pad, removing the planarization film on the electrode pad to expose the electrode pad, forming an outer electrode pad connected to the electrode pad on the planarization film, configuring the outer electrode pad to face the circuit side electrode portion relative to a circuit substrate formed with a circuit side electrode portion, and electrically connecting the front external electrode pad to the circuit side electrode portion (see Patent Document 3).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-153812

[0007] Patent Document 2: Japanese Patent Application Publication No. 2020-52404

[0008] Patent Document 3: Japanese Patent Application Publication No. 2020-68313 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, the LED display device described in the above document has the following problems: the wiring is not sufficiently hidden by the surrounding insulating film or protective film for wiring insulation, partition walls, etc., and the design property is degraded.

[0011] Technical means of solving problems

[0012] In order to solve the above-mentioned problems, the present invention has the following configuration.

[0013] [1] A display device comprising at least wiring, a cured film, and a plurality of light-emitting elements, wherein the light-emitting elements include electrodes on two different surfaces, at least one of the electrodes is connected to the plurality of wirings extending in the cured film, the plurality of wirings are electrically insulating by the cured film, the cured film is a film formed by curing a resin composition containing (A) resin, and the transmittance of the cured film at a wavelength of 450 nm at a thickness of 1 μm is 0.1% or more and 95% or less.

[0014] [2] The display device according to [1], wherein the transmittance of the cured film at a wavelength of 450 nm at a thickness of 5 μm is 0.1% or more and 79% or less.

[0015] [3] The display device according to [1], wherein the transmittance of the cured film at a wavelength of 450 nm at a thickness of 1 μm is 0.1% or more and 25% or less.

[0016] [4] The display device according to any one of [1] to [3], wherein the entire cured film has a thickness of 5 μm or more and 100 μm or less.

[0017] [5] The display device according to any one of [1] to [4], wherein the number of layers of the cured film is 2 or more and 10 or less.

[0018] [6] The display device according to any one of [1] to [5] is a structure in which an opening pattern penetrating in the thickness direction is provided in the cured film, and the wiring is arranged at least in the opening pattern, and the maximum length of the bottom portion of the wiring formed at the position in contact with the light-emitting element is greater than or equal to 2 μm and less than or equal to 20 μm.

[0019] [7] The display device according to any one of [1] to [6], wherein the cured film covers the surface of the light-emitting element other than the light output surface.

[0020] [8] A display device comprising at least a substrate having wiring and / or a thin film transistor (TFT), a cured film, and a plurality of light-emitting elements, wherein the light-emitting elements include electrodes on two different surfaces, at least a portion of the wiring and / or the TFT is in contact with the cured film, the cured film is a film formed by curing a resin composition comprising (A) resin, and the transmittance of the cured film at a wavelength of 450 nm at a thickness reference of 1 μm is 0.1% or more and 95% or less.

[0021] [9] The display device according to any one of [1] to [8], wherein a partition having a thickness greater than that of the light-emitting element is included between the plurality of light-emitting elements.

[0022]

[10] The display device according to any one of [1] to [9], wherein the light-emitting element is an LED having a side length of 5 μm to 700 μm.

[0023]

[11] The display device according to any one of [1] to

[10] further comprises a driving element and a substrate, wherein the driving element is connected to the light-emitting element via wiring, and at least a portion of the wiring extends on a side surface of the substrate.

[0024]

[12] The display device according to any one of [1] to

[11] , wherein a light shielding layer is provided between the plurality of light emitting elements.

[0025]

[13] The display device according to any one of [1] to

[12] , wherein the (A) resin contains one or more resins selected from the group consisting of polyimide, a polyimide precursor, polybenzoxazole, a polybenzoxazole precursor, and copolymers thereof.

[0026]

[14] The display device according to any one of [1] to

[13] , wherein the resin composition containing the (A) resin further contains (B) a photosensitizer.

[0027]

[15] A display device according to any one of [1] to

[14] , wherein the resin composition containing the (A) resin further contains a (C) colorant, and the (C) colorant contains a (C-1) colorant having a maximum absorption in a wavelength range of not less than 400 nm and not more than 490 nm.

[0028]

[16] A display device according to any one of [1] to

[15] , wherein the resin composition containing the (A) resin further contains a (C) colorant, and the (C) colorant contains a (C-2) colorant having a maximum absorption in a wavelength range exceeding 490 nm and not more than 580 nm.

[0029]

[17] A display device according to any one of [1] to

[15] , wherein the resin composition containing the (A) resin further contains a (C) colorant, and the (C) colorant contains a (C-3) colorant having a maximum absorption in a wavelength range of greater than 580 nm and less than 800 nm.

[0030]

[18] A display device according to any one of [1] to

[15] , wherein the (C) colorant contains (C-1) a colorant having a maximum absorption in a wavelength range of greater than 400 nm and less than 490 nm, and further contains (C-2) a colorant having a maximum absorption in a wavelength range of greater than 490 nm and less than 580 nm, and (C-3) a colorant having a maximum absorption in a wavelength range of greater than 580 nm and less than 800 nm.

[0031]

[19] The display device according to any one of [1] to

[18] , wherein the resin composition containing the (A) resin is positive photosensitivity.

[0032] Effects of the Invention

[0033] The display device of the present invention has improved wiring concealability, and can provide a display device with high design properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] [ Figure 1 ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing an example of a first mode of the display device of the present invention.

[0035] [ Figure 1a ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing another example of the first mode of the display device of the present invention.

[0036] [ Figure 2 ] is a cross-sectional view (a) after enlarging the designated area A and a bottom view (b) obtained by observing the surface after removing the light-emitting element from the designated area A from the opposite substrate side.

[0037] [ Figure 3 ] are a cross-sectional view (a) after cutting the light emitting element driving substrate side of the designated area B along a plane parallel to the opposing substrate, a cross-sectional view (b) of the designated area B excluding the position of the wiring orthogonal to the opposing substrate, and a bottom view (c) obtained by observing the surface of the designated area B after removing the opposing substrate from the opposing substrate side.

[0038] [ Figure 4 ] is a cross-sectional view of a surface perpendicular to the facing substrates, showing one mode of the display device of the present invention having a structure with a partition wall.

[0039] [ Figure 5 ] is a cross-sectional view of a surface perpendicular to the opposing substrate of one embodiment of the display device of the present invention having a structure in which a driving element is arranged in a cured film.

[0040] [ Figure 6 ] is a cross-sectional view of a surface perpendicular to the opposing substrates of one embodiment of a display device of the present invention having another structure in which a driving element is arranged in a cured film.

[0041] [ Figure 7 ] is a cross-sectional view of a surface perpendicular to a supporting base or an opposing substrate, showing a manufacturing process of one mode of a display device of the present invention.

[0042] [ Figure 8 ] is a cross-sectional view of a surface perpendicular to a supporting base or an opposing substrate, showing an example of another manufacturing process of the display device of the present invention.

[0043] [ Fig. 9 ] is a cross-sectional view of a surface perpendicular to a supporting base or an opposing substrate, showing an example of another manufacturing process of a display device of the present invention having a structure with a partition wall.

[0044] [ Fig.10 ] is a cross-sectional view of a surface perpendicular to the facing substrates, showing another embodiment of the display device of the present invention.

[0045] [ Fig.11 ] is a cross-sectional view of a surface perpendicular to a supporting base, showing one mode of a display device of the present invention having a structure in which a partition wall is provided in a cured film.

[0046] [ Fig.12 ] is a cross-sectional view of a surface perpendicular to the facing substrates, showing another embodiment of the display device of the present invention.

[0047] [ Fig.13 ] is a cross-sectional view of a surface perpendicular to the facing substrates, showing another embodiment of the display device of the present invention.

[0048] [ Fig.14 ] is a cross-sectional view of a surface perpendicular to the facing substrates, showing another embodiment of the display device of the present invention.

[0049] [ Fig.15 ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing one mode of a display device of the present invention having a structure in which a light-shielding layer is provided.

[0050] [ Fig.16 ] is a cross-sectional view showing the opening pattern of the cured film taken along a plane perpendicular to the support base.

[0051] [ Fig.17 ] is a cross-sectional view taken on a surface perpendicular to a supporting base, showing a manufacturing process of one mode of a display device of the present invention having a structure with a partition wall.

[0052] [ Fig.18 ] is a cross-sectional view of a surface perpendicular to a supporting base, showing a manufacturing process of one mode of a display device of the present invention having a structure having a light-shielding layer.

[0053] [ Fig.19 ] is a cross-sectional view of a surface perpendicular to a light-emitting element driving base, showing an example of a manufacturing process of a display device according to the second embodiment of the present invention.

[0054] [ Fig. 20 ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing one mode of a display device of the present invention using light-emitting elements with different connection methods.

[0055] [ Fig.21 ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing one mode of a display device of the present invention using light-emitting elements with different connection methods.

[0056] [ Fig. 22 ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing one mode of a display device of the present invention using light-emitting elements with different connection methods.

[0057] [ Fig.23 ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing one mode of a display device of the present invention using light-emitting elements with different connection methods.

[0058] [ Fig.24 ] is a cross-sectional view of a surface perpendicular to the opposing substrates, showing one mode of a display device of the present invention using light-emitting elements with different connection methods.

[0059] [ Fig.25 ] is a cross-sectional view taken along a plane perpendicular to an element driving substrate, showing an example of a second embodiment of the display device of the present invention.

[0060] [ Fig.26 ] is a cross-sectional view taken along a plane perpendicular to an element driving substrate, showing an example of a second embodiment of the display device of the present invention.

[0061] [ Fig. 27 ] is a cross-sectional view taken along a plane perpendicular to an element driving substrate, showing an example of a second embodiment of the display device of the present invention.

[0062] [ Fig.28 ] is a cross-sectional view of a surface perpendicular to the supporting substrate, showing another example of the second embodiment of the display device of the present invention using a light-emitting element with a different connection method.

[0063] [ Fig.29 ] is a cross-sectional view of a surface perpendicular to a light-emitting element driving substrate, showing an example of a manufacturing process of a display device according to the second embodiment of the present invention. DETAILED DESCRIPTION

[0064] Hereinafter, preferred embodiments of the display device of the present invention will be described in detail, but the present invention is not limited to the following embodiments and can be implemented with various modifications depending on the purpose and application.

[0065] A first embodiment of the display device of the present invention is a display device comprising at least wiring, a cured film, and a plurality of light-emitting elements, wherein the light-emitting elements include electrodes on two different surfaces, at least one of the electrodes is connected to the plurality of wirings extending in the cured film, the plurality of wirings are structures in which electrical insulation is maintained by the cured film, the cured film is a film formed by curing a resin composition containing (A) resin, and the transmittance of the cured film at a wavelength of 450 nm at a thickness reference of 1 μm is greater than or equal to 0.1% and less than or equal to 95%.

[0066] In the following description, unless the first embodiment or the second embodiment described later is particularly specified, the description is common to both embodiments.

[0067] Regarding the display device of the first aspect of the present invention, Figure 1 This will be described as an example.

[0068] exist Figure 1 In the display device 1, a plurality of light-emitting elements 2 are arranged on the facing substrate 5, and a cured film 3 is arranged on the light-emitting element 2. Here, the light-emitting element has a multi-faceted three-dimensional shape. The multi-faceted three-dimensional shape is a three-dimensional shape having multiple faces, preferably having at least one pair of parallel faces, for example, tetrahedrons, cuboids or cubes such as hexahedrons, octahedrons, etc., but it is not limited to regular shapes such as these, and also includes shapes after the vertices or edges of these shapes are chamfered, etc., and shapes with concave portions, grooves or step differences based on these shapes. In addition, here, the offset of plus or minus 5° is regarded as parallel, and it is also possible to have concave and convex on parallel faces or other faces. The light-emitting element includes electrodes on two different faces. The so-called electrodes are respectively included on two different faces, which means that in the light-emitting element of the multi-faceted three-dimensional shape, when one of the faces having electrodes is used as the reference plane, other electrodes are respectively provided on faces different from the reference plane. Here, the so-called reference plane represents a continuous range of faces within the multi-faceted three-dimensional shape. Even if it exists in the same plane in space, the face divided by the groove in the multi-faceted three-dimensional shape is set as a face different from the reference plane. Furthermore, when focusing on one light-emitting element, the electrodes respectively included on the two different surfaces may be described as a pair of electrodes.

[0069] In the present invention, the electrode included in the light emitting element refers to a connection portion for transmitting a signal, that is, a signal for controlling the light emission of the light emitting element, from a wiring to the light emitting element. Figure 1 In the illustrated embodiment, when focusing on one light-emitting element, the light-emitting element having a multi-faceted three-dimensional shape has one electrode on the surface connected to the wiring 4 extending in the cured film 3, and has the other electrodes on the surface facing the substrate side. Furthermore, when viewed as a whole, one electrode of a pair of electrodes provided in each of the plurality of light-emitting elements is connected to the plurality of wirings 4 extending in the cured film 3.

[0070] exist Figure 1 In the illustrated embodiment, a structure in which a plurality of cured films 3 are further stacked on a cured film 3 configured to be in contact with at least a portion of the light-emitting element 2, and a total of three layers of cured films 3 are stacked is illustrated, but the cured film 3 may also be a single layer. The light-emitting element 2 includes electrodes 6 on two different surfaces, respectively, and one of a pair of electrodes 6 is connected to a wiring 4 extending in the cured film 3. In addition, the plurality of wirings 4 extending in the cured film 3 are separated by the cured film 3. With this structure, the plurality of wirings 4 are electrically insulated by the cured film 3. The cured film 3 is preferably a cured film formed by curing a resin composition containing the (A) resin described later.

[0071] One of the pair of electrodes 6 that is not connected to the wiring 4 extending in the cured film 3 is connected to the wiring 4d. The wiring 4d may be formed on the supporting substrate described later, or may be formed on the opposing substrate 5. When the wiring 4d is formed on the supporting substrate, the wiring 4d may be formed after a temporary adhesive layer is formed on the supporting substrate using a temporary adhesive material. The electrode 6 and the wiring 4d may be connected via a bump or a conductive film, or may be directly connected.

[0072] In addition, the wiring 4d may be a structure that maintains electrical insulation by being covered with the cured film 3, or a stacked structure of two or more layers may be formed by using the cured film 3 and the wiring 4d. The wiring 4d may be connected to the wiring 4 extending in the cured film 3 arranged to be in contact with at least a portion of the light-emitting element 2 via a through electrode or the like, or may be arranged on the side of the light-emitting element 2 or the side of the partition 16 described later and connected to the wiring 4 extending in the cured film 3, or may be connected to the light-emitting element driving substrate 7. Furthermore, the light-emitting element 2 is electrically connected to the driving element 8 attached to the light-emitting element driving substrate 7 disposed at a position facing the opposing substrate 5 via the wiring 4 or the wiring 4c, so that the light emission of the light-emitting element 2 can be controlled. In addition, the light-emitting element driving substrate 7 is electrically connected to the wiring 4, for example, via the bump 10. Furthermore, in order to prevent the diffusion of metal such as the wiring 4, a barrier metal 9 may also be arranged. In addition, the wiring 4c in the figure can be formed on the side of the light emitting element driving substrate 7, or can pass through the light emitting element driving substrate 7. In addition, it can also be connected to the driving element 8 in the form of wiring constituting the light emitting element driving substrate.

[0073] exist Figure 1 The following example is shown: the wiring 4d and the electrode 6 are arranged between the counter substrate 5 and the light emitting element 2, and the cured film 3 is arranged between the counter substrate 5 and the light emitting element 2 in a form adjacent to the wiring 4 and the electrode 6. However, this embodiment also includes the following: the wiring 4 and the electrode 6 are formed in a form covering the entire plane of the light emitting element 2, and the cured film 3 is not arranged between the counter substrate 5 and the light emitting element 2; or the wiring 4 and the electrode 6 are formed in the form of a thin film. Figure 1 In the case of the wiring 4 and the electrode 6 shown, the resin film 21 described later cannot completely enter the vicinity of the wiring 4 and the electrode 6, and the cured film 3 cannot be formed between the counter substrate 5 and the light emitting element 2, resulting in local voids.

[0074] It is important that the cured film 3 has a transmittance of 0.1% to 95% at a wavelength of 450 nm at a thickness of 1 μm. Thus, the cured film 3 hides the wiring 4, suppresses glare of the wiring 4, and makes it difficult to be seen from the outside, thereby improving the design.

[0075] Preferably, the cured film 3 is a film formed by curing a resin composition containing the resin (A) described later, and the transmittance of the cured film 3 at a wavelength of 450 nm at a thickness reference of 5 μm is 0.1% or more and 79% or less. Thus, the cured film 3 hides the wiring 4, suppresses the glare of the wiring 4, and makes it difficult to be seen from the outside, thereby improving the design.

[0076] Preferably, the cured film 3 is a film formed by curing a resin composition containing the resin (A) described later, and the transmittance of the cured film 3 at a wavelength of 450 nm at a thickness reference of 1 μm is 0.1% or more and 25% or less. Thus, the cured film 3 hides the wiring 4, suppresses the glare of the wiring 4, and makes it difficult to be seen from the outside, thereby improving the design, and further, by reducing the reflection of external light or improving the contrast, the visibility can be improved.

[0077] If the transmittance of the cured film 3 at a wavelength of 450 nm at a thickness of 1 μm is less than 0.1%, there is a concern that the sensitivity or resolution of the resin film before curing may be reduced. If the transmittance exceeds 95%, the wiring concealment property may be reduced, the glare of the wiring may not be sufficiently suppressed, and there is a concern that the wiring may be visible from the outside.

[0078] Regarding the determination of the transmittance of light of a wavelength of 450nm under a thickness reference of 1μm of the cured film, the transmittance of light of the cured film produced under the conditions of the evaluation method of the transmittance of light of the cured film described later can be measured. In addition, in the case of forming a multilayer cured film, any cured film can be used for measurement. Regarding the determination of the transmittance of light of a wavelength of 450nm under a thickness reference of 5μm of the cured film, it is also the same as the determination of the transmittance of light of a wavelength of 450nm under a thickness reference of 1μm of the cured film. In the case where the film thickness of the cured film is not 1μm, it is sufficient to convert the film thickness of the measured transmission spectrum to a value of 1μm according to Lambert's law. In addition, in the case where the film thickness of the cured film is not 5μm, it is sufficient to convert it according to Lambert's law, as in the case where the film thickness of the cured film is not 1μm.

[0079] The materials of the wiring 4 , the wiring 4 c , the wiring 4 d , and the electrode 6 are not particularly limited, and metals, conductive films, and the like may be mentioned, and existing materials may be used.

[0080] From the viewpoint of electron mobility, metals are preferred, and examples thereof include gold, silver, copper, aluminum, nickel, titanium, molybdenum, and alloys containing these.

[0081] These metals can be formed, for example, by wet plating such as electroless plating, electroplating, etc.; CVD chemical vapor deposition (CVD), plasma CVD, laser CVD, etc.; dry plating methods such as vacuum evaporation, sputtering, ion plating, etc., in which the metal foil is bonded to the substrate and then etched.

[0082] From the viewpoint of transparency, etc., a conductive film is preferred, for example, a compound containing an oxide of at least one element selected from the group consisting of indium, gallium, zinc, tin, titanium, and niobium as a main component; or a photosensitive conductive paste containing an organic substance and conductive particles, etc., but other existing ones may also be used. Regarding the compound containing an oxide of at least one element selected from the group consisting of indium, gallium, zinc, tin, titanium, and niobium as a main component, specifically, indium tin zinc oxide (ITZO), indium gallium zinc oxide (IGZO: InGaZnO), zinc oxide (ZnO), indium zinc oxide (IZO), indium gallium oxide (IGO), indium tin oxide (ITO), and indium oxide (InO), etc.

[0083] These conductive films can be formed, for example, by wet plating such as electroless plating, electroplating, etc.; CVD chemical vapor deposition (CVD) such as thermal CVD, plasma CVD, laser CVD, etc.; dry plating methods such as vacuum evaporation, sputtering, ion plating, etc., in which the metal foil is bonded to the substrate and then etched.

[0084] In the photosensitive conductive paste containing organic matter and conductive particles, the content of conductive particles is preferably 60% by mass or more and 90% by mass or less. By containing organic matter in the conductive layer, wire breakage can be suppressed in the curved surface or the bent portion, thereby improving the conductivity. If the content of conductive particles is less than 60% by mass, the probability of contact between the conductive particles becomes low, and the conductivity is reduced. In addition, in the bent portion of the wiring, the conductive particles are easy to deviate from each other. The content of conductive particles is preferably 70% by mass or more. On the other hand, if the content of conductive particles exceeds 90% by mass, it is difficult to form a wiring pattern, and wire breakage is likely to occur in the curved portion. The content of conductive particles is preferably 80% by mass or less.

[0085] Examples of organic substances include epoxy resins, phenoxy resins, acrylic copolymers, epoxy carboxylate compounds, and the like. Two or more of these may be contained. In addition, organic substances having carbamate bonds may be contained. By containing organic substances having carbamate bonds, the flexibility of the wiring can be improved. In addition, the organic substance preferably exhibits photosensitivity, so that a fine wiring pattern can be easily formed by photolithography. Photosensitivity is manifested, for example, by containing a photopolymerization initiator or a component having an unsaturated double bond.

[0086] The conductive particles in the present invention are particles having a resistivity of 10 -5Particles of a substance with a resistance of Ω·m or less. Examples of materials constituting the conductive particles include silver, gold, copper, platinum, lead, tin, nickel, aluminum, tungsten, molybdenum, chromium, titanium, indium, or alloys of these metals, and carbon particles. In addition, it is preferred to contain two or more conductive particles. By containing two or more conductive particles, in the heat treatment step described later, it is possible to suppress the sintering of the same type of conductive particles to each other and the volume shrinkage, and as a result, the volume shrinkage of the conductive film as a whole can be suppressed, and the flexibility can be improved.

[0087] The average particle size of the conductive particles is preferably 0.005 μm or more and 2 μm or less. The so-called average particle size here refers to the average particle size of the large-diameter particles when containing two or more conductive particles. If the average particle size of the conductive particles is 0.005 μm or more, the interaction between the conductive particles can be appropriately suppressed, and the dispersed state of the conductive particles can be maintained more stably. The average particle size of the conductive particles is more preferably 0.01 μm or more. On the other hand, if the average particle size of the conductive particles is 2 μm or less, it is easy to form the desired wiring pattern. The average particle size of the conductive particles is more preferably 1.5 μm or less.

[0088] The thickness of the conductive film is preferably 2 μm or more and 10 μm or less. If the thickness of the conductive film is 2 μm or more, the disconnection of the bent portion can be further suppressed, and the conductivity can be further improved. The thickness of the conductive film is more preferably 4 μm or more. On the other hand, if the thickness of the conductive film is 10 μm or less, the wiring pattern can be more easily formed in the manufacturing process. The thickness of the conductive film is more preferably 8 μm or less.

[0089] As another embodiment of the display device of the present invention, the following is exemplified. Fig.10 As shown relative to Figure 1 The display device is provided with a structure in which a cured film 21 is arranged in contact with at least a part of the light-emitting element 2. The cured film 21 arranged in contact with at least a part of the light-emitting element 2 may include a cured film formed by curing a resin composition or a resin sheet containing the (A) resin, and may also contain materials other than the cured film formed by curing a resin composition or a resin sheet containing the (A) resin, and existing materials such as epoxy resin, silicone resin, and fluororesin can be used.

[0090] In the present invention, the light emitting element driving substrate 7 may be a substrate including an element having a driving function, and the like, and preferably the driving element 8 is connected thereto.

[0091] The light emitting element driving substrate 7 is not particularly limited, and an existing light emitting element driving substrate can be used. For example, a glass substrate, a sapphire substrate, a printed wiring board, a TFT array substrate, ceramics, etc. can be listed. Regarding the glass substrate and the sapphire substrate, wiring can be formed on at least one surface. When a printed wiring board is used, it can be connected to the driving element 8 or the bump 10, the wiring 4, etc. without forming the wiring 4c.

[0092] In the present invention, it is preferable that the thickness of the entire cured film is 5 μm or more and 100 μm or less.

[0093] Since the overall thickness of the cured film is 5 μm or more and 100 μm or less, the light transmittance of the cured film 3 is low, so the cured film 3 hides the wiring 4, which can suppress the glare of the wiring 4 and make it difficult to be seen from the outside, thereby improving the design. Furthermore, it is possible to suppress wiring defects such as wiring short circuits caused by the low profile of the display device itself with light-emitting elements and the shortened wiring distance, or suppress low losses, and improve high-speed responsiveness. In addition, visibility can also be improved by reducing external light reflection or increasing contrast.

[0094] The thickness of the entire cured film refers to the thickness of the entire layer of the cured film in which at least a portion of one cured film is connected to another cured film. Figure 1 When a plurality of cured films 3 are stacked, Figure 1 The range shown in 20 is the thickness of the entire layer of the cured film. The overall thickness is preferably 5 μm or more and 70 μm or less, and more preferably 5 μm or more and 60 μm or less. If it is less than 5 μm, the protection of the wiring is insufficient, so there is a concern about wiring defects such as wiring short circuits. If it exceeds 100 μm, there is a concern about insufficient light output efficiency, and there is a possibility of poor wiring such as wiring short circuits caused by the low profile of the display device itself and the shortened wiring distance, or in suppressing low losses and improving high-speed responsiveness.

[0095] When laminating a plurality of cured films, the number of layers of the cured films is preferably 2 or more and 10 or less.

[0096] From the viewpoint of configuring a plurality of light-emitting elements, the cured film is preferably one layer or more, and by setting it to two layers or more, the number of wirings that can be connected to the light-emitting elements can be increased, so that a plurality of light-emitting elements can be configured. In addition, from the viewpoint of suppressing wiring defects such as wiring short circuits caused by low-profile packaging or short-distance wiring, achieving low losses, and improving high-speed responsiveness, the cured film is preferably 10 layers or less.

[0097] In the present invention, it is preferred that an opening pattern penetrating in the thickness direction is provided in the cured film, and the wiring is arranged at least in the opening pattern, and the longest length of the bottom portion of the wiring formed at a position in contact with the light emitting element is 2 μm to 20 μm.

[0098] exist Figure 2 shown in the Figure 1 The enlarged cross-sectional view (a) of the designated area A and the bottom view (b) obtained by observing the surface after the light-emitting element is removed from the designated area A from the opposite substrate side. Figure 2 In the cross-sectional view (a) of the enlarged designated area A, the cured film 3 is provided on the light emitting element 2. The figure shows that the cured film 3 is provided with an opening pattern 12 and the wiring 4 is formed in the opening pattern 12. The bottom portion 13 of the wiring 4 shows the wiring 4 extending in the cured film 3 to the position in contact with the electrode 6 of the light emitting element 2 and the wiring 4 at the contacting location.

[0099] exist Figure 2 In the bottom view (b) obtained by observing the surface after the light-emitting element is removed from the designated area A from the opposite substrate side, the bottom portion 13 of the wiring 4 extending in the cured film 3 is observed from below in a state where the light-emitting element 2 is removed, and the bottom portion 13 is shown. Figure 2 In the bottom view (lower part) of the designated area A after the light-emitting element is removed, the bottom portion 13 of the wiring 4 extending in the cured film 3 is observed from below in a state where the light-emitting element 2 is removed, and the bottom portion 13 is shown. The shape of the bottom portion 13 may differ depending on the product or the form of the light-emitting element. In the case of a circular shape, the diameter is defined as the longest length 14, in the case of an elliptical shape, the major diameter is defined as the longest length 14, and in the case of a polygon such as a rectangle, the longest diagonal line connecting the vertices of the corners is defined as the longest length 14. In addition, regarding Figure 2 The bottom portion 13 in the bottom view (b) obtained by removing the light-emitting element from the designated area A as viewed from the opposing substrate side shows an example of a circular shape.

[0100] Through this structure, tiny light-emitting elements can be applied. In addition, high-density packaging of multiple light-emitting elements can be performed, and a display device with a light-emitting element with a large size and high resolution can be obtained. Furthermore, fine wiring can be formed, and the number of wirings that can be formed per unit area increases, so the overall thickness of the cured film can be reduced. The light transmittance of the cured film 3 is low, so the cured film 3 hides the wiring 4, which can suppress the glare of the wiring 4 and make it difficult to be viewed from the outside, thereby improving the design. Furthermore, it is possible to suppress wiring defects such as wiring short circuits caused by the low profile of the display device itself with light-emitting elements and the shortening of the wiring distance, or suppress low losses, and improve high-speed responsiveness. In addition, visibility can also be improved by reducing external light reflection or increasing contrast.

[0101] In the present invention, the longest length of the bottom portion of the wiring formed at a position close to the light-emitting element is preferably greater than 2 μm and less than 20 μm. By adopting the present structure, tiny light-emitting elements can be applied. In addition, high-density packaging of multiple light-emitting elements can be performed, and a display device with a light-emitting element with a large size and high resolution can be obtained. Furthermore, fine wiring can be formed, and the number of wirings that can be formed per unit area increases, so the overall thickness of the cured film can be reduced. The light transmittance of the cured film 3 is low, so the cured film 3 hides the wiring 4, which can suppress the glare of the wiring 4, making it difficult to be viewed from the outside, thereby improving the design. Furthermore, it is possible to suppress wiring defects such as wiring short circuits caused by the low profile of the display device having the light-emitting element itself and the shortened wiring distance, or suppress low losses, and improve high-speed responsiveness. In addition, visibility can also be improved by reducing external light reflection or increasing contrast.

[0102] From the perspective of applying tiny light-emitting elements and high-density packaging of light-emitting elements, the longest length of the bottom portion of the wiring is preferably 2 μm to 15 μm, more preferably 2 μm to 10 μm, and even more preferably 2 μm to 5 μm. If it is less than 2 μm, poor connection with the light-emitting element 2 may occur, and if it exceeds 20 μm, the application of tiny light-emitting elements or high-density packaging may be hindered.

[0103] The thickness of the cured film is preferably 1.1 times or more and 20.0 times or less with respect to the thickness of the wiring.

[0104] The thickness of the wiring is Figure 2The cross-sectional view (a) after enlarging the designated area A is used to illustrate, which refers to the thickness a of the wiring 4 arranged on the surface of the cured film 3, and does not include the thickness of the wiring 4b extending in the opening pattern that penetrates the cured film 3 in the thickness direction. The thickness of the wiring is preferably greater than 0.1μm and less than 10μm, and more preferably greater than 3μm and less than 10μm. By setting the thickness of the wiring to greater than 0.1μm and less than 10μm, it is possible to suppress wiring defects such as wiring short circuits caused by the low profile of the display device itself with light-emitting elements and the shortening of the wiring distance, or to suppress low losses, thereby improving high-speed responsiveness. Furthermore, by setting it to greater than 3μm and less than 10μm, the wiring resistance can be reduced, which can help to suppress power consumption or increase brightness.

[0105] The thickness of the hardened film is Figure 2 In the description of the cross-sectional view (a) of the enlarged designated area A, it refers to the thickness of the cured film 3a covering the wiring 4a.

[0106] Thereby, it also functions as a protective film for appropriate wiring, and the cured film with excellent reliability in which wiring failures such as wiring short circuit are suppressed can be obtained.

[0107] The thickness of the wiring may be the same or different in each layer. In different cases, as an example, it is preferred that: Figure 1 The thickness of the wiring near the bump 10 is thicker than the thickness of the wiring near the light emitting element 2. Therefore, when the light emitting element driving substrate 7 is connected using the bump 10, wiring defects can be suppressed, and a highly reliable display device can be obtained.

[0108] In the present invention, the cured film preferably covers the surface of the light emitting element except the light output surface. In addition, even if a part of the surface of the light emitting element is covered by the cured film, as long as there is a region where light is output, it is also the light output surface.

[0109] As an example, in Figure 3 The figure shows a plane cut parallel to the opposing substrate. Figure 1 A cross-sectional view (a) of a designated area B after the light emitting element is driven by a substrate, a cross-sectional view (b) of the designated area B excluding the position of the wiring orthogonal to the opposing substrate, and a bottom view (c) of the designated area B obtained by removing the opposing substrate from the opposing substrate side.

[0110] exist Figure 3 In the cross-sectional view (a) obtained by cutting the light-emitting element driving substrate side of the designated area B with a plane parallel to the opposing substrate, the light-emitting element 2 is covered with a cured film 3, and the wiring 4 connected to the electrode 6 of the light-emitting element and extending in the cured film 3 is shown from the upper surface. The cross-sectional shape of the wiring 4 may be circular or polygonal.

[0111] exist Figure 3 In the cross-sectional view (b) not including the position of the wiring perpendicular to the counter substrate, it is shown that the periphery of the light emitting element 2 is covered with the cured film 3 .

[0112] exist Figure 3 In the bottom view (c) obtained by observing the surface of the designated area B from the opposite substrate side after removing the opposite substrate, the light-emitting element 2 is covered with the cured film 3, and the other electrode 6 of the light-emitting element is shown from the bottom surface. The cross-sectional shape of the electrode 6 can be circular or polygonal. The light-emitting element 2 can be covered with the cured film 3 except for the electrode 6. In the above case, the light output surface is the surface where the electrode 6 is arranged.

[0113] By setting Figure 1 and Figure 3 As shown, the light emitting element 2 can be protected from external impact by covering the entire side and upper surface of the light emitting element 2 with the cured film 3. In addition, the step difference caused by the arrangement of the light emitting element 2 can be flattened, and it is easy to bond with the opposing substrate 5, which is preferred.

[0114] The cured film 3 covering the surface of the light emitting element 2 other than the light output surface has such high wiring concealment property, and can suppress the glare of the wiring 4 and make it difficult to be seen from the outside, thereby improving the design property.

[0115] The display device of the second embodiment of the present invention is a display device comprising at least a substrate having wiring and / or TFT, a cured film, and a plurality of light-emitting elements, wherein the light-emitting elements include electrodes on two different surfaces, at least a portion of the wiring and / or TFT is in contact with the cured film, the cured film is a film formed by curing a resin composition containing (A) resin, and the transmittance of the cured film at a wavelength of 450nm at a thickness reference of 1μm is greater than 0.1% and less than 95%.

[0116] Regarding the display device of the second embodiment of the present invention, Fig.25 This will be described as an example.

[0117] exist Fig.25 In the display device 1, the cured film 3 is arranged so that at least a portion of the substrate having wiring and / or TFT is in contact with the cured film 3. The substrate having wiring and / or TFT is, for example, a light emitting element driving substrate 7, and a TFT array substrate having wiring 4 is taken as an example.

[0118] Next, after wiring 4e is arranged on at least a portion of the surface of cured film 3 and a portion of the opening pattern of cured film 3, light emitting element 2 including electrodes on two different surfaces is arranged on wiring 4e.

[0119] exist Fig.25 In the illustrated embodiment, it is shown that for a light-emitting element of a multi-faceted three-dimensional shape, one of the electrodes is provided on the surface connected to the wiring 4e, and the other electrodes are provided on the surface on the opposite substrate side. In addition, a structure in which a cured film 3 is provided between or around the light-emitting elements 2 is illustrated. One electrode 6 of a pair of electrodes 6 that is not connected to the wiring 4e is connected to the wiring 4d. The wiring 4d can be formed on the opposite substrate 5. The electrode 6 and the wiring 4d can be connected via a bump or a conductive film, or can be directly connected. The wiring 4d can be connected to the wiring 4 extending in the cured film 3 arranged to be in contact with at least a part of the light-emitting element 2 via a through electrode, etc., or can be connected to the wiring 4e by arranging the wiring on the side of the light-emitting element 2 or the side of the cured film 3 described later, or can be connected to the light-emitting element driving substrate 7. Furthermore, the light-emitting element 2 is electrically connected to the driving element 8 attached to the light-emitting element driving substrate 7 arranged at a position facing the opposite substrate 5 via the wiring 4 or the wiring 4c, so that the light emission of the light-emitting element 2 can be controlled. In addition, the light emitting element driving substrate 7 is electrically connected to the wiring 4, for example, via the bump 10. Furthermore, in order to prevent the diffusion of metal such as the wiring 4, a barrier metal 9 may also be arranged. In addition, the wiring 4c in the figure may be formed on the side of the light emitting element driving substrate 7, may penetrate the light emitting element driving substrate 7, and may also be connected to the driving element 8 in the form of wiring constituting the light emitting element driving substrate.

[0120] As another example of the display device according to the second aspect of the present invention, for example, Figure 26 to Figure 28 The structure shown.

[0121] In the display device of the second embodiment of the present invention, the thickness of the entire cured film is preferably 1 μm or more and 20 μm or less. By making the thickness of the entire cured film 1 μm or more and 20 μm or less, the light emitted from the light emitting element 2 in all directions is suppressed from being absorbed in the cured film 3, and the light output efficiency can be improved, thereby improving the brightness. Furthermore, it is possible to suppress wiring defects such as wiring short circuits caused by the low profile of the display device itself having the light emitting element and the shortened wiring distance, or suppress low losses, thereby improving high-speed responsiveness.

[0122] In the second aspect of the present invention, the thickness of the entire cured film refers to the thickness of the entire layer of the cured film in which at least a portion of one cured film is connected to another cured film. Fig.25 The range shown in 20 is the thickness of the entire layer of the cured film. The overall thickness is preferably 1 μm or more and 10 μm or less, and more preferably 1 μm or more and 5 μm or less. If it is less than 1 μm, the protection of the wiring is insufficient, so there is a concern about wiring defects such as wiring short circuits. If it exceeds 10 μm, it is difficult to form fine wiring, and there is a possibility of poor wiring such as wiring short circuits.

[0123] In the present invention, it is preferable that a partition wall having a thickness equal to or greater than a thickness of the light emitting element is provided between the plurality of light emitting elements.

[0124] Preferably Figure 4 As shown, a repetitive pattern corresponding to the number of pixels of a display device 1 having light-emitting elements 2, that is, a partition wall 15 is provided between or around each light-emitting element 2. The electrode 6 and the wiring 4 or the wiring 4d can be connected via a bump or a conductive film, or can be directly connected. With the above structure, it is easy to bond with the opposing substrate 5 which can also include the wiring 4d, so it is preferred.

[0125] The thickness of the partition wall is preferably larger than the thickness of each light-emitting element, and specifically, is preferably 5 μm or more and 120 μm or less.

[0126] The partition wall may include a cured film formed by curing a resin composition containing the resin (A), and may also contain materials other than the resin composition containing the resin (A), and existing materials such as epoxy resin, (meth) acrylic polymer, polyurethane, polyester, polyolefin, polysiloxane, etc. may be used. By using these materials, a partition wall with excellent adhesion can be formed.

[0127] In order to suppress light leakage from the light emitting element or color mixing between pixels and improve contrast, a light shielding portion may be provided on the side of the partition or on the partition itself. The light shielding portion is, for example, a portion containing black pigment or the like.

[0128] Furthermore, in order to reflect the light emitted from the light emitting element toward the partition wall to improve the light extraction efficiency and brightness, a reflective portion may be provided on the side of the partition wall. The reflective portion is, for example, a portion containing white pigment or the like.

[0129] It is preferable that a partition wall having a thickness equal to or greater than that of the light emitting element is disposed between the plurality of light emitting elements in the cured film covering the light emitting element.

[0130] As another embodiment of providing a partition wall, the following is exemplified. Fig.11 As shown in the figure, in the cured film 3 covering the light emitting element 2 , the partition wall 15 is provided between the light emitting elements 2 or around them.

[0131] Fig.11 The partition wall shown in the figure may contain materials other than the resin composition containing the resin (A), and existing materials such as epoxy resin, (meth)acrylic polymer, polyurethane, polyester, polyolefin, polysiloxane, etc. can be used. By using these materials, a partition wall with excellent adhesion can be formed.

[0132] By configuring the next wall, it can be used as a mark when the light-emitting element is transferred later, and it can also be used as a photospacer, so the efficiency of the light-emitting element transfer can be improved, so it is preferred. Furthermore, in order to suppress light leakage from the light-emitting element or color mixing between pixels and improve contrast, a shading portion can also be provided on the side of the next wall or the next wall itself. The shading portion is, for example, a portion containing black pigment.

[0133] In order to reflect the light emitted from the light emitting element toward the partition wall to improve the light extraction efficiency and brightness, a reflective portion may be provided on the side of the partition wall. The reflective portion is, for example, a portion containing white pigment.

[0134] In the present invention, a light diffusion layer may be provided around the light emitting element, the cured film, or the wiring.

[0135] In the present invention, the light emitting element is preferably an LED having a side length of 5 μm to 700 μm, and more preferably an LED having a side length of 5 μm to 100 μm.

[0136] LED is constructed by PN junction of P-type semiconductor and N-type semiconductor. When forward voltage is applied to LED, electrons and holes move in the chip, so that current flows. At this time, energy difference is generated by the combination of electrons and holes, and the remaining energy is converted into light energy, thereby emitting light. The wavelength of light emitted from LED varies depending on the compound that constitutes the semiconductor, such as GaN, GaAs, InGaAlP, GaP, etc., and the difference in wavelength determines the color of the light. In addition, white is usually displayed by mixing two or more different colors of light, but in the case of LED, by mixing the three primary colors of red, green, and blue, the color reproducibility is greatly improved, and a more natural white can be displayed.

[0137] As the shape of the LED, a shell shape, a chip shape, a polygonal shape, etc. can be listed, but from the viewpoint of miniaturization of the LED, a chip shape or a polygonal shape is preferred. In addition, since the length of one side of the LED is 5 μm or more and 700 μm or less, a plurality of chips can be arranged, and therefore, the length of one side of the LED is preferably 5 μm or more and 100 μm or less.

[0138] In addition, the light emitting element includes electrodes on two different surfaces. The two different surfaces mean that for a light emitting element having two or more surfaces, when one of the surfaces having electrodes is used as a reference surface, other electrodes are provided on surfaces different from the reference surface.

[0139] In the present invention, it is preferred that electrodes are respectively included on the surfaces facing each other across the light emitting element. In addition, it is preferred that electrodes are respectively included on the adjacent surfaces of the light emitting element. Examples of the light emitting element having electrodes respectively on two different surfaces include: Figure 1 or Fig. 20 As an example of a structure in which electrodes 6 are arranged on the surfaces facing each other across the light emitting element 2, the following examples can be cited as examples of a structure in which electrodes are respectively included on adjacent surfaces of the light emitting element: Fig.21 By including electrodes on the surfaces facing each other across the light emitting element or on the surfaces adjacent to the light emitting element, the size of the light emitting element can be reduced, and a high-resolution display device can be obtained by cost reduction or high-density packaging.

[0140] In the present invention, it is preferred that electrodes are included on discontinuous surfaces. The so-called discontinuous surface includes a surface with a step difference that is not a continuous surface, for example, Figure 22 to Figure 24 By including the electrode 6 on the discontinuous surface, the light-emitting area in the light-emitting element can be controlled, and the productivity or light-emitting efficiency of the light-emitting element can be improved. Regarding the packaging method of the light-emitting element to a substrate such as a light-emitting element driving substrate 7 provided with a cured film 3, for example, a pick and place method or a mass transfer method has been proposed, but it is not limited to these.

[0141] Regarding the packaging of light-emitting elements to the substrate, for example, there can be listed: a method of arranging light-emitting elements that emit red, green, and blue light in a matrix and packaging them in a specified position of the substrate; or a method of arranging and packaging a single type of light-emitting element such as a light-emitting element that emits red or blue light or an ultraviolet light-emitting element that emits ultraviolet light on a substrate. The former method can use light-emitting elements that emit red, green, and blue light, respectively, or can use light-emitting elements that stack light-emitting elements that emit red, green, and blue light longitudinally. The latter method can easily arrange and package light-emitting elements. In the case described, wavelength conversion materials such as quantum dots can be used to make red, green, and blue sub-pixels, and set to full-color display. Furthermore, after packaging two or more light-emitting elements, they can be packaged in a substrate.

[0142] As the wavelength conversion material, an existing wavelength conversion material can be used.

[0143] For example, when a light-emitting element emitting blue light is used, it is preferred that: first, a light-emitting element array substrate on which only light-emitting elements emitting blue light are arranged and packaged is manufactured, and secondly, a wavelength conversion layer that is excited by blue light and converts the wavelength to red or green light and emits light is arranged at positions corresponding to red and green sub-pixels. Thus, red, green, and blue sub-pixels can be formed using only light-emitting elements emitting blue light.

[0144] On the other hand, when using ultraviolet light-emitting elements that emit ultraviolet light, it is preferred that: first, a light-emitting element array substrate on which only ultraviolet light-emitting elements are arranged and packaged is manufactured, and wavelength conversion layers that are excited by ultraviolet light and converted into red, green, and blue light and emit light are arranged at positions corresponding to red, green, and blue sub-pixels. In this way, the difference in the radiation angle of light based on the color of the sub-pixel can be suppressed.

[0145] As the wavelength conversion layer, a conventional wavelength conversion layer can be used, and a color filter or the like may be used as necessary.

[0146] As the opposing substrate in the present invention, there is no particular limitation, and an existing opposing substrate can be used. For example, glass plates, resin plates, resin films, sapphire substrates, printed wiring boards, TFT array substrates, ceramics, etc. are listed. As the material of the glass plate, alkali-free glass is preferred. As the material of the resin plate and the resin film, polyester, (meth) acrylic polymer, transparent polyimide, polyether sulfone, etc. are preferred. The thickness of the glass plate and the resin plate is preferably less than 1 mm, preferably less than 0.8 mm. The thickness of the resin film is preferably less than 100 μm.

[0147] The display device of the present invention preferably includes a driving element, and the light-emitting element and the driving element are electrically connected via wiring extending in the hardened film. By including a driving element in the display device, and the light-emitting element and the driving element are electrically connected via wiring extending in the hardened film, one or more light-emitting elements can be individually switched. As the driving element, a driver integrated circuit (IC) can be listed, and one or more driver ICs can be used according to different functions, relative to the packaging of one or more light-emitting elements or multiple light-emitting elements including red, blue, green, etc.

[0148] As a configuration mode of the driving element, it is preferred that Figure 5 As shown in FIG. 1 , the driving element 8 is arranged in the vicinity of the light emitting element 2 on the counter substrate 5 in the cured film 3. Figure 6 As shown in FIG. 1 , the driving element 8 is arranged in the cured film 3 at a position above the light emitting element 2 .

[0149] This can suppress wiring failures such as wiring short circuits due to shortened wiring distances, suppress loss reduction, and improve high-speed responsiveness.

[0150] In the present invention, it is preferred that: a driving element and a substrate are further provided, wherein the driving element is connected to the light emitting element via wiring, and further, at least a portion of the wiring extends on the side of the substrate. By providing a driving element and a substrate, and the driving element is connected to the light emitting element via wiring, and further, at least a portion of the wiring extends on the side of the substrate, a plurality of light emitting elements can be individually switched, and the low profile or high-speed responsiveness of the display device itself is improved, and further, the display device can be made more compact and have a narrow frame.

[0151] As for the substrate, there is no particular limitation as with the light emitting element driving substrate 7, and an existing substrate can be used. For example, a glass substrate, a sapphire substrate, a TFT array substrate, a ceramic, etc. are listed. As for the wiring that at least partially extends on the side surface of the substrate, as its structure, for example, it is preferably as follows Figure 1 or Figure 4 , Figure 12 to Figure 14 The structure is configured as shown in 4c.

[0152] In the present invention, it is preferred to further include a light shielding layer between the plurality of light emitting elements. By including a light shielding layer between the plurality of light emitting elements, light leakage from the light emitting elements or color mixing between pixels can be suppressed without significantly impairing light output efficiency, thereby improving contrast.

[0153] The light-shielding layer may include a cured film formed by curing a resin composition comprising (A) resin and (E) coloring material. In addition, it may also contain materials other than the resin composition comprising (A) resin, and existing materials such as epoxy resin, (meth) acrylic polymer, polyurethane, polyester, polyolefin, polysiloxane, etc. can be used. As the (E) coloring material, a black pigment can be used, for example, black organic pigments such as carbon black, perylene black, and aniline black; graphite; and inorganic pigments such as metal particles, metal oxides, composite oxides, metal sulfides, metal nitrides, and metal nitrogen oxides of titanium, copper, iron, manganese, cobalt, chromium, nickel, zinc, calcium, and silver. In addition, a red pigment and a blue pigment or a yellow pigment or other pigments as needed can be combined to make black. In addition, dyes can also be used. It can also contain two or more coloring materials.

[0154] The resin composition containing the (A) resin and the (E) coloring material may be provided with photosensitivity, and the (B) photosensitizer described later may also be used.

[0155] As a method for producing a resin composition comprising (A) resin and (E) coloring material, for example, the following method is preferred: using a disperser to disperse a resin solution containing (A) resin, (E) coloring material, a dispersant as needed, and an organic solvent to prepare a coloring material dispersion having a high coloring material concentration, and then adding (A) resin or other components such as a photosensitizer as needed, stirring. Filtering may be performed as needed.

[0156] As a dispersing machine, for example, a ball mill, a bead mill, a sand mill, a three-roll mill, a high-speed impact mill, etc. can be cited. Among these, in order to achieve dispersion efficiency and micro-dispersion, a bead mill is preferably used. As a bead mill, for example, a co-ball mill, a basket mill, a pin mill, a Dyno-mill, etc. can be cited. As beads for a bead mill, for example, titanium dioxide beads, zirconium oxide beads, zircon beads can be cited. The bead diameter of the bead mill is preferably 0.03 mm or more and 1.0 mm or less. In the case where the primary particle size of the coloring material (E) and the particle size of the secondary particles formed by the aggregation of the primary particles are small, it is preferred to use micro beads with a diameter of 0.03 mm or more and 0.10 mm or less. In the case, it is preferred to include a bead mill comprising a separator, which utilizes a centrifugal separation method and can separate the micro beads from the dispersion. On the other hand, when dispersing a coloring material including submicron-sized coarse particles, it is preferred to use beads having a diameter of 0.10 mm or more in order to obtain sufficient pulverization force.

[0157] The resin composition comprising the resin (A) and the coloring material (E) is applied to various substrates and dried, and then subjected to heat treatment to obtain a light-shielding layer. In the case of having photosensitivity, after exposure to chemical rays described later, development and heat treatment described later are performed to obtain a patterned light-shielding layer.

[0158] The thickness of the light shielding layer is preferably 0.1 μm or more and 5 μm or less. If the thickness of the light shielding layer is 0.1 μm or more, light leakage from the light emitting element or color mixing between pixels can be suppressed, thereby improving the contrast. The thickness of the light shielding layer is more preferably 0.5 μm or more. On the other hand, if the thickness of the wiring is 5 μm or less, light leakage from the light emitting element or color mixing between pixels can be suppressed without significantly impairing the light output efficiency, thereby improving the contrast. The thickness of the light shielding layer is more preferably 4 μm or less.

[0159] Regarding the light-shielding layer, a colored film is formed on an alkali-free glass having a thickness of 0.7 mm so that the film thickness becomes 1.0 μm, and the reflected chromaticity values ​​(a*, b*) obtained by measuring the chromaticity from the glass surface are preferably -0.5≤a*≤1.0 and -1.0≤b*≤0.5, and preferably -0.5≤a*≤0.5 and -1.0≤b*≤0.4. The reflected chromaticity becomes an index of the hue of the image reflected in the colored film, and the closer it is to (a*, b*) = (0.0, 0.0), the more it can be said to be achromatic. On the other hand, regarding the reflected hue of the black display of a liquid crystal display device or an organic EL display, b* is generally a negative value and a blue hue, so as a decorative film used in a display device, it is preferred that b* be a negative value.

[0160] The reflection chromaticity (L*, a*, b*) of the colored film was obtained by measuring the total reflection chromaticity (including the specular component (SCI)) with respect to light incident from the transparent substrate under the measurement conditions of standard illuminant D65 (color temperature 6504K), viewing angle 2° (International Commission on Illumination (CIE) 1976), atmospheric pressure, and 20°C using a spectrophotometer (CM-2600d; manufactured by Konica Minolta Co., Ltd.) calibrated using a white calibration plate (CM-A145; manufactured by Konica Minolta Co., Ltd.).

[0161] As a structure of the light shielding layer, for example, it is preferably as follows Fig.15 The light shielding layer 25 may be in contact with the light emitting element 2 or may be separated from the light emitting element 2.

[0162] In the present invention, the cured film formed by curing the resin composition containing the resin (A) has a transmittance of light of wavelength 450nm at a thickness of 1μm of 0.1% or more and 95% or less. Thus, by having such high wiring concealment, the glare of the wiring can be suppressed, making it difficult to be seen from the outside, thereby improving the design.

[0163] The transmittance of the cured film at a wavelength of 450 nm at a thickness of 5 μm is preferably 0.1% to 79%. This can suppress glare from wiring, making it difficult to be seen from the outside, and improve design properties.

[0164] The transmittance of the cured film at a wavelength of 450 nm at a thickness of 1 μm is preferably 0.1% to 25%. This can suppress glare from wiring and make it difficult to see from the outside, thereby improving design, and further, by reducing external light reflection or increasing contrast, visibility can be improved.

[0165] If the transmittance of the cured film at a wavelength of 450 nm at a thickness of 1 μm is less than 0.1%, the sensitivity and resolution of the resin film before curing may be reduced. If the transmittance exceeds 95%, the wiring concealment property may be reduced, the glare of the wiring may not be sufficiently suppressed, and the wiring may be visible from the outside.

[0166] In addition, the resin (A) preferably has high heat resistance, and specifically, preferably has little degradation at a high temperature of 160° C. or higher during or after heat treatment. Such a cured film is preferred because it has a reduced outgassing amount, which is one of the excellent properties of the cured film used as a display device, such as an insulating film, a protective film, and a partition.

[0167] From the viewpoint of forming a desired opening pattern by exposure and development, the (A) resin preferably has a high transmittance of light of an exposure wavelength before curing.

[0168] In order to obtain such characteristics, for example, it is preferable to shorten the conjugated chain derived from the aromatic ring of the resin or to reduce the charge transfer within or between molecules.

[0169] In order to protect the wiring, it is preferred that the processability is excellent even if the film has a thickness of 10 μm or more.

[0170] (A) The resin is not particularly limited, but is preferably an alkali-soluble resin from the viewpoint of reducing the environmental load. The so-called alkali solubility is as follows: a solution in which a resin is dissolved in γ-butyrolactone is applied to a silicon wafer, and pre-baked at 120°C for 4 minutes to form a pre-baked film with a film thickness of 10μm±0.5μm. Here, prebaking is a process of heating and drying after coating, and the so-called pre-baked film refers to a film obtained by heating and drying. In addition, the pre-baked film and the resin film have the same meaning. Secondly, the pre-baked film is immersed in a 2.38% by mass tetramethylammonium hydroxide aqueous solution at 23±1°C for 1 minute, and then rinsed with pure water to calculate the reduction in film thickness at this time. Resins whose dissolution rate of the pre-baked film is 50nm / minute or more are defined as alkali-soluble.

[0171] The resin (A) preferably contains one or more resins selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, and copolymers thereof. The resin (A) may contain these resins alone or in combination of a plurality of resins.

[0172] Polyimide, a polyimide precursor, polybenzoxazole, and a polybenzoxazole precursor are described.

[0173] As long as polyimide has an imide ring, it is not particularly limited. In addition, as long as the polyimide precursor has a structure that becomes a polyimide with an imide ring by dehydration ring closure, it is not particularly limited, and may contain polyamic acid or polyamic acid esters. As long as polybenzoxazole has an oxazole ring, it is not particularly limited. As long as the polybenzoxazole precursor has a structure that becomes a polybenzoxazole with a benzoxazole ring by dehydration ring closure, it is not particularly limited, and may contain polyhydroxyamides, etc.

[0174] The polyimide has a structural unit represented by the general formula (1), the polyimide precursor and the polybenzoxazole precursor have a structural unit represented by the following general formula (2), and the polybenzoxazole has a structural unit represented by the general formula (3). Two or more of these may be contained, and a resin obtained by copolymerizing the structural unit represented by the general formula (1), the structural unit represented by the general formula (2), and the structural unit represented by the general formula (3) may be contained.

[0175] [Chemistry 1]

[0176]

[0177] In the general formula (1), V represents a tetravalent to decavalent organic group having 4 to 40 carbon atoms, and W represents a divalent to octavalent organic group having 4 to 40 carbon atoms. a and b each represent an integer of 0 to 6. 1 and R 2 represents a group selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfonic acid group and a thiol group, and a plurality of R 1 and R 2 They may be the same or different.

[0178] [Chemistry 2]

[0179]

[0180] In the general formula (2), X and Y each independently represent a divalent to octavalent organic group having 4 to 40 carbon atoms. 3 and R 4 Each independently represents a hydrogen atom or a monovalent organic group having a carbon number of 1 to 20. c and d each represent an integer of 0 to 4, and e and f each represent an integer of 0 to 2.

[0181] [Chemistry 3]

[0182]

[0183] In the general formula (3), T and U each independently represent a divalent to octavalent organic group having 4 to 40 carbon atoms.

[0184] In order to make the (A) resin alkali-soluble, in the general formula (1), a+b>0 is preferred. In the general formula (2), c+d+e+f>0 is preferred. In the general formula (2), in the case of a polyimide precursor, X and Y in the general formula (2) preferably have an aromatic group. Furthermore, X in the general formula (2) has an aromatic group, e>2, has a carboxyl group or a carboxyl ester group at the ortho position of the aromatic amide group, and forms a structure of an imide ring by dehydration ring closure.

[0185] In the general formula (2), in the case of a polybenzoxazole precursor, X in the general formula (2) has an aromatic group, d>0, has a hydroxyl group at the ortho position of the aromatic amide group, and forms a benzoxazole ring by dehydration ring closure.

[0186] The number n of repetitions of the structural unit represented by the general formula (1), the general formula (2) or the general formula (3) in the resin (A) is preferably 5 to 100,000, more preferably 10 to 100,000.

[0187] (A) resin may also have other structural units in addition to the structural units represented by general formula (1), general formula (2) or general formula (3). As other structural units, for example, cardo structure, siloxane structure, etc. can be listed, but are not limited to these. In the case described, it is preferred to set the structural unit represented by general formula (1) or general formula (2) as the main structural unit. The so-called main structural unit here refers to the structural unit represented by general formula (1), general formula (2) or general formula (3) with more than 50 mol% in the number of all structural units, and more preferably with more than 70 mol%.

[0188] In the general formula (1), V-(R 1 ) a , (OH) in the general formula (2) c -X-(COOR 3 ) e and T in the general formula (3) represents an acid residue. V is a tetravalent to decavalent organic group having 4 to 40 carbon atoms, preferably an organic group having 4 to 40 carbon atoms containing an aromatic ring or a cyclic aliphatic group. X and T are divalent to octavalent organic groups having 4 to 40 carbon atoms, preferably an organic group having 4 to 40 carbon atoms containing an aromatic ring or an aliphatic group.

[0189] Examples of the acid component constituting the acid residue include terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, triphenyl dicarboxylic acid, suberic acid, dodecafluorosuberic acid, azelaic acid, sebacic acid, hexadecanoic acid, 1,9-nonane dioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosanedioic acid, heneicosanedioic acid, dihydrogen iodide ... Examples of the present invention include dodecanedioic acid, tricosanedioic acid, tetracosanedioic acid, pentacosanedioic acid, hexacosanedioic acid, heptacosanedioic acid, octacosanedioic acid, nonacosanedioic acid, triacontanedioic acid, etc. Examples of tricarboxylic acids include trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, biphenyltricarboxylic acid, etc. Examples of tetracarboxylic acids include pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-dicarboxylic acid, Phenyl ether tetracarboxylic acid, 3,3',4,4'-benzophenone tetracarboxylic acid, 2,2',3,3'-benzophenone tetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)ether, 1,2,5,6-naphthalene tetracarboxylic acid, Carboxylic acid, 9,9-bis(3,4-dicarboxyphenyl)fluorene, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane and aromatic tetracarboxylic acids of the structures shown below, butanetetracarboxylic acid, cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, etc., but are not limited to these. Two or more of these may be used.

[0190] [Chemistry 4]

[0191]

[0192] In the formula, R 17 represents an oxygen atom, C(CF3)2 or C(CH3)2. 18 and R 19 represents a hydrogen atom or a hydroxyl group.

[0193] These acids may be used directly or in the form of anhydrides, halides or active esters.

[0194] In the general formula (1), W-(R 2 ) b, (OH) in the general formula (2) d -Y-(COOR 4 ) f and U in the general formula (3) represents a residue of a diamine. W, Y and U are divalent to octavalent organic groups having 4 to 40 carbon atoms, and preferably are organic groups having 4 to 40 carbon atoms containing an aromatic ring or a cyclic aliphatic group.

[0195] Specific examples of the diamine constituting the diamine residue include hydroxyl-containing diamines such as bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methylene, bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxy)biphenyl, and bis(3-amino-4-hydroxyphenyl)fluorene; sulfonic acid-containing diamines such as 3-sulfonic acid-4,4'-diaminodiphenyl ether; thiol group-containing diamines such as dithiophenylene diamine; 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diamino Diphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, petroleum ether (benzine), m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxyphenyl) sulfone, bis(3-aminophenoxyphenyl) sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diamine Aromatic diamines such as biphenylamine, 2,2'-diethyl-4,4'-biphenylamine, 3,3'-dimethyl-4,4'-biphenylamine, 3,3'-diethyl-4,4'-biphenylamine, 2,2',3,3'-tetramethyl-4,4'-biphenylamine, 3,3',4,4'-tetramethyl-4,4'-biphenylamine, and 2,2'-bis(trifluoromethyl)-4,4'-biphenylamine, or compounds wherein a portion of the hydrogen atoms in the aromatic rings are substituted with an alkyl group or fluoroalkyl group having 1 to 10 carbon atoms, a halogen atom, or the like; 2,4-diamino-1,3,5-triazine (guanamine), 2,4-diamino-6-methyl Diamines having a nitrogen-containing heteroaromatic ring such as 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(p-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(p-aminophenethyl)-1,1,3,3-tetramethyldisiloxane, 1,7-bis(p-aminophenyl)-1,1,3,5,5,7,7-octamethyltetrasiloxane; alicyclic diamines such as cyclohexyldiamine and methylenebiscyclohexylamine, and diamines of the structures shown below. Two or more of these may be used.

[0196] [Chemistry 5]

[0197]

[0198] In the formula, R 20represents an oxygen atom, C(CF3)2 or C(CH3)2. 21 ~R 24 Each independently represents a hydrogen atom or a hydroxyl group.

[0199] Among these, from the viewpoint of improving alkali developability or the transmittance of the (A) resin or its cured film, a diamine containing at least one or more structures shown below is preferred.

[0200] [Chemistry 6]

[0201]

[0202] In the formula, R 20 represents an oxygen atom, C(CF3)2 or C(CH3)2. 21 ~R 22 Each independently represents a hydrogen atom or a hydroxyl group.

[0203] These diamines may be used in the form of diamines, or in the form of diisocyanate compounds obtained by reacting diamines with phosgene, or trimethylsilylated diamines.

[0204] The resin (A) preferably contains a group selected from an alkylene group and an alkylene ether group. These groups may also contain an aliphatic ring. As the group selected from an alkylene group and an alkylene ether group, a group represented by the general formula (4) is particularly preferred.

[0205] [Chemistry 7]

[0206]

[0207] In the general formula (4), R 5 ~R 8 R each independently represents an alkylene group having 1 to 6 carbon atoms. 9 ~R 16 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 6 carbon atoms. The structures in the parentheses are different from each other. g, h, and i each independently represent an integer of 0 to 35, and g+h+i>0.

[0208] Examples of the group represented by the general formula (4) include an ethylene oxide group, a propylene oxide group, and a butylene oxide group. The group may be linear, branched, or cyclic.

[0209] The resin (A) having a group selected from an alkylene group and an alkylene ether group can improve the mechanical properties of the resin (A) and the cured film thereof, particularly the elongation, and can also improve the transmittance of light at 450 nm before and after curing.

[0210] The resin (A) preferably contains a group selected from the group consisting of an alkylene group and an alkylene ether group in W in the general formula (1) or Y in the general formula (2). This can improve the mechanical properties of the resin (A) and its cured film, especially the elongation, and further improve the transmittance of light at 450 nm before and after curing, and can obtain the cured film of the resin composition with high chemical resistance due to promotion of ring closure in low-temperature heating treatment, high adhesion to the substrate metal, and resistance to constant temperature and humidity test (highly accelerated stress test (HAST)).

[0211] Specific examples of the diamine containing a group selected from an alkylene group and an alkylene ether group include ethylenediamine, 1,3-diaminopropane, 2-methyl-1,3-propanediamine, 1,4-diaminobutane, 1,5-diaminopentane, 2-methyl-1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane Hexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), KH-511, ED-600, ED-900, ED-2003, EDR-148, EDR-176, D-200, D-400, D-2000, THF-100, THF-140, THF-170, RE-600, RE-900, RE-2000, RP-405, RP-409, RP-2005, RP-2009, RT-1000, HE-1000, HT-1100, HT-1700 (these are trade names, manufactured by Huntsman Co., Ltd.), etc.

[0212] In addition, these diamines may also contain bonds such as -S-, -SO-, -SO2-, -NH-, -NCH3-, -N(CH2CH3)-, -N(CH2CH2CH3)-, -N(CH(CH3)2)-, -COO-, -CONH-, -OCONH-, and -NHCONH-.

[0213] The diamine residue containing a group selected from an alkylene group and an alkylene ether group preferably contains 5 mol% or more of all diamine residues, and more preferably contains 10 mol% or more. In addition, among all diamine residues, it is preferably contained 40 mol% or less, and more preferably contains 30 mol% or less. By setting it to the range, the developability in the alkaline developer can be improved, and the mechanical properties of (A) resin and its cured film can be improved, especially the elongation, and then the transmittance of 450nm light after curing can be improved, and the cured film of the resin composition can be obtained. The high chemical resistance brought about by promoting closed loops in low-temperature heating treatment, the high adhesion to the metal surface, and the resistance relative to the constant temperature and humidity test (HAST) can be obtained.

[0214] It is also possible to copolymerize diamine residues having an aliphatic polysiloxane structure within a range that does not reduce heat resistance. By copolymerizing diamine residues having an aliphatic polysiloxane structure, adhesion to the substrate can be improved. Specifically, as diamine components, diamine components such as bis(3-aminopropyl)tetramethyldisiloxane and bis(p-aminophenyl)octamethylpentasiloxane copolymerized with 1 mol% to 15 mol% of all diamine residues can be cited. When copolymerized within the range, adhesion to substrates such as silicon wafers is improved, and solubility in alkaline solutions is not reduced, which is preferred in these aspects.

[0215] By blocking the terminal of the resin (A) with a monoamine, anhydride, acid chloride or monocarboxylic acid having an acidic group, a resin having an acidic group at the main chain terminal can be obtained. As the monoamine, anhydride, acid chloride or monocarboxylic acid having an acidic group, existing ones can be used or multiple types can be used.

[0216] The content of the terminal blocking agent such as monoamine, acid anhydride, acid chloride, monocarboxylic acid is preferably 2 to 25 mol % based on 100 mol % of the total of the acid component and the amine component constituting the resin (A).

[0217] (A) The resin preferably has a weight average molecular weight of 10,000 or more and 100,000 or less. If the weight average molecular weight is 10,000 or more, the mechanical properties of the cured film after curing can be improved. More preferably, the weight average molecular weight is 20,000 or more. On the other hand, if the weight average molecular weight is 100,000 or less, the developability using various developers can be improved, and further, if the weight average molecular weight is 50,000 or less, the developability using alkaline solutions can be improved, so it is preferred.

[0218] The weight average molecular weight (Mw) can be confirmed by gel permeation chromatography (GPC), for example, by measuring with N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as NMP) as the developing solvent and calculating the weight average molecular weight in terms of polystyrene.

[0219] The content of the resin (A) is preferably 3 to 55% by mass, more preferably 5 to 40% by mass, based on 100% by mass of all components including the solvent. By setting the content within the above range, an appropriate viscosity can be achieved during spin coating or slit coating.

[0220] In addition, phenol resins, polymers containing radical polymerizable monomers having alkali-soluble groups as monomer units, such as polyhydroxystyrene or acryl, siloxane polymers, cyclic olefin polymers, and cardo resins, etc., can also be used. These resins can be used in existing ones, and can be used alone or in combination of multiple resins.

[0221] Furthermore, from the viewpoint of reducing the transmittance, the phenol resin is preferably a wholly aromatic phenol resin containing a phenol compound and an aromatic aldehyde compound.

[0222] In the present invention, it is preferred that the resin composition containing the (A) resin contains the (B) photosensitizer (hereinafter, sometimes referred to as the (B) component).

[0223] The resin composition containing the (A) resin preferably further contains the (B) photosensitizer, because photosensitivity can be imparted to the resin composition, thereby forming a fine opening pattern.

[0224] (B) The photosensitive agent is a compound that changes its chemical structure in response to ultraviolet rays, and examples thereof include: a photoacid generator, a photobase generator, a photopolymerization initiator, etc. When a photoacid generator is used as the (B) component, an acid is generated in the light-irradiated portion of the photosensitive resin composition, and the solubility of the light-irradiated portion in the alkaline developer increases, so that a positive pattern in which the light-irradiated portion is dissolved can be obtained.

[0225] When a photobase generator is contained as the (B) photosensitizer, a base is generated in the light-irradiated portion of the resin composition to reduce the solubility of the light-irradiated portion in an alkaline developer, thereby obtaining a negative pattern in which the light-irradiated portion is insolubilized.

[0226] When a photopolymerization initiator is included as the photosensitizer (B), free radicals are generated in the light-irradiated part of the resin composition to undergo free radical polymerization, which makes it insoluble in an alkaline developer, thereby forming a negative pattern. In addition, ultraviolet (UV) curing during exposure is accelerated, which can improve sensitivity.

[0227] In the present invention, regarding the cured film formed by curing the resin composition containing the resin (A), the transmittance of light of a wavelength of 450nm at a thickness reference of 1μm is 0.1% or more and 95% or less. Thus, by having the high wiring concealment of the cured film, the glare of the wiring can be suppressed, making it difficult to be visually recognized from the outside, thereby improving the design. If the transmittance of light is less than 0.1%, there is a concern that the sensitivity or resolution of the resin film before curing will be reduced. If the transmittance of light exceeds 95%, the wiring concealment is reduced, the glare of the wiring is not sufficiently suppressed, and there is a concern that it can be visually recognized from the outside.

[0228] In order to obtain such characteristics, the (B) photosensitive agent is preferably: (B) the photosensitive agent itself has low transmittance of light at a wavelength of 450nm, and the structural change is small after heat treatment; or (B) the reaction product of the photosensitive agent and (A) resin or thermal crosslinking agent has low transmittance of light; (B) the decomposition product of the photosensitive agent itself or the reaction product derived from the decomposable product has low transmittance of light.

[0229] From the viewpoint of fine processing properties, the resin composition containing the (A) resin is preferably positive-type photosensitivity. Furthermore, the resin composition containing the (A) resin and the (B) photosensitive agent is preferably positive-type photosensitivity.

[0230] Among the above-mentioned (B) photosensitizers, photoacid generators are preferred from the viewpoints of high wiring concealment, high sensitivity, and fine processing. Examples of photoacid generators include quinonediazide compounds, sulfonium salts, phosphonium salts, diazonium salts, and iodonium salts. Furthermore, a sensitizer may be included as needed.

[0231] The quinonediazide compound is preferably a compound in which naphthoquinonediazide sulfonic acid is ester-bonded to a compound having a phenolic hydroxyl group. As the compound having a phenolic hydroxyl group used herein, an existing compound having a phenolic hydroxyl group can be used, and a compound into which 4-naphthoquinonediazide sulfonic acid or 5-naphthoquinonediazide sulfonic acid is introduced via an ester bond can be exemplified as a preferred compound having a phenolic hydroxyl group, but other compounds can also be used.

[0232] In addition, it is preferred that more than 50 mol% of the functional groups of the compound having a phenolic hydroxyl group are substituted with quinone diazide. By using more than 50 mol% of the substituted quinone diazide compound, the affinity of the quinone diazide compound to the alkaline aqueous solution is reduced. As a result, the solubility of the resin composition in the unexposed portion to the alkaline aqueous solution is greatly reduced. Furthermore, by exposure, the quinone diazide sulfonyl group is changed to indene carboxylic acid, and a large dissolution rate of the photosensitive resin composition in the exposed portion relative to the alkaline aqueous solution can be obtained. That is, as a result, the dissolution rate ratio of the exposed portion to the unexposed portion of the composition can be increased, thereby obtaining a pattern with high resolution.

[0233] By containing such a quinonediazide compound, a resin composition having positive photosensitivity can be obtained which is sensitive to i-ray (365nm), h-ray (405nm), g-ray (436nm) of a common mercury lamp or a broadband thereof. In addition, the photosensitive agent (B) may contain only one kind or a combination of two or more kinds, and a highly sensitive resin composition can be obtained.

[0234] Examples of quinonediazide include 5-naphthoquinonediazidesulfonyl group, 4-naphthoquinonediazidesulfonyl group, and quinonediazide containing 4-naphthoquinonediazidesulfonyl group and 5-naphthoquinonediazidesulfonyl group in the same molecule.

[0235] As naphthoquinonediazidesulfonylester compounds, 5-naphthoquinonediazidesulfonylester compounds (B-1) and 4-naphthoquinonediazidesulfonylester compounds (B-2) can be cited. In the present invention, it is preferred to include the (B-2) compound. The (B-2) compound has a large absorption in the i-ray region of the mercury lamp, and is therefore suitable for i-ray exposure. In addition, during curing, the (B-2) compound decomposes or reacts with the (A) resin and the like to be colored, thereby reducing the transmittance of 450nm light, so it is preferred from the perspective of transmittance after heat treatment. In the case where the photosensitive agent is a single component of the (B-2) compound or is mixed with other components, the (B-2) compound is preferably contained at 46% by mass or more. In the case of a mixture of the (B-1) compound and the (B-2) compound, the content ratio of the (B-2) compound is preferably 46% by mass or more and 100% by mass or less relative to the total photosensitizer dose, i.e., the (B-1) compound + (B-2) compound. By setting it as said content ratio, the cured film with low light transmittance can be obtained.

[0236] The quinone diazide compound can be synthesized by an existing method through an esterification reaction between a compound having a phenolic hydroxyl group and a naphthoquinone diazide sulfonic acid compound. By using the quinone diazide compound, the resolution, sensitivity and residual film rate are further improved.

[0237] The molecular weight of the (B) photosensitizer is preferably 300 or more, more preferably 350 or more, and is preferably 3,000 or less, more preferably 1,500 or less, from the viewpoint of heat resistance, mechanical properties, and adhesiveness of the film obtained by heat treatment.

[0238] (B) Among the photosensitizers, sulfonium salts, phosphonium salts, and diazonium salts are preferred because they can appropriately stabilize the acid component generated by light exposure. Among them, sulfonium salts are preferred.

[0239] The content of the photosensitive agent (B) is preferably 0.1 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the resin (A). If the content of the photosensitive agent (B) is 0.1 parts by mass or more and 100 parts by mass or less, photosensitivity can be imparted while maintaining the heat resistance, chemical resistance and mechanical properties of the film after heat treatment.

[0240] When the photosensitive agent (B) contains a quinone diazide, the content of the photosensitive agent (B) is more preferably 1 part by mass or more, and more preferably 3 parts by mass or more, relative to 100 parts by mass of the component (A). In addition, it is more preferably 100 parts by mass or less, and more preferably 80 parts by mass or less. If it is 1 part by mass or more and 100 parts by mass or less, it is possible to impart photosensitivity while maintaining the heat resistance, chemical resistance and mechanical properties of the film after heat treatment.

[0241] When the (B) photosensitive agent contains a sulfonium salt, a phosphonium salt or a diazonium salt, the content of the (B) photosensitive agent is more preferably 0.1 parts by mass or more, more preferably 1 parts by mass or more, and particularly preferably 3 parts by mass or more, relative to 100 parts by mass of the (A) resin. In addition, it is more preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and particularly preferably 50 parts by mass or less. If it is 0.1 parts by mass or more and 100 parts by mass or less, it is possible to impart photosensitivity while maintaining the heat resistance, chemical resistance and mechanical properties of the film after heat treatment.

[0242] When a photobase generator is contained as the (B) photosensitizer, specific examples of the photobase generator include amide compounds and ammonium salts.

[0243] Examples of the amide compound include 2-nitrophenylmethyl-4-methacryloyloxypiperidine-1-carboxylate, 9-anthrylmethyl-N,N-dimethylcarbamate, 1-(anthraquinone-2-yl)ethylimidazolecarboxylate, and (E)-1-[3-(2-hydroxyphenyl)-2-propionyl]piperidine.

[0244] Examples of the ammonium salt include 1,2-diisopropyl-3-(bis(dimethylamino)methylene)guanidine 2-(3-benzoylphenyl)propionate, (Z)-{[bis(dimethylamino)methylene]amino}-N-cyclohexylamino)methaniminiumtetrakis(3-fluorophenyl)borate, and 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidine-n-butyltriphenylborate.

[0245] In the case of containing a photobase generator as (B) photosensitizer, the content of (B) photosensitizer in the resin composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and further preferably 0.7 parts by mass or more, and particularly preferably 1 parts by mass or more relative to 100 parts by mass of (A) resin. If the content is within the range, the sensitivity during exposure can be improved. On the other hand, the content is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 17 parts by mass or less, and particularly preferably 15 parts by mass or less. If the content is within the range, the resolution after development can be improved.

[0246] When a photopolymerization initiator is contained as the photosensitive agent (B), the photopolymerization initiator is preferably, for example, a benzyl ketal photopolymerization initiator, an α-hydroxyketone photopolymerization initiator, an α-aminoketone photopolymerization initiator, an acylphosphine oxide photopolymerization initiator, an oxime ester photopolymerization initiator, an acridine photopolymerization initiator, a benzophenone photopolymerization initiator, an acetophenone photopolymerization initiator, an aromatic ketone ester photopolymerization initiator or a benzoate photopolymerization initiator, or a titanocene photopolymerization initiator, and any existing photopolymerization initiator may be used for each of them, or a plurality of them may be used. Among them, from the viewpoint of improving the sensitivity during exposure, more preferred are α-hydroxyketone-based photopolymerization initiators, α-aminoketone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, oxime ester-based photopolymerization initiators, acridine-based photopolymerization initiators or benzophenone-based photopolymerization initiators, and further preferred are α-aminoketone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators and oxime ester-based photopolymerization initiators.

[0247] In the case of containing a photopolymerization initiator as the (B) photosensitive agent, the content of the (B) photosensitive agent in the resin composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, further preferably 0.7 parts by mass or more, and particularly preferably 1 parts by mass or more relative to 100 parts by mass of the (A) resin. If the content is within the range, the sensitivity during exposure can be improved. On the other hand, the content is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, further preferably 17 parts by mass or less, and particularly preferably 15 parts by mass or less. If the content is within the range, the resolution after development can be improved.

[0248] In the present invention, it is preferred that the resin composition containing the resin (A) further contains a colorant (C), and the colorant (C) contains a colorant (C-1) having a maximum absorption in a wavelength range of not less than 400 nm and not more than 490 nm (hereinafter referred to as component (C) or component (C-1)).

[0249] (C) The colorant includes thermochromic compounds, dyes, pigments, etc. Among them, from the viewpoint of heat resistance, sensitivity, and resolution, it is preferred to use at least one of a dye and an organic pigment, and a dye is more preferred.

[0250] When the component (C) contains the component (C-1), light in the wavelength range of 400 nm to 490 nm can be absorbed to suppress the amount of light transmitted, and the transmittance of the cured film of the present invention at a wavelength of 450 nm at a thickness of 1 μm can be set to 0.1% to 95%. When the cured film has high wiring concealment, the glare of the wiring can be suppressed and the wiring can be difficult to be seen from the outside, thereby improving the design.

[0251] The component (C-1) is preferably a colorant having maximum absorption in a wavelength range of preferably 420 nm to 480 nm, more preferably in a wavelength range of 430 nm to 470 nm.

[0252] Since the component (C-1) has the property of transmitting light of wavelength 350 nm to 390 nm, which is a part of the exposure wavelength, both sensitivity and resolution to the exposure wavelength can be achieved. - 5 In the mol / L compound solution, the transmittance of light having a wavelength of 350 nm to 390 nm is preferably 40% or more, more preferably 70% or more.

[0253] The component (C-1) only needs to contain at least one, and examples thereof include: a method of using one thermochromic compound or one dye or organic pigment; a method of using a mixture of two or more thermochromic compounds or dyes or organic pigments; a method of using a combination of one or more thermochromic compounds with one or more dyes and one or more organic pigments, etc.

[0254] Examples of the component (C-1) include yellow dyes and orange dyes. Examples of the type of dye include oil-soluble dyes, disperse dyes, reactive dyes, acid dyes, and direct dyes.

[0255] The skeleton structure of the dye used as component (C-1) includes, but is not limited to, anthraquinone, methine, quinoline, and perinone. In addition, each of these dyes may be used alone or as a metal-containing complex salt. Specifically, Sumilan, Lanyl dyes (manufactured by Sumitomo Chemical Industries, Ltd.), Orasol, Oracet, Filamid, Irgasperse dyes (manufactured by CIBA Specialty Chemicals Co., Ltd.), Zapon, Neozapon, Neptune, Acidol dyes (manufactured by BASF), Kayaset, Kayakalan dyes (manufactured by Nippon Kayaku Co., Ltd.), Valifast Colors dyes (manufactured by ORIENT Chemical Industry Co., Ltd.), Savinyl, Sandoplast, Polysynthren, Lanasyn dyes (manufactured by CLARIANT Japan Co., Ltd.), The dyes include, but are not limited to, SUPERIOR DYES (manufactured by Japan) (co., Ltd.), Aizen Spilon dyes (manufactured by Hodogaya Chemical Industry Co., Ltd.), functional pigments (manufactured by Yamada Chemical Industry Co., Ltd.), Plast Color dyes, Oil Color dyes (manufactured by Arimoto Chemical Industry Co., Ltd.), etc. These dyes may be used alone or in combination.

[0256] From the viewpoint of fading during curing, the pigment used as the component (C-1) is preferably a pigment with high heat resistance. When a specific example is shown by a color index (CI) number, examples of yellow pigments include pigment yellow 83, 117, 129, 138, 139, 150, 180, etc. Examples of orange pigments include pigment orange 38, 43, 64, 71, 72, etc. In addition, relative to 100 parts by mass of the resin (A), the content of the component (C-1) is preferably 0.1 to 100 parts by mass, and more preferably 0.2 to 50 parts by mass. By setting the content of the component (C-1) to 0.1 parts by mass or more, light of the corresponding wavelength can be absorbed. In addition, by setting it to 100 parts by mass or less, the transmittance, sensitivity, and resolution of light can be taken into account.

[0257] In the present invention, it is preferred that the resin composition containing the (A) resin further contains a (C) colorant, wherein the (C) colorant contains a (C-2) colorant having a maximum absorption in a wavelength range exceeding 490 nm and not more than 580 nm (hereinafter referred to as the (C-2) component).

[0258] In the present invention, it is preferred that the resin composition containing the (A) resin further contains a (C) colorant, wherein the (C) colorant contains a (C-3) colorant having a maximum absorption in a wavelength range exceeding 580 nm and not more than 800 nm (hereinafter, sometimes referred to as the (C-3) component).

[0259] In the present invention, it is preferred that the colorant (C) contains, in addition to the component (C-1), a colorant (C-2) having a maximum absorption in a wavelength range exceeding 490 nm and not exceeding 580 nm, and a colorant (C-3) having a maximum absorption in a wavelength range exceeding 580 nm and not exceeding 800 nm.

[0260] By containing the components (C-2) and (C-3) in addition to the component (C-1), in addition to the wiring concealment, the external light reflection can be reduced or the contrast can be improved by blackening, so that the visibility can be improved, which is preferred.

[0261] Similar to component (C-1), component (C-2) and component (C-3) preferably have high solvent solubility or heat resistance and high transmittance at a wavelength of 350 nm to 390 nm, and preferably use one or more of a dye and an organic pigment, and more preferably a dye. Thus, in addition to achieving blackening by mixing component (C-1) and component (C-2) and component (C-3), high sensitivity and high resolution can be achieved in the resin film, so it is preferred.

[0262] As the skeleton structure of the dyestuff that can be preferably used as (C-2) component and (C-3) component, for example, triphenylmethane system, anthraquinone system etc. can be listed, but are not limited to these.In addition, these each dyestuff can be used alone, and also can be used as metal complex salt system.Specifically, can apply respectively Similan (Sumilan), Lanilu (Lanyl) dyestuff (Sumitomo Chemical Industries (stock) manufacture), Orasol (Orasol), Oraset (Oracet), Filamid (Filamid), Irgasperse dyestuff (Irgasperse) dyestuff (CIBA (CIBA) special chemicals (stock) manufacture), Zapon (Zapon), Neozapon (Neozapon), Neptune (Neptune), Acidol dyestuff (BASF (BASF) (stock) manufacture) , Kayaset, Kayakalan dyes (manufactured by Nippon Kayaku Co., Ltd.), Valifast Colors dyes (manufactured by Oriental Chemical Industry Co., Ltd.), Savinyl, Sandoplast, Polysynthren, Lanasyn dyes (manufactured by CLARIANT Japan Co., Ltd.), Aizen Spilon dyes (manufactured by Hodogaya Chemical Industry Co., Ltd.), functional pigments (manufactured by Yamada Chemical Industry Co., Ltd.), Plast Color dyes, Oil Color dyes (manufactured by Arimoto Chemical Industry Co., Ltd.), etc., but are not limited to these. These dyes can be used alone or in combination.

[0263] As an organic pigment that can be preferably used as the component (C-2), when specific examples are shown by color index (CI) number, examples of red pigments include pigment yellow 48:1, 122, 168, 177, 202, 206, 207, 209, 224, 242, 254, etc. Examples of purple pigments that can be preferably used as the component (C-2) include pigment violet 19, 23, 29, 32, 33, 36, 37, 38, etc. Examples of blue pigments that can be preferably used as the component (C-3) include pigment blue 15 (15:3, 15:4, 15:6, etc.), 21, 22, 60, 64, etc. Examples of green pigments that can be preferably used as the component (C-3) include pigment green 7, 10, 36, 47, 58, etc. In addition, pigments other than these can also be used. In addition, organic pigments subjected to surface treatment can also be used as needed in the same manner as described above.

[0264] The content of the component (C-2) and the component (C-3) is preferably 0.1 to 100 parts by mass, and more preferably 0.2 to 50 parts by mass, relative to 100 parts by mass of the resin (A). By setting the content of the component (C-1) to 0.1 parts by mass or more, light of the corresponding wavelength can be absorbed. In addition, by setting it to 100 parts by mass or less, the transmittance, sensitivity and resolution of light can be taken into account.

[0265] In addition, from the viewpoint of storage stability and fading during curing, the dyes used as the components (C-1), (C-2) and (C-3) are preferably dyes that are soluble in the organic solvent that dissolves the resin (A) and have high heat resistance and are compatible with the resin. Examples of the organic solvent include polar aprotic solvents such as N-methyl-2-pyrrolidone, γ-butyrolactone, γ-valerolactone, δ-valerolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, 1,3-dimethyl-2-imidazolidinone, N,N'-dimethylpropylene urea, N,N-dimethylisobutyric acid amide, and methoxy-N,N-dimethylpropionamide; ethers such as tetrahydrofuran, dioxane, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; ketones such as acetone, methyl ethyl ketone, and diisobutyl ketone; esters such as ethyl acetate, butyl acetate, isobutyl acetate, propyl acetate, propylene glycol monomethyl ether acetate, and 3-methyl-3-methoxybutyl acetate; alcohols such as ethyl lactate, methyl lactate, diacetone alcohol, and 3-methyl-3-methoxybutanol; and aromatic hydrocarbons such as toluene and xylene. In addition, regarding heat resistance, it is preferred that no change in the absorption spectrum is observed before and after heating at 250° C. for 1 hour in an environment with an oxygen concentration of 100 ppm or less.

[0266] Organic pigments that have been subjected to surface treatments such as rosin treatment, acidic treatment, and alkaline treatment may be used as needed. In addition, they may be used together with a dispersant as appropriate. Examples of dispersants include cationic, anionic, nonionic, amphoteric, silicone, and fluorine-based surfactants.

[0267] In the present invention, it is preferred that the resin composition containing the resin (A) further contains a colorant (C), and the colorant (C) contains a (C-4) black colorant (hereinafter, sometimes referred to as component (C-4)).

[0268] When the component (C) contains the component (C-4), the transmittance of the light of wavelength 450 nm at a thickness basis of 1 μm of the cured film of the present invention can be set to 0.1% or more and 95% or less. When the cured film has high wiring concealment, the glare of the wiring can be suppressed and it is difficult to be seen from the outside, thereby improving the design. Furthermore, by reducing the reflection of external light or improving the contrast, the visibility can be improved.

[0269] The component (C-4) may contain at least one kind, and examples thereof include a method of using one kind of inorganic black pigment, organic black pigment or black dye, and a method of using two or more kinds of inorganic black pigments, organic black pigments or black dyes in combination.

[0270] Examples of inorganic black pigments include, but are not limited to, inorganic black pigments having titanium atoms, inorganic black pigments having zirconium atoms, amorphous carbon black, and carbon black. The amorphous carbon black referred to herein refers to amorphous carbon black particles. On the other hand, carbon black simply refers to crystalline carbon black particles that are commonly used as colorants.

[0271] The so-called inorganic black pigment having titanium atoms refers to any one or more of titanium nitride represented by TiN, titanium oxynitride represented by TiNxOy (0<x<2.0, 0.1<y<2.0), titanium carbide represented by TiC, a solid solution of titanium nitride and titanium carbide, and a composite oxide or composite nitride of titanium and a metal other than titanium. Among them, in terms of high light shielding properties in the visible light region and high exposure transmittance in the exposure process, any one of titanium nitride and titanium oxynitride is preferred, and in terms of low dielectric constant, titanium nitride is more preferred. As a method for preparing titanium nitride, gas phase reaction can be cited, among which, in terms of easy acquisition of particles with a small primary particle size and a sharp particle size distribution, titanium nitride synthesized by a thermal plasma method is preferred. In addition, with regard to inorganic black pigments having titanium atoms, in order to avoid an increase in dielectric constant, the less the content of titanium dioxide represented by an inorganic white pigment, i.e., TiO2, as an impurity, the better, and more preferably, no content.

[0272] The so-called inorganic black pigment having zirconium atoms refers to any one or more of zirconium nitride represented by Zr3N4, zirconium nitride represented by ZrN, zirconium oxynitride represented by ZrOxNy (0<x<2.0, 0.1<y<2.0), and composite oxides or composite nitrides of zirconium and metals other than zirconium. Among them, in terms of high exposure transmittance and low dielectric constant in the exposure process, zirconium nitride represented by ZrN is preferred. As a preparation method, gas phase reaction can be listed, among which zirconium nitride synthesized by thermal plasma method is preferred in terms of easy acquisition of particles with small primary particle size and sharp particle size distribution. In addition, with regard to inorganic black pigments having zirconium atoms, in order to avoid an increase in dielectric constant, the less the content of zirconium dioxide represented by ZrO2 as an impurity, the better, and more preferably, no content.

[0273] The inorganic black pigment having titanium atoms and the inorganic black pigment having zirconium atoms may be subjected to surface treatment for modifying the surface of the pigment as needed. As the surface treatment method, for example, there can be cited a method of introducing an organic group containing silicon atoms in the form of a surface modification group by treatment with a silane coupling agent; a method of coating a part or all of the surface of the pigment with a coating material such as silicon dioxide, metal oxides and / or organic resins, etc., and a variety of surface treatments may also be combined. There are the following situations: By implementing these surface treatments, the long-term storage stability of the resin composition in the present invention can be improved. In addition, the inorganic black pigment having zirconium atoms and the inorganic black pigment having titanium atoms may also constitute a primary particle in the form of a solid solution of the two.

[0274] Amorphous carbon black refers to amorphous carbon black containing diamond structure (SP 3 structure) and graphite structure (SP 2 Amorphous carbon black (structure). Equivalent to carbon classified as diamond-like carbon (DLC). Amorphous carbon black has higher insulation than crystalline carbon black described later, and can be used as a coloring material without surface treatment. As a production method, it is preferred to gasify the carbon source, cool the carbon vapor obtained by gasification and resolidify it, and then temporarily make it into flakes, and perform dry pulverization to micronize it. Regarding the structure of amorphous carbon black, in the presence of a large amount of SP 3 In the case of a structure, the light shielding property of visible light and near infrared light is low, but on the other hand, the insulation property can be improved. 2 In the case of a structure, the insulation is low, but on the other hand, the light shielding property of visible light and near infrared light can be improved. That is, the above-mentioned properties inherent in the pigment can be controlled by using the synthesis conditions. Among them, in the photosensitive composition of the present invention, SP 3 The content of structure relative to SP 3 Structure and SP 2 The total amount of the structure is 30atom% to 70atom% of amorphous carbon black. 3 Structure and SP 2 The structural ratio can be analyzed by X-ray photoelectron spectroscopy.

[0275] In terms of further improving the near-infrared light-shielding property, the total amount of the above inorganic black pigment having titanium atoms, the inorganic black pigment having zirconium atoms, and amorphous carbon is preferably 5.0% by mass or more in the total solid content of the photosensitive composition of the present invention. In addition, in terms of avoiding excessive increase in dielectric constant, it is preferably 35.0% by mass or less in the total solid content in the photosensitive composition. The so-called total solid content mentioned here refers to the component after removing the solvent component from the photosensitive composition.

[0276] As carbon black, furnace black, thermal black, channel black, acetylene black, Ketjen black, and lamp black, which are classified according to their preparation methods, are listed. Among them, furnace black produced by a furnace method is preferred in terms of excellent dispersibility and industrially easy control of the acidity of the pigment surface or the miniaturization of the particle size. Among them, from the perspective of improving insulation, the shorter the structure length of the particles of carbon black that are firmly connected in a beaded shape, the more preferred it is, and further more preferred is carbon black with an organic group surface modified or carbon black coated with a highly insulating coating material. As such surface-modified carbon black, commercially available products can be used, for example, carbon black with an acidic functional group containing a sulfur atom surface modified, i.e., "TPK-1227", and carbon black with a pigment surface coated with silica, i.e., "TPX-1409" (all of the above are manufactured by CABOT).

[0277] In terms of further improving the near infrared light shielding property, the total amount of carbon black is preferably 5.0% by mass or more in the total solid content of the resin composition of the present invention. In addition, in terms of avoiding excessive increase in dielectric constant, it is preferably 10.0% by mass or less in the total solid content in the resin composition.

[0278] In order to make the cured film have the desired optical properties, multiple types may be used in combination. For example, by using zirconium nitride that exhibits purplish black and amorphous carbon that exhibits yellowish black to adjust the color, the reflection color of the cured film can be set to neutral black with low chromaticity.

[0279] From the viewpoint of improving dispersibility and storage stability after dispersion, the average primary particle size of the inorganic black pigment is preferably 5 nm or more, more preferably 10 nm or more. On the other hand, from the perspective of obtaining high flexibility, it is preferably 150 nm or less, more preferably 100 nm or less. The so-called average primary particle size described here refers to the number average of the primary particle size calculated by the particle size determination method using an image analysis type particle size distribution measuring device. In the shooting of the image, a transmission electron microscope (TEM) can be used, and the average primary particle size can be calculated under the condition of a magnification of 50,000 times. In the case where the (C-4) component is not spherical, the average value of its major diameter and minor diameter is used as the primary particle size. In the image analysis, the image analysis type particle size distribution software Mac-View manufactured by MOUNTECH is used. In the case where it is necessary to reduce the average primary particle size or grind the coarse components to make the particle size distribution sharp, a dry pulverization process can be performed. In the dry pulverization process, for example, a hammer mill, a ball mill, etc. can be used. In addition, since the hardness of the pigment is too high, dry pulverization has its limits. In such cases, it is ideal to remove coarse components by classification without crushing.

[0280] As an organic black pigment, it refers to benzodifuranone black pigment, perylene black pigment, azo black pigment and isomers thereof. The so-called isomer described herein also includes tautomers. Isomers can be included in the form of a mixture of multiple pigment powders, and can also be included in the form of mixed crystals on the basis of constituting a primary particle. In addition, in general, organic pigments are extremely lacking in light-shielding properties in the near-infrared region, but on the other hand, have the advantage of low dielectric constant, so in the resin composition comprising (A) resin in the present invention, it can be effectively used as a component for imparting light-shielding properties only to the visible light region while avoiding the increase in dielectric constant.

[0281] As benzodifuranone-based black pigments, for example, "Irgaphor (registered trademark)" black S0100 manufactured by BASF can be cited, but it is not limited to these. In addition, by mixing a part of benzodifuranone-based black pigments having substituents such as SO3H, SO3- or COOH in the form of a dispersing aid and performing a wet dispersion treatment, the dispersibility can be improved.

[0282] As the perylene-based black pigment, when indicated by a Color Index (CI) number, CI Pigment Black 31 and 32 are exemplified, and for example, FK4280 manufactured by BASF is exemplified, but the present invention is not limited to these.

[0283] The resin composition containing (A) resin in the present invention may further contain a dispersant. The so-called dispersant refers to a dispersant that contains a pigment affinity group having a chemical bond or adsorption effect on the pigment surface and a polymer chain or group having a solvent affinity. As the mechanism of action of the dispersant, in addition to the acid-base interaction, the complex participation of hydrogen bonds, Van-der-Waals forces, etc., in the wet medium dispersion treatment performed when making the pigment dispersion liquid described later, plays the following effects: by improving the wettability of the organic pigment surface to the dispersion medium, and improving the three-dimensional repulsion effect and / or electrostatic repulsion effect of the organic pigments caused by the polymer chain, the pigment is promoted to be miniaturized, and the dispersion stability is improved. By promoting miniaturization and improving dispersion stability, the flexibility can be further improved.

[0284] As the dispersant, a dispersant having a basic adsorption group, a dispersant having an acidic group, or a nonionic dispersant can be preferably used. Examples of the dispersant having a basic adsorption group include DisperBYK-142, 145, 164, 167, 182, 187, 2001, 2008, 2009, 2010, 2013, 2020, 2025, 9076, 9077, BYK-LPN6919, BYK-LP N21116, BYK-JET9152 (all manufactured by BYK-Chemie), "Solsperse (registered trademark)" 9000, 11200, 13650, 20000, 24000, 24000SC, 24000GR, 32000, 32500, 32550, 326000, 33000, 34750, 35100, 35200, 37500, 39000, 56000, 76500 (all manufactured by Lubrizol), Efka-PX4310, 4320, 4710 (all manufactured by BASF). Examples of dispersants having an acidic group include "Tego dispers (registered trademark)" 655 (manufactured by Evonik), DisperBYK-102, 118, 174, 2096 (all manufactured by BYK-Chemie), and examples of nonionic dispersants include "SOLSPERSE (registered trademark)" 54000 (manufactured by Lubrizol), "Tego dispers (registered trademark)" 650, 652, 740W (all manufactured by Evonik). In consideration of the inherent surface properties or average primary particle size of the pigment, these dispersants may be used alone or in combination to obtain an average dispersed particle size described below.

[0285] In terms of sufficient deagglomeration in the wet medium dispersion treatment described later and suppression of reagglomeration after the dispersion treatment, the content of the dispersant is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, relative to 100 parts by mass of the total amount of the pigment. On the other hand, in terms of sufficiently ensuring the content of the constituent components other than the dispersant, it is preferably 100 parts by mass or less, more preferably 60 parts by mass or less.

[0286] The resin composition containing the resin (A) may contain a thermal crosslinking agent, a radical polymerizable compound, an antioxidant, a solvent, a compound having a phenolic hydroxyl group, an adhesion improver, an adhesion improver, and a surfactant as other components as necessary.

[0287] Next, the method for producing the resin composition of the present invention is described. For example, the resin composition can be obtained by mixing and dissolving the resin (A) with the optional (B) photosensitizer, (C) colorant, thermal crosslinking agent, free radical polymerizable compound, antioxidant, solvent, compound having phenolic hydroxyl group, adhesion improver, adhesion improver, surfactant, etc.

[0288] As the dissolving method, conventional methods such as heating and stirring may be mentioned.

[0289] The viscosity of the resin composition is preferably 2 mPa·s to 5,000 mPa·s. By adjusting the solid content concentration so that the viscosity is 2 mPa·s or more, it is easy to obtain the desired film thickness. On the other hand, if the viscosity is 5,000 mPa·s or less, it is easy to obtain a resin film with high uniformity. A resin composition having such a viscosity can be easily obtained, for example, by setting the solid content concentration to 5% by mass to 60% by mass. Here, the so-called solid content concentration refers to the components other than the solvent.

[0290] The obtained resin composition is preferably filtered using a filter to remove foreign matter or particles. The filter material includes polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc., preferably polyethylene or nylon.

[0291] When forming the cured film obtained by curing the resin composition containing the resin (A) resin, a resin sheet may be formed from the resin composition containing the resin (A) resin, and then the resin sheet may be cured to form a film.

[0292] The resin sheet is a sheet formed on a substrate using the resin composition. Specifically, it is a resin sheet obtained by applying the resin composition on a substrate and drying it.

[0293] The substrate for coating the resin composition can be a film such as polyethylene terephthalate (PET). When the resin sheet is attached to a substrate such as a silicon wafer, if it is necessary to peel off the substrate, it is preferred to use a substrate with a release agent such as a silicone resin applied on the surface, so that the resin sheet and the substrate can be easily peeled off.

[0294] Next, a method for manufacturing the display device of the present invention will be described.

[0295] The manufacturing method of the display device of the present invention is a manufacturing method of a display device having at least wiring, a cured film and a plurality of light-emitting elements each including electrodes on two different surfaces, and comprises: a step (D1) of configuring the light-emitting element on a supporting substrate; a step (D2) of forming a resin film comprising a resin composition containing (A) resin on the supporting substrate and the light-emitting element; a step (D3) of forming a plurality of through-opening patterns on the resin film by exposing and developing the resin film; a step (D6) of curing the resin film to form the cured film having a transmittance of 0.1% or more and 95% or less for light of a wavelength of 450 nm at a thickness reference of 1 μm; and a step (D5) of forming the wiring on at least a portion of the surface of the cured film and the opening pattern of the cured film.

[0296] exist Figure 7 2 is a cross-sectional view taken along a plane perpendicular to a supporting substrate, showing a manufacturing process of an example of a display device having a plurality of light-emitting elements of the present invention.

[0297] Hereinafter, the resin film refers to a film obtained by coating a resin composition containing the resin (A) on a substrate or laminating a resin sheet and drying it. Here, there are also cases where the resin composition containing the resin (A) contains a solvent and is recorded as a varnish. In addition, the cured film refers to a film obtained by curing the resin film or the resin sheet.

[0298] exist Figure 7 In a, process (D1) is a process of configuring a light-emitting element 2 on a supporting substrate 18, that is, a light-emitting element 2 including electrodes 6 on two different surfaces. The supporting substrate may be a glass substrate, a silicon substrate, a ceramic, gallium arsenide, an organic circuit substrate, an inorganic circuit substrate, or a supporting substrate having a circuit constituent material configured on these substrates, etc., but is not limited to these. A temporary adhesive material or wiring 4d may be configured on the supporting substrate. In addition, a TFT array substrate may also be used. The supporting substrate may be used as an opposing substrate or a light-emitting element driving substrate, and may also be removed in the middle of the process. In addition, another opposing substrate or a light-emitting element driving substrate may be configured after removal. In Figure 7 In FIG. 1 , a case where a temporary adhesive layer is formed on a supporting substrate 18 and a wiring 4d is formed thereon is shown as an example. The electrode 6 and the wiring 4d may be connected via a bump or a conductive film, or may be directly connected. In addition, the wiring 4d may be connected to the wiring 4 extending in the cured film 3 arranged to be in contact with at least a portion of the light-emitting element 2 via a through electrode, or may be connected to the light-emitting element driving substrate 7.

[0299] Next, step (D2) is as follows Figure 7b is a step of coating a resin composition containing the resin (A) on the supporting substrate 18 and the light emitting element 2 or laminating a resin sheet formed of a resin composition containing the resin (A) to form a resin film 19 .

[0300] In addition, the so-called "on the supporting substrate" and "on the light-emitting element" not only refer to the surface of the supporting substrate or the surface of the light-emitting element, but also refer to the upper side of the supporting substrate or the light-emitting element. A resin film may be formed by coating a resin composition containing (A) resin on a cured film, wiring, or partition wall, or laminating a resin sheet formed from a resin composition containing (A) resin.

[0301] The coating method includes spin coating, slit coating, dip coating, spray coating, printing, etc. The coating film thickness varies depending on the coating technique, solid content concentration of the composition, viscosity, etc., but the coating is usually performed so that the film thickness after drying becomes 0.1 μm to 150 μm.

[0302] Before coating, the supporting substrate for coating the resin composition containing resin (A) may be pre-treated in advance with the adhesion improver described above. For example, the following method can be cited: using a solution in which the adhesion improver is dissolved in isopropanol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, diethyl adipate and other solvents at 0.5% by mass to 20% by mass, the substrate surface is treated by spin coating, slit die coating, rod coating, dip coating, spraying, steam treatment and other methods. After the substrate surface is treated, a reduced pressure drying treatment may be performed as needed. In addition, the reaction between the substrate and the adhesion improver may be carried out by heat treatment at 50°C to 280°C.

[0303] Next, the applied film of the resin composition containing the resin (A) is dried to obtain a resin film 19. Drying is preferably performed using an oven, a hot plate, infrared rays, etc. at 50°C to 140°C for 1 minute to several hours.

[0304] On the other hand, when the resin sheet is used, if there is a protective film on the resin sheet, the protective film is peeled off, and the resin sheet and the supporting substrate are made to face each other and bonded by thermocompression (there is also a case where the process of making the resin sheet and the supporting substrate face each other and bonding by thermocompression is described as laminating the resin sheet on the supporting substrate). Next, the resin sheet laminated on the supporting substrate is dried in the same manner as when the resin film is obtained, thereby forming a resin film 19. The resin sheet can be obtained by applying a resin composition containing the (A) resin on a supporting film containing polyethylene terephthalate or the like as a removable substrate and drying it.

[0305] Thermocompression bonding can be performed by heat pressing, heat lamination, heat vacuum lamination, etc. In terms of adhesion to the substrate and embedding properties, the lamination temperature is preferably 40° C. or higher. In addition, when the resin sheet is photosensitive, in order to prevent the resin film from being hardened during lamination and the resolution of pattern formation in the exposure and development steps from being reduced, the lamination temperature is preferably 140° C. or lower.

[0306] Next, step (D3) is to use a photolithography step to form a resin film 19 such as Figure 7 c is a step of forming a through opening pattern 12 corresponding to the form of the wiring 4.

[0307] Since the resin composition or resin sheet containing the resin (A) can be finely processed, high-density arrangement of light-emitting elements can be achieved.

[0308] A photosensitive resin film is irradiated with chemical radiation through a mask having a desired pattern. Examples of chemical radiation used for exposure include ultraviolet rays, visible rays, electron beams, and X-rays. In the present invention, g-rays (436 nm), h-rays (405 nm), or i-rays (365 nm) are preferably used as common exposure wavelengths. In the case of a non-photosensitive resin film, the chemical radiation is irradiated after a photoresist is formed after the resin film is formed.

[0309] The exposed photosensitive resin film 19 is developed. As a developer, aqueous solutions of alkaline compounds such as tetramethylammonium, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and hexamethylenediamine are preferred. In addition, depending on the situation, one or more of the following can be added to these alkaline aqueous solutions: polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, and dimethylacrylamide; alcohols such as methanol, ethanol, and isopropanol; esters such as ethyl lactate and propylene glycol monomethyl ether acetate; ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, and methyl isobutyl ketone. After development, rinsing with water is usually performed. Here, alcohols such as ethanol and isopropanol; esters such as ethyl lactate and propylene glycol monomethyl ether acetate, etc. may be added to water to perform elution treatment.

[0310] Next, step (D6) is performed by Figure 7 The resin film 19 shown in c is cured to form a cured film 3 having a transmittance of 0.1% or more and 95% or less for light of a wavelength of 450 nm at a thickness reference of 5 μm.

[0311] In addition, step (6) can be a step (D4) of forming a cured film 3 having a transmittance of 0.1% to 79% for light of a wavelength of 450 nm at a thickness reference of 5 μm by curing the resin film 19, or a step (D7) of forming a cured film 3 having a transmittance of 0.1% to 25% for light of a wavelength of 450 nm at a thickness reference of 1 μm by curing the resin film 19.

[0312] The resin film 19 is heated to cause a ring-closing reaction or a thermal cross-linking reaction to be performed, thereby obtaining a cured film 3. The cured film 3 is cross-linked with (A) resins, or with (B) a photosensitive agent or a thermal cross-linking agent, etc., so that the heat resistance and chemical resistance are improved. The heating treatment can be carried out by increasing the temperature in stages, or it can be carried out while continuously increasing the temperature. The heating treatment is preferably carried out for 5 minutes to 5 hours. As an example, an example of heating treatment at 110°C for 30 minutes and then performing a heat treatment at 230°C for 60 minutes can be cited. As a heating treatment condition, it is preferably above 140°C and below 400°C. In order to allow the thermal cross-linking reaction to proceed, the heating treatment condition is preferably above 140°C, and more preferably above 160°C. In addition, in order to provide an excellent cured film and to improve the reliability of the display device, the heating treatment condition is preferably below 300°C, and more preferably below 250°C.

[0313] During heating, the treatment may be carried out in an air environment, or in an environment with a low oxygen concentration in order to suppress fading of the component (C). The oxygen concentration is preferably 1000 ppm or less, more preferably 300 ppm or less, further preferably 100 ppm or less, and particularly preferably 50 ppm or less.

[0314] The cured film obtained in this way has an opening pattern, and the angle of the inclined side of the opening pattern section is preferably 40° or more and 85° or less. If the angle of the cross-sectional shape of the opening is 40° or more, multiple light-emitting elements can be efficiently configured, and high precision can be achieved. The angle of the cross-sectional shape of the opening is more preferably 50° or more. On the other hand, if the angle of the cross-sectional shape of the opening is 85° or less, it is possible to suppress wiring defects such as short circuits in the wiring. The angle of the cross-sectional shape of the opening is more preferably 80° or less.

[0315] exist Fig.16 A cross-sectional view of a surface perpendicular to the support base showing the opening pattern of the cured film is shown in FIG. Fig.16 In the figure, the angle of the inclined side 26 of the opening pattern formed in the cured film 3 is 27. The inclined side is an inclined side connecting the opening pattern at a position 29 which is 1 / 2 in the thickness direction of the cured film 3 and the opening pattern at the bottom with a straight line.

[0316] Then, in Figure 7In c, in order to improve the adhesion between the cured film 3 and the wiring 4, a barrier metal such as titanium is sputtered on the cured film 3, and a copper seed crystal (seed layer) is further formed thereon by a sputtering method.

[0317] Next, step (D5) is as follows Figure 7 d, after forming a photoresist layer (not shown), a wiring 4 made of a metal such as copper or a conductive film is formed on the opening pattern 12 of the cured film 3 and a part of the surface of the cured film 3 by plating, sputtering, processing with a photosensitive conductive paste, etc. The wiring 4 is used to be electrically connected to at least one electrode 6 of the light emitting element 2. Thereafter, unnecessary photoresist, seed layer, and barrier metal are removed.

[0318] Thus, the cured film 3 hides the wiring 4, suppresses the glare of the wiring 4, and makes it difficult to be seen from the outside, thereby improving the design. Furthermore, by reducing the reflection of external light or improving the contrast, the visibility can be improved.

[0319] The method for manufacturing a display device of the present invention preferably includes a step of repeating the step (D2), the step (D3), the step (D6), and the step (D5) a plurality of times to form a plurality of layers of the cured film having the wiring in the cured film.

[0320] The hardened film 3 and the wiring 4 are as follows Figure 7 By repeating the same method again as shown in e to f, the cured film 3 including two or more layers can be formed.

[0321] Thus, by forming a cured film having wiring in a multilayer, a plurality of light emitting elements can be arranged, and wiring defects such as wiring short circuits caused by low-profile packages or short wiring distances can be suppressed, and loss can be reduced, thereby improving high-speed responsiveness.

[0322] Afterwards, if Figure 7 As shown in FIG. g, the barrier metal 9 is formed in the opening pattern 12 of the cured film 3 by sputtering, and the bump 10 is formed. The barrier metal 9 may or may not be provided.

[0323] Afterwards, if Figure 7 h, the support substrate 18 is peeled off, and the counter substrate 5 is bonded with an adhesive, thereby obtaining a display device 1 having a plurality of light emitting elements 2. The wiring 4 may also include an electrode.

[0324] The driving element 8 can be used one or more according to different functions, with respect to one light emitting element 2 or a light emitting element 2 of a unit including red, blue and green, a plurality of light emitting elements 2 or a plurality of light emitting elements 2. Figure 7In the process of , one or more driving elements are arranged near the light emitting element, etc. In this case, the driving element can be electrically connected to the light emitting element 2 via the light emitting element driving substrate 7 or the wiring 4c, the wiring 4 extending in the cured film 3, etc.

[0325] Thus, the cured film hides the wiring, suppresses the glare of the wiring, and makes it difficult to see from the outside, thereby improving the design. Furthermore, by reducing the reflection of external light or increasing the contrast, the visibility can be improved.

[0326] The method for manufacturing a display device of the present invention preferably includes, before the step (D1), a step (D8) of providing a partition wall having a thickness equal to or greater than a thickness of the light-emitting element.

[0327] An example of step (D8) is shown in Fig.17 . Fig.17 a is a step (D8) of providing a partition wall 15 having a thickness greater than that of the light emitting element 2 on the supporting substrate 18. Fig.17 b represents a step (D1) of providing a plurality of light emitting elements 2 between partition walls having a thickness equal to or greater than the thickness of the light emitting element 2 . Fig.17 c is in the state where the partition wall 15 is set, and Figure 7 The process (D2) shown in b is similar to the process of disposing the resin film 19. The following process is as follows Figure 7 As the partition wall, the (A) resin can be used, and existing ones such as epoxy resin, (meth) acrylic polymer, polyurethane, polyester, polyolefin, polysiloxane, etc. can also be used. In addition, a light shielding part or a reflecting part can also be provided.

[0328] In the manufacturing method of the display device of the present invention, it is preferred that a step (D9) is further included after the step (D5), wherein the step (D9) includes a driving element and a substrate, the driving element is connected to the light-emitting element via wiring, and further, at least a portion of the wiring extends on the side of the substrate.

[0329] An example of step (D9) is shown in Figure 7 . Figure 7 h represents a step (D9) of providing a driving element and a substrate, and connecting the driving element to the light emitting element via wiring. Figure 7 h is connected to the light emitting element 2 via the wiring 4 or the wiring 4c, and a part of the wiring 4c extends on the side of the light emitting element driving substrate 7. In addition, when the light emitting element driving substrate 7 has a through electrode, it can also be connected to the driving element 8 via the through electrode.

[0330] This can reduce the height of the display device itself or improve the high-speed response, thereby making the display device more compact and having a narrow frame.

[0331] The method for manufacturing a display device of the present invention preferably further comprises a step (D10) of providing a light shielding layer between the plurality of light emitting elements.

[0332] An example of step (D10) is shown in Fig.18 . Fig.18 a represents a step (D10) of providing a light shielding layer 25 between a plurality of light emitting elements 2. The light shielding layer 25 may be formed before or after the light emitting elements 2 are formed.

[0333] The light shielding layer 25 may include a cured film formed by curing a resin composition containing (A) resin and (E) coloring material. In addition, it may also contain materials other than the resin composition containing (A) resin, and existing materials such as epoxy resin, (meth) acrylic polymer, polyurethane, polyester, polyolefin, polysiloxane, etc. can be used. As the (E) coloring material, a black pigment can be used, for example, black organic pigments such as carbon black, perylene black, and aniline black; graphite; and inorganic pigments such as metal particles, metal oxides, composite oxides, metal sulfides, metal nitrides, and metal nitride oxides of titanium, copper, iron, manganese, cobalt, chromium, nickel, zinc, calcium, and silver. In addition, a red pigment and a blue pigment or a yellow pigment or other pigments as needed can be combined to make black. In addition, dyes can also be used. It can also contain two or more coloring materials.

[0334] The resin composition containing the (A) resin and the (E) coloring material may be provided with photosensitivity, and the (B) photosensitizer described later may also be used.

[0335] As a method for forming a light-shielding layer, a photolithography process can be used in the case of photosensitivity. In the case of no photosensitivity, a photolithography process or an etching process can be used after forming a photoresist on the light-shielding layer, or an etching process using a mask can be used. By heat-treating the obtained pattern (post-baking), a patterned colored film can be obtained. The heat treatment can be carried out in air, under a nitrogen environment, and in a vacuum state. The heating temperature is preferably 100°C to 300°C, and the heating time is preferably 0.25 hours to 5 hours. The heating temperature can be changed continuously or in stages.

[0336] The manufacturing method of the display device of the present invention is a manufacturing method of a display device having at least wiring, a cured film and a plurality of light-emitting elements each including electrodes on two different surfaces, and comprises: a step (E1) of configuring a pad on a supporting substrate; a step (E2) of forming a resin film comprising a resin composition containing (A) resin on the supporting substrate and the pad; a step (E3) of forming a plurality of through-opening patterns in the resin film by exposing and developing the resin film; a step (E10) of curing the resin film to form the cured film having a transmittance of 0.1% or more and 95% or less of light of a wavelength of 450 nm at a thickness reference of 1 μm; a step (E5) of forming the wiring on at least a portion of the surface of the cured film and the opening pattern of the cured film; and a step (E6) of configuring the light-emitting element on the cured film in a manner that maintains electrical connection with the wiring.

[0337] exist Figure 8 2 is a cross-sectional view of a surface perpendicular to a support base or a counter substrate, showing another example of a manufacturing process of the display device 1 of the present invention. Figure 7 The process is repeated, specifically Figure 8 b~e due to Figure 7 b to f are repeated, so their description is omitted.

[0338] Step (E1) is as follows Figure 8 A step of disposing the pad 17 on the supporting substrate 18 as shown in FIG.

[0339] Examples of the pad include copper and aluminum.

[0340] Next, step (E2) is as follows Figure 8 As shown in b, a resin composition containing the resin (A) is applied onto the support substrate 18 and the pad 17 or a resin sheet is laminated to form the resin film 19.

[0341] In addition, the so-called on the supporting substrate and on the pad does not only refer to the surface of the supporting substrate or the surface of the pad, but also refers to the upper side of the supporting substrate or the pad. The resin film can also be formed by coating a resin composition containing (A) resin on the cured film, wiring, or partition, or laminating a resin sheet formed by a resin composition containing (A) resin.

[0342] Next, step (E3) is as follows Figure 8 As shown in c, a step of forming a plurality of penetrating opening patterns 12 in the resin film 19 using a photolithography step.

[0343] Next, step (E10) is as follows Figure 8 As shown in c, the resin film 19 is cured to form a cured film 3 having a transmittance of 0.1% or more and 95% or less at a wavelength of 450 nm at a thickness of 1 μm.

[0344] In addition, it can be a process (E4) of forming a cured film 3 having a transmittance of 0.1% to 79% for light of 450 nm at a thickness reference of 5 μm by curing the resin film 19, and it can be a process (E8) of forming a cured film 3 having a transmittance of 0.1% to 25% for light of 450 nm at a thickness reference of 1 μm by curing the resin film 19.

[0345] Then, in Figure 8 In c, in order to improve the adhesion between the cured film 3 and the wiring 4, a barrier metal such as titanium is sputtered on the cured film 3, and a copper seed crystal (seed layer) is further formed thereon by a sputtering method.

[0346] Next, step (E5) is as follows Figure 8 d, after forming a photoresist layer (not shown), a process of forming wiring 4 made of copper or a conductive film on the opening pattern 12 of the cured film 3 and a part of the surface of the cured film 3 by plating, sputtering, processing with a photosensitive conductive paste, etc. Thereafter, unnecessary photoresist, seed layer, and barrier metal are removed.

[0347] The method for manufacturing a display device of the present invention preferably includes a step of repeating the step (E2), the step (E3), the step (E10), and the step (E5) a plurality of times to form a plurality of cured films each having the wiring therein.

[0348] The hardened film 3 and the wiring 4 are as follows Figure 8 By repeating the same method as shown in b to d, Figure 8 As shown in e, a cured film 3 including two or more layers is formed.

[0349] Next, step (E6) is as follows Figure 8 As shown in f, the light emitting element 2 is disposed on the cured film 3 so as to be electrically connected to the wiring 4. The electrode 6 of the light emitting element 2 and the wiring 4 may be directly connected or may be connected through, for example, a bump or a conductive film.

[0350] In addition, it is preferred to have Figure 8 g, forming a cured film 21 on the cured film 3 and the light emitting element 2 (E7). As the cured film 21, it is preferred that a resin film containing the resin composition is formed by coating a resin composition containing the resin (A) or laminating a resin sheet containing the resin composition containing the resin (A) and then curing to form the cured film 21. In addition, a material other than the resin composition containing the resin (A) may be contained, and existing materials such as epoxy resin, silicone resin, and fluororesin can be used.

[0351] The curing conditions vary depending on the type of resin, and examples thereof include 80° C. to 230° C. and 15 minutes to 5 hours.

[0352] The purpose is to protect the light-emitting element or to planarize the light-emitting element by forming a cured film on the light-emitting element.

[0353] In addition, Figure 8 In FIG. 6 , after forming the cured film 21, a wiring 4d is formed thereon as an example. The electrode 6 and the wiring 4d may be connected via a bump or a conductive film, or may be directly connected. In addition, the wiring 4d may be connected to the wiring 4 extending in the cured film 3 arranged to be in contact with at least a portion of the light-emitting element 2 via a through electrode, or may be connected to the light-emitting element driving substrate 7.

[0354] Afterwards, if Figure 8 As shown in FIG. 1 , the counter substrate 5 is bonded to the cured film 21 using an adhesive or the like. The support substrate 18 is peeled off, and the barrier metal 9 and the bumps 10 are formed, and are electrically connected to the light emitting element driving substrate 7 to which the driving element 8 such as a driver IC is attached via the bumps 10 .

[0355] The driving element 8 is electrically connected to the light emitting element 2 via the wiring 4 extending in the cured film 3, thereby obtaining a display device 1 having a plurality of light emitting elements 2. In addition, the wiring 4 may also include an electrode.

[0356] The driving element 8 can be used one or more according to different functions, with respect to one light emitting element 2 or a light emitting element 2 of a unit including red, blue and green, a plurality of light emitting elements 2 or a plurality of light emitting elements 2. Figure 8 In the process of , one or more driving elements are arranged near the light emitting element, etc. In this case, the driving element can be electrically connected to the light emitting element 2 via the light emitting element driving substrate 7 or the wiring 4c, the wiring 4 extending in the cured film 3, etc.

[0357] Thus, the cured film 3 hides the wiring 4, suppresses the glare of the wiring 4, and makes it difficult to be seen from the outside, thereby improving the design. Furthermore, by reducing the reflection of external light or improving the contrast, the visibility can be improved.

[0358] The method for manufacturing a display device of the present invention preferably includes, after the step (E5), a step (E9) of providing a partition wall having a thickness equal to or greater than a thickness of the light-emitting element.

[0359] An example of step (E9) is shown in Fig. 9 . Fig. 9 f indicates that in the formation of multiple layers Figure 8 e) after the cured film 3 is provided with the partition wall 15 (E9). Fig. 9g, a light emitting element 2 is provided between the partition walls 15, and then, Fig. 9 The wiring 4d is electrically connected to the electrode 6 as shown in h. In addition, the opposing substrate 5 is adhered to the upper part of the partition wall 15 and the light-emitting element 2, and the supporting substrate 18 is peeled off to form a barrier metal 9 and a bump 10, which is electrically connected to the light-emitting element driving substrate 7 having a driving element 8 such as a driver IC via the bump 10.

[0360] The manufacturing method of the display device of the present invention preferably further includes a step (E11) after the step (E7), wherein the step (E11) includes a driving element and a substrate, the driving element is connected to the light-emitting element via wiring, and further, at least a portion of the wiring extends on the side of the substrate.

[0361] An example of step (E11) is shown in Figure 8 . Figure 8 h represents a step (E11) of providing a driving element and a substrate and connecting the driving element to the light emitting element via wiring. Figure 8 h is connected to the light emitting element 2 via the wiring 4 or the wiring 4c, and a part of the wiring 4c extends on the side of the light emitting element driving substrate 7. In addition, when the light emitting element driving substrate 7 has a through electrode, it can also be connected to the driving element 8 via the through electrode.

[0362] This can reduce the height of the display device itself or improve the high-speed response, thereby making the display device more compact and having a narrow frame.

[0363] The method for manufacturing a display device of the present invention is a method for manufacturing a display device having at least wiring, a cured film, and a plurality of light-emitting elements each including electrodes on two different surfaces, and comprises: a step (F1) of forming a resin film containing a resin composition containing (A) resin on a substrate or the like; a step (F2) of forming a plurality of through-opening patterns in the resin film by exposing and developing the resin film; a step (F3) of curing the resin film to form the cured film having a transmittance of light of a wavelength of 450 nm of 0.1% or more and 95% or less at a thickness reference of 1 μm; a step (F4) of forming the wiring on at least a portion of the surface of the cured film and a portion of the opening pattern of the cured film; and a step (F5) of arranging the light-emitting element on the cured film in a manner that maintains electrical connection with the wiring.

[0364] exist Fig.19 2 is a cross-sectional view taken along a plane perpendicular to a light emitting element driving base, showing an example of a manufacturing process of the display device 1 according to the second embodiment of the present invention.

[0365] The process (F1) is as follows Fig.19A step of forming a resin film made of a resin composition containing the resin (A) on a substrate etc. as shown in a. The resin film may be formed by coating a resin composition containing the resin (A) or laminating a resin sheet formed of a resin composition containing the resin (A).

[0366] As the substrate, a light emitting element driving substrate 7 can be used. Fig.19 A shows a TFT array substrate in which TFTs 22 , an insulating film 23 , and wirings 4 are arranged on a glass substrate as an example.

[0367] The insulating film 23 is not particularly limited, and examples thereof include a silicon oxide film, a silicon nitride film, and an insulating film containing an organic substance.

[0368] Next, the process (F2) is as follows Fig.19 As shown in a, a process of forming a plurality of penetrating opening patterns in a resin film using a photolithography process.

[0369] Next, the process (F3) is as follows Fig.19 A step of forming a cured film 3 having a transmittance of 0.1% to 95% at a wavelength of 450 nm at a thickness of 1 μm by curing the resin film as shown in a.

[0370] Next, the process (F4) is as follows Fig.19 b) is a process for forming wiring on at least a portion of the surface of the cured film and a portion of the opening pattern of the cured film. This is a process for forming wiring 4e on a portion of the surface of the cured film 3 by, for example, sputtering or processing with a photosensitive conductive paste after forming a photoresist layer (not shown). Thereafter, unnecessary photoresist is removed.

[0371] As wiring 4e, gold, silver, copper, aluminum, nickel, titanium, molybdenum or alloys containing these or compounds containing oxides of at least one element selected from the group consisting of indium, gallium, zinc, tin, titanium and niobium as main components; or photosensitive conductive pastes containing organic matter and conductive particles, etc., but other existing ones may also be used.

[0372] The method for manufacturing a display device of the present invention preferably includes a step of repeating the step (F2), the step (F3), and the step (F4) a plurality of times to form a plurality of cured films each having the wiring therein.

[0373] The cured film 3 is then repeatedly processed in the same manner, so that Fig.19 As shown in c, a cured film 3 including two or more layers is formed. Thereafter, wiring 4c is formed.

[0374] Next, the process (F5) is as follows Fig.19d is a step of arranging the light emitting element 2 on the cured film 3 so as to maintain electrical connection with the wiring 4e. The electrode 6 and the wiring 4e may be connected via a bump or a conductive film, or may be directly connected.

[0375] In addition, the partition wall 15 may be formed before or after the light emitting element 2 is arranged. Then, the wiring 4d is formed after the cured film 21 is formed. The wiring 4d may be connected to the wiring 4 and the wiring 4e extending in the cured film 3 arranged to be in contact with at least a part of the light emitting element 2 via a through electrode or the like, or may be connected to the light emitting element driving substrate 7.

[0376] Afterwards, if Fig.19 e) and the counter substrate 5 is bonded using an adhesive or the like. In addition, a driving element 8 such as a driver IC is electrically connected to the light emitting element 2 via the wiring 4c or the wiring 4 and wiring 4e extending in the cured film 3, thereby obtaining a display device 1 having a plurality of light emitting elements 2. In addition, the wiring 4d and wiring 4e also include electrodes.

[0377] The driving element 8 can be used one or more according to different functions, with respect to one light emitting element 2 or a light emitting element 2 of a unit including red, blue and green, a plurality of light emitting elements 2 or a plurality of light emitting elements 2. Fig.19 In the process of , one or more driving elements are arranged near the light emitting element, etc. In this case, the driving element can be electrically connected to the light emitting element 2 via the light emitting element driving substrate 7 or the wiring 4c, the wiring 4 extending in the cured film 3, etc.

[0378] Thus, the hardened film can be used to ensure the electrical insulation of the wiring, and the electrodes of the light-emitting element are electrically connected to the driving element by extending the wiring in the hardened film, thereby controlling the light-emitting action. In addition, the hardened film hides the wiring, which can suppress the glare of the wiring and make it difficult to see from the outside, thereby improving the design. Furthermore, by reducing the reflection of external light or increasing the contrast, the visibility can be improved.

[0379] The manufacturing method of the display device of the present invention is a manufacturing method of a display device having at least wiring, a cured film and a plurality of light-emitting elements each including electrodes on two different surfaces, and may include: a step (G1) of forming a resin film containing a resin composition containing (A) resin on a substrate or the like; a step (G2) of forming a plurality of through-opening patterns in the resin film by exposing and developing the resin film; a step (G3) of curing the resin film to form the cured film having a transmittance of 0.1% or more and 95% or less of light of a wavelength of 450 nm at a thickness reference of 1 μm; a step (G4) of forming the wiring on at least a portion of the surface of the cured film and a portion of the opening pattern of the cured film; and a step (G5) of configuring the light-emitting element in a manner that maintains electrical connection with the wiring.

[0380] exist Fig.29 2 is a cross-sectional view taken along a plane perpendicular to a light emitting element driving substrate, showing an example of a manufacturing process of the display device 1 according to the second embodiment of the present invention.

[0381] The process (G1) is as follows Fig.29 A step of forming a resin film made of a resin composition containing the resin (A) on a substrate etc. as shown in a. The resin film may be formed by coating a resin composition containing the resin (A) or laminating a resin sheet formed of a resin composition containing the resin (A).

[0382] As the substrate, a light emitting element driving substrate 7 can be used. Fig.29 A shows a TFT array substrate in which TFTs 22 , an insulating film 23 , and wirings 4 are arranged on a glass substrate as an example.

[0383] The insulating film 23 is not particularly limited, and examples thereof include a silicon oxide film, a silicon nitride film, and an insulating film containing an organic substance.

[0384] Next, the process (G2) is as follows Fig.29 As shown in a, a process of forming a plurality of penetrating opening patterns in a resin film using a photolithography process.

[0385] Next, step (G3) is as follows Fig.29 A step of forming a cured film 3 having a transmittance of 0.1% to 95% at a wavelength of 450 nm at a thickness of 1 μm by curing the resin film as shown in a.

[0386] Next, step (G4) is as follows Fig.29 b) is a process for forming wiring on at least a portion of the surface of the cured film and a portion of the opening pattern of the cured film. This is a process for forming wiring 4e on a portion of the surface of the cured film 3 by, for example, sputtering or processing with a photosensitive conductive paste after forming a photoresist layer (not shown). Thereafter, unnecessary photoresist is removed.

[0387] As wiring 4e, gold, silver, copper, aluminum, nickel, titanium, molybdenum or alloys containing these or compounds containing oxides of at least one element selected from the group consisting of indium, gallium, zinc, tin, titanium and niobium as main components; or photosensitive conductive pastes containing organic matter and conductive particles, etc., but other existing ones may also be used.

[0388] Afterwards, if Fig.29 The wiring 4c is formed as shown in c.

[0389] Next, step (G5) is as follows Fig.29d is a step of arranging the light emitting element 2 so as to be electrically connected to the wiring 4e. The electrode 6 and the wiring 4e may be connected via a bump or a conductive film, or may be directly connected.

[0390] The cured film 3 or the partition wall 15 may be formed before or after the light emitting element 2 is arranged. Then, after the cured film 21 is formed, the wiring 4d is formed. The wiring 4d may be connected to the wiring 4 and the wiring 4e extending in the cured film 3 arranged to be in contact with at least a portion of the light emitting element 2 via a through electrode or the like, or may be connected to the light emitting element driving substrate 7.

[0391] Afterwards, if Fig.29 e) and the counter substrate 5 is bonded using an adhesive or the like. In addition, a driving element 8 such as a driver IC is electrically connected to the light emitting element 2 via the wiring 4c or the wiring 4 and wiring 4e extending in the cured film 3, thereby obtaining a display device 1 having a plurality of light emitting elements 2. In addition, the wiring 4d and wiring 4e also include electrodes.

[0392] The driving element 8 can be used one or more according to different functions, with respect to one light emitting element 2 or a light emitting element 2 of a unit including red, blue and green, a plurality of light emitting elements 2 or a plurality of light emitting elements 2. Fig.29 In the process of , one or more driving elements are arranged near the light emitting element, etc. In this case, the driving element can be electrically connected to the light emitting element 2 via the light emitting element driving substrate 7 or the wiring 4c, the wiring 4 extending in the cured film 3, etc.

[0393] Thus, the hardened film can be used to ensure the electrical insulation of the wiring, and the electrodes of the light-emitting element are electrically connected to the driving element by extending the wiring in the hardened film, thereby controlling the light-emitting action. In addition, the hardened film hides the wiring, which can suppress the glare of the wiring and make it difficult to see from the outside, thereby improving the design. Furthermore, by reducing the reflection of external light or increasing the contrast, the visibility can be improved.

[0394] The display device of the present invention can be suitably used for display devices such as various LED displays, various vehicle-mounted lamps, and the like.

[0395] Example

[0396] The present invention will be described below with reference to Examples, but the present invention is not limited to these Examples.

[0397] Moreover, the display device in the Example or the evaluation of the cured film containing the resin composition used for the display device was performed by the following method.

[0398] <Evaluation method of light transmittance of cured film>

[0399] On a 5 cm square glass substrate, a varnish containing a resin composition was spin-coated so that the film thickness after heating at 230°C for 1 hour was 1.0 μm or more, and pre-baked at 120°C for 3 minutes. Then, using a high-temperature clean oven CLH-21CD-S manufactured by Koyo Thermo Systems (Co., Ltd.), the temperature was raised from 50°C to 110°C at a rate of 3.5°C / min at an oxygen concentration of 100 ppm or less under a nitrogen flow, and the heating treatment was continued at 110°C for 30 minutes. Thereafter, the temperature was raised to 230°C as a heating temperature at 3.5°C / min, and the heating treatment was continued for 1 hour at the heating temperature after the temperature increase, and the coated film was dried and heated to obtain a cured film. The film thickness of the coating film after prebaking and development was measured using an optical interference film thickness measuring device LambdaAce STM-602 manufactured by Dainippon Screen Manufacturing Co., Ltd., with a refractive index of 1.629. The film thickness of the cured film was measured with a refractive index of 1.629.

[0400] The transmittance of the cured film obtained in this manner was measured at a wavelength of 450 nm using a double beam spectrophotometer U-2910 (manufactured by Hitachi Hi-Tech Science Co., Ltd.) When the film thickness of the heat-resistant resin film after the heat treatment is not 1.0 μm or 5.0 μm, the film thickness of the measured transmission spectrum was converted to 1.0 μm or 5.0 μm according to Lambert's law.

[0401] <Evaluation method for concealment of wiring obtained by cured film>

[0402] The hiding property of the wiring obtained by the cured film was evaluated using the display device described in the following examples and comparative examples. A microscope was used for the measurement. Whether the glare of the wiring was suppressed and the wiring was hidden was visually evaluated using a microscope. Display devices in which the glare of at least a part of the wiring was suppressed by the cured film and was not easily visible were considered to be hidden and set to good and 2, and display devices in which the wiring could be clearly confirmed by visual observation through the cured film were considered to be poor and 1.

[0403] <Evaluation of opening pattern shape of cured film composed of resin composition>

[0404] A varnish containing a resin composition was prepared, and the varnish was applied to an 8-inch silicon wafer by spin coating using a coating and developing device ACT-8 (manufactured by Tokyo Electron Co., Ltd.) so that the film thickness after heat treatment was 5 μm, and pre-baked to prepare a pre-baked film. The pre-baking was performed at 120° C. for 3 minutes. Thereafter, an i-ray stepper (manufactured by Nikon Co., Ltd., NSR-2205i14) was used at 50 mJ / cm 2 ~1000mJ / cm 2 The exposure is performed with an exposure amount of . The size of the circular pattern used in the exposure is 5μm to 30μm. After exposure, a 2.38% by mass tetramethylammonium (tetramethylammonium hydroxide (TMAH)) aqueous solution (manufactured by Tama Chemical Industry) is used to develop under conditions such that the film thickness of the unexposed part before and after development changes to 1.0μm to 1.5μm, and then it is rinsed with pure water and spin-dried to obtain a pattern-forming film. Alternatively, cyclopentanone is used for development, and spin-dried to obtain a pattern-forming film. In the case of non-photosensitive materials, exposure and development are performed after a photoresist is formed before exposure, and the photoresist is removed after development. In addition, the film thickness after pre-baking and development is measured using Lambda Ace STM-602, an optical interference film thickness measuring device manufactured by Dainippon Screen Manufacturing Co., Ltd., with the refractive index set to 1.629.

[0405] After development, the temperature was raised from 50° C. to 100° C. at a rate of 3.5° C. / min at an oxygen concentration of 20 ppm or less under a nitrogen flow using an inert oven CLH-21CD-S (manufactured by Koyo Thermo Systems Co., Ltd.), and heat treatment was continued at 100° C. for 30 minutes. Thereafter, the temperature was raised to 230° C. at a rate of 3.5° C. / min, and heat treatment was continued for 1 hour to cure the pattern-forming film to obtain a cured film.

[0406] When the temperature becomes 50°C or lower, the wafer is taken out, and then the wafer is cut, and the cross-sectional shape of the circular pattern of 5 μm to 30 μm is observed and measured using a scanning electron microscope S-4800 (manufactured by Hitachi Hi-Tech). In addition, the opening pattern at the position of 1 / 2 in the thickness direction of the cured film and the opening pattern at the bottom are connected by a straight line as an inclined side, and the angle of the inclined side is calculated.

[0407] As a result, those with an angle of the inclined side of 55° or more and 80° or less were evaluated as grade A, those with an angle of 40° or more and less than 55° or greater than 80° and less than 85° were evaluated as grade B, and those with an angle of less than 40° or greater than 85° were evaluated as grade C.

[0408] <Synthesis Example 1 Synthesis of hydroxyl-containing diamine compound>

[0409] 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (manufactured by Central Glass Co., Ltd., hereinafter referred to as BAHF) was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide (manufactured by Tokyo Chemical Industry Co., Ltd.), and the mixture was cooled to -15°C. A solution prepared by dissolving 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) in 100 mL of acetone was added dropwise thereto. After completion of the dropwise addition, the mixture was stirred at -15°C for 4 hours, and then returned to room temperature. The precipitated white solid was separated by filtration and vacuum dried at 50°C.

[0410] 30 g of the obtained white solid was placed in a 300 mL stainless steel autoclave, dispersed in 250 mL of methyl cellosolve, and 2 g of 5% palladium-carbon (produced by Wako Pure Chemical Industries, Ltd.) was added. Hydrogen was introduced by balloon, and reduction reaction was carried out at room temperature. After about 2 hours, it was confirmed that the balloon no longer shrank and the reaction was terminated. After the reaction was completed, the palladium compound as a catalyst was removed by filtration, and concentrated by rotary evaporator to obtain a hydroxyl-containing diamine compound represented by the following formula.

[0411] [Chemistry 8]

[0412]

[0413] <Synthesis Example 2 Synthesis of polybenzoxazole precursor (A-1)>

[0414] Under a dry nitrogen stream, 1.5 g (0.0075 mol) of 4,4'-diaminodiphenyl ether (hereinafter referred to as 4,4'-DAE), 12.8 g (0.035 mol) of BAHF, and 5.0 g (0.0050 mol) of RT-1000 (manufactured by Huntsman Co., Ltd.) were dissolved in 100 g of NMP. Diimidazole dodecanoate (7.4 g, 0.023 mol) and 1,1'-(4,4'-oxybenzoyl)diimidazole (hereinafter referred to as PBOM) (8.1 g, 0.023 mol) were added thereto together with 25 g of NMP, and the mixture was reacted at 85°C for 3 hours. Next, 0.6 g (0.0025 mole) of 1,3-bis(3-aminopropyl)tetramethyldisiloxane (hereinafter referred to as SiDA), 0.8 g (0.0025 mole) of 4,4'-oxydiphthalic anhydride (hereinafter referred to as ODPA), and 0.8 g (0.0050 mole) of 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also recorded as NA) were added together with 25 g of NMP, and reacted at 85°C for 1 hour. After the reaction was completed, it was cooled to room temperature, and 13.2 g (0.25 mole) of acetic acid was added together with 25 g of NMP, and stirred at room temperature for 1 hour. After the stirring was completed, the solution was put into 1.5 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and dried for three days using a ventilated dryer at 50°C to obtain a powder of a polybenzoxazole precursor (A-1).

[0415] <Synthesis Example 3 Synthesis of polybenzoxazole precursor (A-2)>

[0416] Under a dry nitrogen stream, 27.5 g of BAHF (0.075 mol) was dissolved in 257 g of NMP. 17.2 g of PBOM (0.048 mol) was added thereto together with 20 g of NMP, and the mixture was reacted at 85° C. for 3 hours. Subsequently, 20.0 g (0.02 mol) of RT-1000 (manufactured by Huntsman Co., Ltd.), 1.2 g (0.005 mol) of SiDA, and 14.3 g (0.04 mol) of PBOM were added together with 50 g of NMP, and the mixture was reacted at 85° C. for 1 hour. Furthermore, 3.9 g (0.024 mol) of 5-norbornene-2,3-dicarboxylic anhydride as a terminal blocking agent was added together with 10 g of NMP, and the mixture was reacted at 85° C. for 30 minutes. After the reaction was completed, the mixture was cooled to room temperature, and 52.8 g (0.50 mol) of acetic acid was added together with 87 g of NMP, and stirred at room temperature for 1 hour. After the stirring was completed, the solution was put into 3 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and dried for three days in a ventilated dryer at 50° C. to obtain a powder of a polybenzoxazole precursor (A-2).

[0417] <Synthesis Example 4 Synthesis of polyimide precursor (A-3)>

[0418] Under a dry nitrogen stream, 51.9 g (0.086 mole) of the hydroxyl-containing diamine obtained in Synthesis Example 1 and 1.0 g (0.004 mole) of SiDA were dissolved in 200 g of NMP. 31.0 g (0.10 mole) of ODPA was added thereto, and the mixture was stirred at 40°C for 2 hours. Then, 1.1 g (0.01 mole) of 3-aminophenol (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a capping agent together with 10 g of NMP, and the mixture was reacted at 40°C for 1 hour. After that, a solution prepared by diluting 7.1 g (0.06 mole) of dimethylformamide dimethyl acetal (manufactured by Mitsubishi Rayon Co., Ltd., hereinafter referred to as DFA) with 5 g of NMP was added dropwise. After the addition, stirring was continued at 40°C for 2 hours. After the stirring was completed, the solution was put into 2 L of water, and the precipitate of the polymer solid was collected by filtration. Furthermore, the mixture was washed three times with 2 L of water, and the collected polymer solid was dried in a vacuum dryer at 50° C. for 72 hours to obtain a polyimide precursor (A-3).

[0419] <Synthesis Example 5 Synthesis of polyimide precursor (A-4)>

[0420] Under a dry nitrogen stream, 41.1 g (0.068 mole) of the hydroxyl-containing diamine obtained in Synthesis Example 1, 18.0 g (0.018 mole) of a diamine containing propylene oxide and a tetramethylene ether glycol structure (RT-1000, manufactured by HUNTSMAN (HUNTSMAN)) and 1.0 g (0.004 mole) of SiDA were dissolved in 200 g of NMP. 31.0 g (0.10 mole) of ODPA was added thereto, and the mixture was stirred at 40°C for 2 hours. Then, 1.1 g (0.01 mole) of 3-aminophenol as a capping agent was added together with 10 g of NMP, and the mixture was reacted at 40°C for 1 hour. Thereafter, a solution prepared by diluting 6.0 g (0.05 mole) of DFA with 5 g of NMP was added dropwise. After the addition, stirring was continued at 40°C for 2 hours. After the stirring was completed, the solution was put into 2 L of water, and the precipitate of the polymer solid was collected by filtration. Furthermore, the mixture was washed three times with 2 L of water, and the collected polymer solid was dried in a vacuum dryer at 50° C. for 72 hours to obtain a polyimide precursor (A-4).

[0421] <Synthesis Example 6 Synthesis of polyimide (A-5)>

[0422] Under a dry nitrogen stream, BAHF 29.3g (0.08 mol), SiDA 1.2g (0.005 mol), and 3.3g (0.03 mol) of 3-aminophenol as a capping agent were dissolved in NMP 80g. ODPA 31.2g (0.1 mol) was added together with NMP 20g, and the mixture was reacted at 60°C for 1 hour, followed by stirring at 180°C for 4 hours. After stirring, the solution was added to 3L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and dried in a vacuum dryer at 80°C for 20 hours to obtain a powder of polyimide (A-5).

[0423] <Synthesis Example 7 Synthesis of Cardol Resin (A-6)>

[0424] Under a dry nitrogen stream, a four-necked flask equipped with a reflux cooler was charged with 198.53 g of a 50% propylene glycol monomethyl ether acetate (PGMEA) solution of an equivalent reaction product of a bisphenol fluorene type epoxy resin and acrylic acid (manufactured by Nippon Steel Chemical Co., Ltd., product name "ASF-400" solution), 39.54 g (0.12 mol) of benzophenonetetracarboxylic dianhydride, 8.13 g (0.08 mol) of succinic anhydride, 48.12 g of PGMEA and 0.45 g of triphenylphosphine. The mixture was stirred at 120° C. to 125° C. for 1 hour, and then heated and stirred at 75° C. to 80° C. for 6 hours. Thereafter, 8.6 g of glycidyl methacrylate was added, and the mixture was stirred at 80° C. for 8 hours to obtain a resin (A-6) having a skeleton structure in which two cyclic structures are bonded to a quaternary carbon atom constituting a cyclic structure.

[0425] <Synthesis Example 8 Synthesis of phenol resin (A-7)>

[0426] Under a dry nitrogen stream, 108.1 g (1.0 mol) of m-cresol, 34.0 g (0.32 mol) of benzaldehyde, 90.4 g (0.74 mol) of salicylaldehyde, 200 g of ethanol, and 8.6 g (0.05 mol) of p-toluenesulfonic acid were placed in a reaction vessel and reacted at 65° C. under reflux for 18 hours. The reaction system was neutralized with caustic soda, and then methyl isobutyl ketone and water were added, and liquid separation and washing were performed 5 times. Methyl isobutyl ketone was removed by reduced pressure distillation at 100° C. using an evaporator to obtain a phenol resin (A-7).

[0427] <Synthesis Example 9 Synthesis of photosensitizer (quinonediazide compound) (B-1)>

[0428] Under a dry nitrogen stream, 21.2 g (0.05 mol) of 4,4'-[1-[4-[1-(4-hydroxyphenyl-1)-1-methylethyl]phenyl]ethylidene]bisphenol (manufactured by Honshu Chemical Industry Co., Ltd., hereinafter referred to as TrisP-PA) and 26.8 g (0.10 mol) of 5-naphthoquinonediazidesulfonyl chloride (manufactured by Toyo Gosei Co., Ltd., NAC-5) were dissolved in 450 g of γ-butyrolactone (hereinafter referred to as GBL) at room temperature. 12.7 g of triethylamine mixed with 50 g of γ-butyrolactone was added dropwise so that the temperature in the system would not exceed 35°C. After the addition, the mixture was stirred at 40°C for 2 hours. The triethylamine salt was filtered and the filtrate was poured into water. Thereafter, the precipitate was collected by filtration and washed with 1 L of 1% hydrochloric acid water. Thereafter, the mixture was washed twice with 2 L of water. The precipitate was dried using a vacuum dryer to obtain a quinonediazide compound (B-1) represented by the following formula.

[0429] [Chemistry 9]

[0430]

[0431] <Synthesis Example 10 Synthesis of photosensitizer (quinonediazide compound) (B-2)>

[0432] Under a dry nitrogen stream, 21.2 g (0.05 mol) of TrisP-PA and 26.8 g (0.10 mol) of 4-naphthoquinonediazidesulfonyl chloride (manufactured by Toyo Gosei Co., Ltd., NAC-5) were dissolved in 450 g of γ-butyrolactone at room temperature. 12.7 g of triethylamine mixed with 50 g of γ-butyrolactone was added dropwise in such a way that the temperature in the system would not exceed 35°C. After the addition, the mixture was stirred at 40°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. Thereafter, the precipitate was collected by filtration, and then washed with 1 L of 1% hydrochloric acid water. Thereafter, the mixture was washed twice with 2 L of water. The precipitate was dried using a vacuum dryer to obtain a quinonediazide compound (B-2) represented by the following formula.

[0433] [Chemistry 10]

[0434]

[0435] <Synthesis Example 11 Synthesis of polyimide precursor (A-8)>

[0436] Under a dry nitrogen stream, 3.2 g (0.03 mol) of 1,4-p-phenylenediamine and 12.0 g (0.06 mol) of 4,4'-DAE were dissolved in 200 g of NMP. 31.0 g (0.10 mol) of ODPA was added thereto, and the mixture was stirred at 40°C for 2 hours. Then, 1.1 g (0.01 mol) of 3-aminophenol (manufactured by Tokyo Chemical Industry Co., Ltd.) as a capping agent was added together with 10 g of NMP, and the mixture was reacted at 40°C for 1 hour. After that, a solution prepared by diluting 7.1 g (0.06 mol) of DFA with 5 g of NMP was added dropwise. After the addition, stirring was continued at 40°C for 2 hours. After the stirring was completed, the solution was added to 2 L of water, and the precipitate of the polymer solid was collected by filtration. Furthermore, the mixture was washed three times with 2 L of water, and the collected polymer solid was dried in a vacuum dryer at 50° C. for 72 hours to obtain a polyimide precursor (A-8).

[0437] <Synthesis Example 12 Synthesis of polyimide precursor (A-9)>

[0438] 155.1 g (0.50 mol) of ODPA was placed in a 2-liter separable flask, and 134.0 g (1.00 mol) of 2-hydroxyethyl methacrylate (HEMA) and 400 g of γ-butyrolactone were added. 79.1 g of pyridine was added while stirring at room temperature to obtain a reaction mixture. After the heat generated by the reaction was terminated, the mixture was cooled to room temperature and then allowed to stand for 16 hours.

[0439] Next, under ice cooling, a solution of 206.3 g (1.00 mole) of dicyclohexylcarbodiimide (DCC) dissolved in 180 g of γ-butyrolactone was added to the reaction mixture while stirring for 40 minutes. Subsequently, a suspension of 16.2 g (0.15 mole) of 1,4-p-phenylenediamine and 60.1 g (0.30 mole) of 4,4'-DAE suspended in 350 g of γ-butyrolactone was added while stirring for 60 minutes. After stirring at room temperature for 2 hours, 30 ml of ethyl alcohol was added and stirred for 1 hour. Thereafter, 400 g of γ-butyrolactone was added. The precipitate produced in the reaction mixture was removed by filtration to obtain a reaction solution.

[0440] The reaction solution was poured into 3 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed twice with water, washed once with isopropyl alcohol, and then dried in a vacuum dryer at 50° C. for 72 hours to obtain a polyimide precursor (A-9).

[0441] <Synthesis Example 13 Synthesis of acrylic resin (A-10)>

[0442] 150 g of dimethylaminomethanol (hereinafter referred to as "DMEA"; manufactured by Tokyo Chemical Industry Co., Ltd.) was placed in a reaction container in a nitrogen atmosphere, and the temperature was raised to 80°C using an oil bath. A mixture containing 20 g of ethyl acrylate (hereinafter referred to as "EA"), 40 g of 2-ethylhexyl methacrylate (hereinafter referred to as "2-EHMA"), 20 g of styrene (hereinafter referred to as "St"), 15 g of acrylic acid (hereinafter referred to as "AA"), 0.8 g of 2,2'-azobisisobutyronitrile and 10 g of DMEA was added dropwise over 1 hour. After the addition was completed, a polymerization reaction was further performed at 80°C and in a nitrogen atmosphere for 6 hours. Thereafter, 1 g of hydroquinone monomethyl ether was added to stop the polymerization reaction. Subsequently, a mixture containing 5 g of glycidyl methacrylate (hereinafter referred to as "GMA"), 1 g of triethylbenzylammonium chloride and 10 g of DMEA was added dropwise over 0.5 hours. After the addition was completed, an addition reaction was further carried out at 80° C. under a nitrogen atmosphere for 2 hours. The obtained reaction solution was purified by methanol to remove unreacted impurities, and then vacuum dried for 24 hours to obtain an acrylic resin (A-10) having a copolymerization ratio (weight basis): EA / 2-EHMA / St / GMA / AA=20 / 40 / 20 / 5 / 15. The acid value of the obtained acrylic resin (A-10) was 103 mgKOH / g.

[0443] <Synthesis Example 14 Synthesis of acrylic resin (A-11)>

[0444] A methyl methacrylate / methacrylic acid / styrene copolymer (mass ratio 30 / 40 / 30) was synthesized by the method described in Example 1 of Japanese Patent No. 3120476. 40 parts by mass of glycidyl methacrylate was added to 100 parts by mass of the obtained copolymer, and the mixture was reprecipitated with purified water, filtered, and dried to obtain an acrylic resin (A-11) having a weight average molecular weight of 15,000 and an acid value of 110 mgKOH / g.

[0445] <Preparation Example 1 Preparation of Photosensitive Conductive Paste 1>

[0446] In a 100 mL clean bottle, 10.0 g of acrylic resin (A-10) as a resin, 0.50 g of "IRGACURE (registered trademark)" OXE-01 (manufactured by Ciba Japan Co., Ltd.) as a photopolymerization initiator, 5.0 g of DMEA as a solvent, and 2.0 g of "Light Acrylate (registered trademark)" BP-4EA (manufactured by Kyoeisha Chemical Co., Ltd.) as a compound having an unsaturated double bond were placed and mixed using a rotation-revolution vacuum mixer "DEBUBA ARE-310" (manufactured by Thinky Co., Ltd.) to obtain 17.5 g of a resin solution (solid content: 71.4% by mass).

[0447] 17.50 g of the obtained resin solution was mixed with 44.02 g of silver particles having an average particle size of 1.0 μm and 0.28 g of carbon black having an average particle size of 0.05 μm, and kneaded using a three-roll mill "EXAKT M-50" (manufactured by EXAKT) to obtain 61.8 g of photosensitive conductive paste 1. In addition, regarding the average particle size of the silver particles and carbon black, each particle was observed using an electron microscope (scanning electron microscope (SEM)) at a magnification of 10,000 times and a field width of 12 μm, and the maximum width of each of 40 randomly selected primary particles of the silver particles and carbon black was measured, and the number average of these was calculated.

[0448] <Preparation Example 2: Production of Coloring Material Dispersion Liquid (DC-1)>

[0449] As a coloring material, zirconium oxide compound particles Zr-1 (manufactured by Nissin Engineering Co., Ltd.) produced by a thermal plasma method were used. 200 g of Zr-1, 114 g of a 35% by mass solution of propylene glycol monomethyl ether acetate (PGMEA) of an acrylic polymer (P-1), 625 g of "DISPERBYK (registered trademark)" LPN-2111 having a tertiary amino group and a quaternary ammonium salt as a polymer dispersant, and 661 g of PGMEA were placed in a tank and stirred for 20 minutes using a homogenizer to obtain a pre-dispersion liquid. The obtained preliminary dispersion was supplied to an Ultra Apex Mill manufactured by Kotobukiya Kogyo Co., Ltd., which includes a centrifugal separator filled with 75% by volume of 0.05 mmΦ zirconia beads, and dispersed at a rotation speed of 8 m / s for 3 hours to obtain a coloring material dispersion (DC-1) having a solid content concentration of 25% by mass and a coloring material / resin (mass ratio) of 80 / 20.

[0450] <Preparation Example 3 Preparation of Photosensitive Colored Resin Composition 1>

[0451] To 283.1 g of the coloring material dispersion (DC-1), 184.4 g of a 35 mass % solution of PGMEA of the acrylic resin (A-11), 50.1 g of dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd.) as a multifunctional monomer, 7.5 g of "Irgacure (registered trademark)" 907 (manufactured by BASF) and 3.8 g of "KAYACURE (registered trademark)" DETX-S (manufactured by Nippon Kayaku Co., Ltd.) as a photopolymerization initiator, 12.0 g of KBM5103 (manufactured by Shin-Etsu Chemical Co., Ltd.) as an adhesion improver, and PGMEA of a silicone surfactant "BYK (registered trademark)" 333 (manufactured by BYK Chemie) as a surfactant were added. A solution prepared by dissolving 3 g of the 10 mass % solution in 456.1 g of PGMEA was obtained to obtain a photosensitive color resin composition 1 having a total solid content concentration of 20 mass % and a coloring material / resin (mass ratio) of 30 / 70.

[0452] <Preparation Example 4: Production of Coloring Material Dispersion Liquid (DC-2)>

[0453] According to the method described in Japanese Patent Publication No. 2008-517330, the surface element composition of carbon black (CB-Bk1) modified with sulfonic acid groups on the surface is (C: 88%, O: 7%, Na: 3%, S: 2%), and as the state of the S element, the components belonging to CS and SS in the S2p peak component are 90%, the components belonging to SO and SOx are 10%, and the Brunauer-Emmett-Teller (BET) value is 54m2 / g.

[0454] The carbon black CB-Bk1 (200 g), a 40% by mass solution (94 g) of propylene glycol monomethyl ether acetate of acrylic resin (A-11), a 40% by mass solution (31 g) of BYK Chemie Japan LPN21116 as a polymer dispersant, and propylene glycol monomethyl ether acetate (675 g) were placed in a tank and stirred for 1 hour using a homogenizer (manufactured by Tokushige Kabushiki Kaisha) to obtain a pre-dispersion liquid. Thereafter, the pre-dispersion liquid was supplied to a disperser Ultra Apex Mill (manufactured by Kotobuki Kogyo) including a centrifugal separator filled with 70% 0.05 mm Φ zirconium oxide beads (YTZ balls manufactured by NIKKATO), and the dispersion was performed at a rotation speed of 8 m / s for 2 hours to obtain a coloring dispersion liquid DC-2 having a solid content concentration of 25% by mass and a pigment / resin (mass ratio) of 80 / 20.

[0455] <Preparation Example 5 Preparation of Photosensitive Colored Resin Composition 2>

[0456] To 534.8 g of the coloring material dispersion (DC-2), 122.1 g of a 40 mass % solution of PGMEA of the acrylic resin (A-11), 47.3 g of dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd.) as a multifunctional monomer, 11.8 g of "Adeka arc Luz" NCI-831 (manufactured by ADEKA Co., Ltd.) as a photopolymerization initiator, 12.0 g of KBM5103 (manufactured by Shin-Etsu Chemical Co., Ltd.) as an adhesion improver, and 333 (manufactured by BYK Chemie), a silicone surfactant, were added. A solution prepared by dissolving 4 g of the 10 mass % solution in 194.0 g of PGMEA was obtained to obtain a photosensitive color resin composition 2 having a total solid content concentration of 25 mass % and a coloring material / resin (mass ratio) of 45 / 55.

[0457] <Preparation Example 6 Preparation of Pigment Dispersion Liquid 1 (C-4-1)>

[0458] 57.7 g of "Solsperse (registered trademark)" 20000 (a polyether polymer resin dispersant having a tertiary amino group at the molecular end) was mixed with 750.0 g of PGMEA as a solvent and stirred for 10 minutes, and then 192.3 g of titanium nitride (average primary particle size 25 nm; "TiN" in the table) was added and stirred for 30 minutes, and then wet media dispersion treatment and filtration (PP filter pore size 0.8 μm) were performed using a horizontal bead mill to prepare pigment dispersion 1 (C-4-1). In addition, the average dispersed particle size of titanium nitride contained in pigment dispersion 1 was 85 nm.

[0459] <Preparation Example 7 Preparation of Pigment Dispersion Liquid 2 (C-4-2)>

[0460] Using CI Pigment Blue 60 (average primary particle size 60 nm) as an organic blue pigment, CI Pigment Red 190 (average primary particle size 55 nm) as an organic red pigment, and CI Pigment Yellow 192 (average primary particle size 40 nm) as an organic yellow pigment, each pigment dispersion was prepared by the same procedure as in Preparation Example 1. In addition, the average dispersed particle size of CI Pigment Blue 60 contained in the pigment dispersion was 162 nm, the average dispersed particle size of CI Pigment Red 190 was 110 nm, and the average dispersed particle size of CI Pigment Yellow 192 was 90 nm. 400.0 g of the organic blue pigment dispersion, 300.0 g of the organic red pigment dispersion, and 300.0 g of the organic yellow pigment dispersion were mixed and stirred for 10 minutes to prepare a pigment dispersion 2 (C-4-2) as a pseudo black dispersion.

[0461] <Preparation Example 8 Preparation of Pigment Dispersion Liquid 3>

[0462] 30.00 g of "Solsperse (registered trademark)" 20000 was mixed with 850.0 g of PGMEA and stirred for 10 minutes, and then 120.0 g of a benzodifuranone pigment (average primary particle size 50 nm; "Irgaphor (registered trademark)" Black S0100 manufactured by BASF) as an organic black pigment was added and stirred for 30 minutes. Then, a pigment dispersion 3 (C-4-3) was prepared using a horizontal bead mill in the same procedure as in Preparation Example 3. The average dispersed particle size of the benzodifuranone pigment contained in the pigment dispersion 3 was 120 nm.

[0463] The (B-3) component, (C-1) component, (C-2) component, (C-3) component, (F-1) component, (F-2) component, other components, and solvent used in Examples and Comparative Examples are shown below.

[0464] (B-3) Component: Photopolymerization initiator NCI-831 (manufactured by ADEKA Co., Ltd.)

[0465] (C-1) Component: Plast Yellow 8070 (maximum absorption wavelength: 460 nm) (manufactured by Arimoto Chemical Industry Co., Ltd.)

[0466] (C-2) Component: Oil Scarlet 5206 (maximum absorption wavelength: 530 nm) (manufactured by Arimoto Chemical Industry Co., Ltd.)

[0467] (C-3) Component: Plast Blue 8540 (maximum absorption wavelength: 660 nm) (manufactured by Arimoto Chemical Industry Co., Ltd.)

[0468] Other Ingredients:

[0469] Free radical polymerizable compounds:

[0470] (F-1) Component: Dipentaerythritol hexaacrylate (DPHA, manufactured by Kyoeisha Chemical Co., Ltd.)

[0471] Thermal crosslinking agent:

[0472] (G-1) Ingredients: HMOM-TPHAP (manufactured by Honshu Chemical Industry Co., Ltd.)

[0473] (G-2) Component: YX4000H (manufactured by Mitsubishi Chemical Co., Ltd.)

[0474] Solvent:

[0475] GBL: gamma-butyrolactone

[0476] PGMEA: propylene glycol monomethyl ether acetate.

[0477] [Chemistry 11]

[0478] (G1)

[0479]

[0480] (G2)

[0481]

[0482] Table 1 shows the formulation of the resin composition containing (A) resin, (B) photosensitizer and (C) colorant, etc. Resin composition 1 to resin composition 21 were prepared using the solvent described in Table 1 in a manner such that the solid content concentration was 40% by mass. In addition, Table 2-1 and Table 2-2 show the resin composition used in the examples, the transmittance (%) of the cured film of the resin composition at a wavelength of 450nm at a thickness reference of 5μm, the thickness (μm) of the entire cured film, the number of layers of the cured film, the shape and length of the opening pattern processed in the cured film, and the angle of the inclined side of the opening pattern.

[0483] [Table 1]

[0484]

[0485]

[0486]

[0487] Regarding the evaluation level (1), a display device in which the glare of the wiring is suppressed by the cured film and the wiring is hidden, and the maximum length of the opening pattern is 2 μm or less is set to level A, a display device in which the glare of the wiring is suppressed by the cured film and the wiring is hidden, and the maximum length of the opening pattern is 5 μm or less is set to level B, a display device in which the glare of the wiring is suppressed by the cured film and the wiring is hidden, and the maximum length of the opening pattern is 20 μm or less is set to level C, a display device in which the glare of the wiring is suppressed by the cured film and the wiring is hidden, and the maximum length of the opening pattern is greater than 20 μm is set to level D, and a display device in which the wiring can be clearly confirmed by visual observation through the cured film is set to level E.

[0488] Regarding the evaluation level (2), the angle of the inclined side is evaluated as level A if it is 55° or more and 80° or less, if it is 40° or more and less than 55°, or if it is more than 80° or less than 85°, and if it is less than 40° or more than 85°, it is evaluated as level C.

[0489] (Example 1) Figure 7 Structure)

[0490] according to Figure 7 An embodiment of the display device of the present invention is described with reference to a cross-sectional view of a surface perpendicular to a supporting base or an opposing substrate, which shows a manufacturing process.

[0491] like Figure 7 As shown in FIG. 1 , a glass substrate is used as the support substrate 18. A temporary adhesive material containing polyimide is arranged on the glass substrate, and ITO is formed as wiring 4d on a part of the surface of the temporary adhesive material by sputtering. Then, a light-emitting element 2 as a light-emitting element is arranged on the support substrate 18 (equivalent to step (D1)). The light-emitting element 2 has a thickness of 7 μm, a length of one side of 30 μm, and a length of the other side of 50 μm.

[0492] Secondly, if Figure 7 As shown in b, the resin composition 1 described in Table 1 was applied on the supporting substrate 18 and the light emitting element 2 to a thickness of 10 μm after heat treatment to form a resin film 19 (corresponding to step (D2)).

[0493] Secondly, if Figure 7 As shown in step (D3), i-rays (365 nm) are irradiated on the resin film 19 through a mask having a desired pattern. The exposed resin film 19 is developed using a 2.38 mass % tetramethylammonium (TMAH) aqueous solution to form a plurality of opening patterns 12 that penetrate the resin film 19 in the thickness direction (equivalent to step (D3)). The shape of the opening pattern is circular, and the longest length of the bottom portion in the smallest area of ​​the opening pattern is 2 μm in diameter.

[0494] Next, the resin film 19 is heat-treated at 110° C. for 30 minutes in an environment with an oxygen concentration of 100 ppm or less, and then heat-treated at 230° C. for 60 minutes to cure, thereby forming a cured film 3 having a thickness of 10 μm (corresponding to step ( D4 )). The resin film 19 is cured directly to form the cured film 3 .

[0495] Secondly, if Figure 7 d, titanium as a barrier metal is sputtered on the cured film 3, and a copper seed layer is formed thereon by sputtering. After that, after forming a photoresist layer, a wiring 4 containing copper electrically connected to the light-emitting element 2 is formed on the opening pattern 12 of the cured film 3 and a part of the surface of the cured film 3 by plating, and then the photoresist, seed layer, and barrier metal are removed (equivalent to step (D5)). The thickness of the wiring 4a formed on a part of the surface of the cured film 3 is 5 μm.

[0496] Afterwards, if Figure 7 Step (D2), step (D3), step (D4), and step (D5) were repeated twice as in steps e to f to form a three-layer cured film 3. As a result, the total thickness of the three-layer cured film 3 was 30 μm.

[0497] Afterwards, in Figure 7 In g, the barrier metal 9 is formed in the opening pattern 12 of the cured film 3 by sputtering, and the bump 10 is formed. Figure 7 h, the solder is reflowed at 260°C for 1 minute, and electrically connected to the light emitting element driving substrate 7 having the driver IC as the driving element 8 via the bump 10. After that, the supporting substrate 18 is peeled off, and the counter substrate 5 is bonded using an adhesive or the like, thereby obtaining a display device 1 having a plurality of light emitting elements 2. In addition, as the light emitting element driving substrate 7, a glass substrate having copper wiring is used, and on its side, as shown in FIG. Figure 7 The wiring 4c was used as shown in h, and the photosensitive conductive paste 1 of Preparation Example 1 (corresponding to step D9) was used as the wiring 4c. The wiring 4c was prepared as follows.

[0498] <Production of Wiring 4c Using Photosensitive Conductive Paste 1 of Preparation Example 1>

[0499] On a release PET film having a thickness of 16 μm and coated with a release agent, photosensitive conductive paste 1 was applied so that the film thickness after drying would be 6.0 μm, and the obtained coating film was dried in a drying oven at 100° C. for 10 minutes. Thereafter, an exposure machine equipped with an ultra-high pressure mercury lamp was used to expose the film at 350 mJ / cm 2After exposure with an exposure amount of , a 0.1 mass % sodium carbonate aqueous solution was used as a developer, and spray development was performed for 30 seconds at a pressure of 0.1 MPa to obtain a pattern. Thereafter, the obtained pattern was cured in a drying oven at 140°C for 30 minutes to obtain a transfer sample with wiring. The obtained pattern had a line width of 50 μm and a line length of 90 mm. The transfer sample was bonded to both sides in such a way that a part of the wiring was arranged at the end of the glass with an R chamfered portion, and the side surface of the glass was pressed to a hot plate at 130°C for 30 seconds, and then the remaining part was transferred using a hot roller laminator at 130°C and 1.0 m / min.

[0500] (Example 2)

[0501] The display device 2 was obtained by the same method as in Example 1 except that the resin composition 1 of Example 1 was changed to a resin sheet containing the resin composition 2 and the resin film 19 was formed by lamination.

[0502] (Examples 3 to 14)

[0503] Display devices 3 to 14 were obtained by the same method as in Example 1 except that the resin composition 1 in Example 1 was changed to resin compositions 3 to 14.

[0504] (Example 15)

[0505] In Example 1, the resin composition 1 was applied on the support substrate 18 and the light emitting element 2 to form a resin film 19 so as to have a thickness of 20 μm after heat treatment. As a result, the display device 15 was obtained by the same method as in Example 1 except that the total thickness of the three-layer cured film 3 was 40 μm.

[0506] (Example 16)

[0507] according to Figure 8 An embodiment of the display device of the present invention is described with reference to a cross-sectional view of a surface perpendicular to a supporting base or an opposing substrate, which shows a manufacturing process.

[0508] First, if Figure 8 As shown in a, a pad 17 made of copper is placed on a supporting substrate 18 (corresponding to step (E1)). The thickness of the pad is 0.2 μm.

[0509] Secondly, if Figure 8 As shown in b, the resin composition 2 described in Table 1 was applied on the support substrate 18 and the pad 17 to a thickness of 10 μm after heat treatment to form a resin film 19 (corresponding to step (E2)).

[0510] Secondly, if Figure 8As shown in FIG. 3 c, a plurality of opening patterns 12 are formed in the resin film 19 under the same conditions as the photolithography step shown in Example 1 (corresponding to step (E3)).

[0511] Next, the resin film 19 was cured under the same conditions as in Example 1 to form a cured film 3 having a thickness of 10 μm (corresponding to step ( E4 )).

[0512] Then, in Figure 8 In c, in order to improve the adhesion between the cured film 3 and the wiring 4, a barrier metal such as titanium is sputtered on the cured film 3, and a copper seed crystal (seed layer) is further formed thereon by a sputtering method.

[0513] Secondly, if Figure 8 After forming a photoresist layer as shown in FIG. d, a wiring 4 made of copper is formed on the opening pattern 12 of the cured film 3 and a portion of the surface of the cured film 3 by plating (corresponding to step (E5)). The thickness of the wiring 4 formed on a portion of the surface of the cured film 3 is 5 μm. Thereafter, the photoresist, seed layer, and barrier metal are removed.

[0514] Then, the steps (E2), (E3), (E4) and (E5) are repeated twice, as shown in FIG. Figure 8 As shown in FIG. e, a three-layer cured film 3 having wiring 4 in the cured film 3 was formed. As a result, the thickness of the three-layer cured film 3 as a whole was 30 μm.

[0515] Secondly, if Figure 8 As shown in step f, the light emitting element 2 was arranged on the cured film 3 so as to maintain electrical connection with the wiring 4 (corresponding to step (E6)). The thickness of the light emitting element 2 was 7 μm.

[0516] Secondly, if Figure 8 As shown in FIG. 1 , a resin film 19 containing a resin composition 2 is formed on the light emitting element 2, and hardened by heat treatment to form a cured film 21. In addition, after heat treatment at 110° C. for 30 minutes in an environment with an oxygen concentration of 100 ppm or less, heat treatment at 230° C. for 60 minutes is performed to form a cured film 21. Thereafter, ITO is formed as wiring 4d on a portion of the surface of the cured film 21 by sputtering.

[0517] Secondly, if Figure 8 h, the support substrate 18 is peeled off, and electrically connected to the light emitting element driving substrate 7 having a driver IC as the driving element 8 via the bumps 10, and the counter substrate 5 is bonded to the light emitting element 2 using an adhesive or the like, thereby obtaining a display device 16 having a plurality of light emitting elements 2. In addition, as the light emitting element driving substrate 7, a glass substrate having copper wiring is used, and on its side, as shown in FIG. Figure 8Wiring 4c was used as shown in h. As the wiring 4c, the photosensitive conductive paste 1 of Preparation Example 1 was used.

[0518] (Example 17)

[0519] A display device 17 was obtained by the same method as in Example 16, except that the resin composition 2 in Example 16 was changed to the resin composition 10 and the supporting substrate 18 was used as the light-emitting element driving substrate 7 formed with the wiring 4c and was directly used without going through the peeling step.

[0520] (Example 18)

[0521] In Example 16, as the cured film 21 formed on the light-emitting element 2, a display device 18 was obtained by the same method as in Example 16, except that a heat treatment was performed at 150°C for 60 minutes using T693 / R4000 Series (manufactured by Nagase Chemtex Co., Ltd.) to form the cured film 21.

[0522] (Example 19)

[0523] In the same manner as in Example 15, a multilayer Figure 8 After the cured film 3 shown in e is formed, the resin composition 2 is used between and around the light emitting elements 2 to be arranged later. Fig. 9 f) to form a partition wall 15 (corresponding to step (E9)), and then, Fig. 9 As shown in g, multiple light emitting elements 2 are arranged. Fig. 9 h, the support substrate 18 is peeled off, and electrically connected to the light emitting element driving substrate 7 having a driver IC as a driving element 8 via the bump 10, and the counter substrate 5 is bonded to the light emitting element 2 using an adhesive or the like, thereby obtaining a display device 19 having a plurality of light emitting elements 2. In addition, the thickness of the light emitting element 2 is 7 μm, and the thickness of the partition wall is 10 μm.

[0524] (Example 20)

[0525] like Fig.17 As shown in a, a partition wall 15 is formed on the supporting substrate 18 (corresponding to step D8). Fig.17 As shown in FIG. 2 , the light emitting element 2 is formed between the partition walls 15 (step (equivalent to D1)). The display device 20 is manufactured by the same steps as in Example 3 except for the above. The light emitting element 2 has a thickness of 7 μm and the partition walls 15 have a thickness of 10 μm. The partition walls 15 are made of acrylic resin containing a conventional white pigment.

[0526] (Example 21)

[0527] A display device 21 was obtained by the same method as in Example 1, except that the resin composition 1 in Example 1 was changed to the resin composition 17, a photoresist was formed before exposure, and the photoresist was removed after development.

[0528] (Example 22)

[0529] A display device 22 was obtained by the same method as in Example 1 except that the resin composition 1 in Example 1 was changed to the resin composition 18.

[0530] (Example 23)

[0531] A display device 23 was obtained by the same method as in Example 1 except that the resin composition 1 of Example 1 was changed to the resin composition 19 and the exposed resin film 19 was developed using cyclopentanone.

[0532] (Examples 24-25)

[0533] The resin composition 1 of Example 1 was changed to resin composition 20 to resin composition 21, and the resin composition 1 described in Table 1 was applied on the supporting substrate 18 and the light-emitting element 2 to a thickness of 8 μm after heat treatment to form a resin film 19 (corresponding to step (D2)).

[0534] Secondly, if Figure 7 As shown in step (c), i-rays (365 nm) are irradiated on the resin film 19 through a mask having a desired pattern. The exposed resin film 19 is developed using a 2.38 mass % tetramethylammonium (TMAH) aqueous solution to form a plurality of opening patterns 12 that penetrate the resin film 19 in the thickness direction (equivalent to step (D3)).

[0535] Next, the resin film 19 is heat-treated at 110° C. for 30 minutes in an environment with an oxygen concentration of 100 ppm or less, and then heat-treated at 230° C. for 60 minutes to cure, thereby forming a cured film 3 having a thickness of 8 μm (corresponding to step ( D4 )). The resin film 19 is cured directly to form the cured film 3 .

[0536] Secondly, if Figure 7 d, titanium as a barrier metal is sputtered on the cured film 3, and a seed layer of copper is formed thereon by sputtering. After that, after forming a photoresist layer, a wiring 4 containing copper electrically connected to the light-emitting element 2 is formed on the opening pattern 12 of the cured film 3 and a part of the surface of the cured film 3 by plating, and then the photoresist, seed layer, and barrier metal are removed (equivalent to step (D5)). The thickness of the wiring 4a formed on a part of the surface of the cured film 3 is 2 μm.

[0537] Afterwards, if Figure 7 Step (D2), step (D3), step (D4) and step (D5) are repeated twice as in Example 1 to form a three-layer cured film 3. In addition, the second and third layers of the cured film 3 are formed in such a way that the thickness becomes 4 μm after the heat treatment. As a result, the thickness of the three-layer cured film 3 as a whole is 16 μm. In addition, the same method as in Example 1 is used to obtain display devices 24 to 25.

[0538] (Example 26)

[0539] A display device 26 was obtained by the same method as in Example 16 except that the resin composition 2 in Example 16 was changed to the resin composition 18.

[0540] (Example 27)

[0541] A display device 27 was obtained by the same method as in Example 16, except that the resin composition 2 in Example 16 was changed to the resin composition 19 and the exposed resin film 19 was developed using cyclopentanone.

[0542] (Examples 28-29)

[0543] The resin composition 2 of Example 16 is changed to resin composition 20 to resin composition 21, such as Figure 8 As shown in b, the resin compositions 20 and 21 are applied on the support substrate 18 and the pad 17 to a thickness of 4 μm after heat treatment to form a resin film 19 (corresponding to step (E2)).

[0544] Secondly, if Figure 8 As shown in FIG. 3 c, a plurality of opening patterns 12 are formed in the resin film 19 under the same conditions as the photolithography step shown in Example 1 (corresponding to step (E3)).

[0545] Next, the resin film 19 was cured under the same conditions as in Example 1 to form a cured film 3 having a thickness of 4 μm (corresponding to step ( E4 )).

[0546] Then, in Figure 8 In c, in order to improve the adhesion between the cured film 3 and the wiring 4, a barrier metal such as titanium is sputtered on the cured film 3, and a copper seed crystal (seed layer) is further formed thereon by a sputtering method.

[0547] Secondly, if Figure 8 After forming a photoresist layer as shown in FIG. d, a wiring 4 made of copper is formed on the opening pattern 12 of the cured film 3 and a portion of the surface of the cured film 3 by plating (corresponding to step (E5)). The thickness of the wiring 4 formed on a portion of the surface of the cured film 3 is 2 μm. Thereafter, the photoresist, seed layer, and barrier metal are removed.

[0548] Then, the steps (E2), (E3), (E4) and (E5) are repeated twice, as shown in FIG. Figure 8 As shown in Fig. e, a three-layer cured film 3 having wiring 4 in the cured film was formed. As a result, the total thickness of the three-layer cured film 3 was 12 μm. Display devices 28 to 29 were obtained by the same method as in Example 16 except for this.

[0549] (Example 30)

[0550] In Example 3, Figure 7 As shown in step D9, a TFT substrate is used as the light emitting element driving substrate 7, a groove is formed on the side surface by laser processing, titanium and copper are formed in sequence by sputtering, and copper is formed by plating to form wiring 4c (equivalent to step D9). Except for this, the display device 30 is obtained by the same method as in Example 3.

[0551] (Example 31)

[0552] In Example 16, Figure 8 As shown in step h, a TFT substrate is used as the light emitting element driving substrate 7, grooves are formed on the side surface by laser processing, titanium and copper are formed in sequence by sputtering, and copper is formed by plating to form wiring 4c (equivalent to step E11). Except for this, the same method as in Example 16 is used to obtain a display device 31.

[0553] (Example 32)

[0554] On the side of the light emitting element driving substrate 7 of Example 30, as shown in FIG. Figure 7 The wiring 4c was used as shown in h, and the photosensitive conductive paste 1 of Preparation Example 1 (corresponding to step D9) was used as the wiring 4c. Except for this, the display device 32 was obtained by the same method as Example 30.

[0555] (Example 33)

[0556] On the side of the light emitting element driving substrate 7 of Example 31, as shown Figure 8 The wiring 4c was used as shown in h, and the photosensitive conductive paste 1 described in Example 32 (corresponding to step E11) was used as the wiring 4c. Except for this, the display device 33 was obtained by the same method as in Example 31.

[0557] (Example 34)

[0558] A display device 34 is obtained by the same method as in Example 30 except that a printed wiring board is used as the light emitting element driving substrate 7 of Example 30 and the driving element 8 is connected to the wiring 4 via the wiring and bump 10 in the printed wiring board without forming the wiring 4c.

[0559] (Example 35)

[0560] A display device 35 is obtained by the same method as in Example 31 except that a printed wiring board is used as the light emitting element driving substrate 7 of Example 31 and the driving element 8 is connected to the wiring 4 via the wiring and bump 10 in the printed wiring board without forming the wiring 4c.

[0561] (Example 36)

[0562] like Fig.18 As shown in a, a light shielding layer 25 is formed on the supporting substrate 18 (corresponding to step D10). Fig.18 As shown in a, the light emitting element 2 is formed between the light shielding layers 25 (step (corresponding to D1)). Except for this, the display device 36 is manufactured by the same steps as in Example 3. The light shielding layer 25 is manufactured as follows.

[0563] <Production of light shielding layer 25>

[0564] The colored resin composition 1 was applied to the support substrate 18 so as to have a thickness of 1 μm after heat treatment, and the applied film was dried by heating on a hot plate at 100° C. for 2 minutes. The dried film was exposed to light at 200 mJ / cm using an exposure machine equipped with an ultra-high pressure mercury lamp. 2 The pattern film was then exposed to ultraviolet light at an exposure amount of . Next, the pattern film was developed using a 0.045 mass % potassium hydroxide aqueous solution as an alkaline developer, followed by pure water washing to obtain a pattern film. The obtained pattern film was post-baked in a hot air oven at 230° C. for 30 minutes to obtain a light shielding layer.

[0565] (Example 37)

[0566] A display device 37 was manufactured by the same steps as in Example 36, except that the light-shielding layer 25 of Example 36 was formed by changing the light-shielding layer 25 to the colored resin composition 2.

[0567] (Example 38)

[0568] exist Figure 7 In f, a display device 38 is obtained by the same process as in Example 3 except that the thickness of the wiring 4a in contact with the bump 10 is set to 10 μm, the thickness of the cured film 3 formed on a portion of the surface of the wiring 4a is set to 15 μm, and the thickness of the entire cured film 3 is set to 35 μm.

[0569] (Example 39)

[0570] exist Figure 8 In b, a display device 39 was obtained by the same steps as in Example 16 except that the thickness of the pad 18 was 10 μm, the thickness of the cured film 3 formed on a part of the surface of the pad was 15 μm, and the thickness of the entire cured film 3 was 35 μm.

[0571] (Example 40)

[0572] according to Fig.19 An embodiment of the display device of the present invention is described with reference to a cross-sectional view of the manufacturing process.

[0573] like Fig.19 As shown in a, a TFT array substrate is used as a light emitting element driving substrate 7, and a resin composition 2 described in Table 1 is applied on the light emitting element driving substrate 7 in such a manner that the thickness becomes 3 μm after heat treatment to form a resin film 19 (corresponding to step (F1)). In addition, the thickness of the wiring 4 is 1 μm.

[0574] Next, a plurality of opening patterns 12 are formed in the resin film 19 under the same conditions as the photolithography process described in Example 2 (corresponding to step ( F2 )).

[0575] Next, the resin film 19 was cured under the same conditions as in Example 3 to form a cured film 3 having a thickness of 3 μm (corresponding to step ( F3 )).

[0576] Secondly, if Fig.19 b) is a process for forming the wiring on at least a portion of the surface of the cured film and a portion of the opening pattern of the cured film. After forming a photoresist layer (not shown), ITO is formed as wiring 4e on a portion of the surface of the cured film 3 by sputtering. Thereafter, the useless photoresist is removed. (Equivalent to process (F4)). The thickness of the ITO is 0.1 μm.

[0577] Secondly, if Fig.19 c, the resin composition 3 described in Table 1 was cured to form a cured film 3 having a thickness of 3 μm. Then, wiring 4c was formed using the photosensitive conductive paste 1 of Preparation Example 1.

[0578] Secondly, if Fig.19d, a partition wall 15 is formed on the cured film 3. Next, a light-emitting element 2 is formed between the partition walls 15 (process (equivalent to F5)). In addition, the thickness of the light-emitting element 2 is 7 μm, and the thickness of the partition wall 15 is formed to be 8 μm. The partition wall 15 uses an acrylic resin containing an existing white pigment. A resin film 19 containing a resin composition 2 is formed on the cured film 3 and the light-emitting element 2, and is cured by heat treatment to form a cured film 21. ITO is formed as wiring 4d on a portion of the surface of the cured film 3 by sputtering.

[0579] Afterwards, if Fig.19 The counter substrate 5 is bonded using an adhesive as shown in FIG. e. The driver IC or other driving element 8 is electrically connected to the light emitting element 2 via the wiring 4c or the wiring 4 extending in the cured film 3, and the wiring 4e, thereby obtaining a display device 40 having a plurality of light emitting elements 2.

[0580] (Examples 41-42)

[0581] Display devices 41 and 42 were obtained by the same method as in Example 40 except that the resin composition 2 in Example 40 was changed to the resin composition 13 and the resin composition 21.

[0582] (Example 43)

[0583] Use as Fig. 22 A light-emitting element 2 including electrodes on discontinuous surfaces as shown is provided, a temporary adhesive material containing polyimide is arranged on a glass substrate, and then, the light-emitting element 2 as a light-emitting element is arranged on a supporting substrate 18 provided with the temporary adhesive material (equivalent to process (D1)). Except for this, the display device 43 is obtained by the same method as in Example 3.

[0584] (Example 44)

[0585] Use as Fig.23 A display device 44 is obtained by the same method as in Example 16 except that the light-emitting element 2 includes electrodes on discontinuous surfaces as shown.

[0586] (Example 45)

[0587] Use as Fig.24 A display device 45 is obtained by carrying out the same method as in Example 40 except that the light-emitting element 2 includes electrodes on discontinuous surfaces as shown.

[0588] (Example 46)

[0589] A display device 46 was obtained by the same method as in Example 25 except that the number of layers of the cured film 3 was one and the total thickness was 5 μm.

[0590] (Example 47)

[0591] A display device 47 was obtained by the same method as in Example 3 except that the number of layers of the cured film 3 was 5 and the total thickness was 50 μm.

[0592] (Example 48)

[0593] A display device 48 was obtained by the same method as in Example 3 except that the number of layers of the cured film 3 was 4 and the total thickness was 60 μm.

[0594] (Example 49)

[0595] A display device 49 was obtained by the same method as in Example 3 except that the number of layers of the cured film 3 was 11 and the total thickness was 110 μm.

[0596] (Example 50)

[0597] according to Fig.29 A 50th embodiment of the display device according to the second embodiment of the present invention is described with reference to a cross-sectional view taken along a plane perpendicular to a light emitting element driving substrate, which shows a manufacturing process.

[0598] like Fig.29 As shown in a, a TFT array substrate is used as a light emitting element driving substrate 7, and a resin composition 13 described in Table 1 is applied on the light emitting element driving substrate 7 in such a manner that the thickness becomes 3 μm after heat treatment to form a resin film 19 (corresponding to step (G1)). In addition, the thickness of the wiring 4 is 1 μm.

[0599] Next, a plurality of opening patterns 12 are formed in the resin film 19 under the same conditions as the photolithography step described in Example 3 (corresponding to step (G2)).

[0600] Next, the resin film 19 was cured under the same conditions as in Example 3 to form a cured film 3 having a thickness of 3 μm (corresponding to step ( G3 )).

[0601] Secondly, if Fig.29 b) is a process for forming the wiring on at least a portion of the surface of the cured film and a portion of the opening pattern of the cured film. After forming a photoresist layer (not shown), ITO is formed as wiring 4e on a portion of the surface of the cured film 3 by sputtering. Thereafter, the useless photoresist is removed. (Equivalent to process (G4)). The thickness of the ITO is 0.1 μm.

[0602] Secondly, if Fig.29 As shown in c, wiring 4c using the photosensitive conductive paste 1 of Preparation Example 1 was formed as wiring 4c.

[0603] Secondly, if Fig.29 d, a partition wall 15 is formed on the cured film 3. Next, a light-emitting element 2 is formed between the partition walls 15 (process (equivalent to G5)). In addition, the thickness of the light-emitting element 2 is 7 μm, and the thickness of the partition wall 15 is formed to be 8 μm. The partition wall 15 uses an acrylic resin containing an existing white pigment. A resin film 19 containing a resin composition 2 is formed on the cured film 3 and the light-emitting element 2, and is cured by heat treatment to form a cured film 21. ITO is formed as wiring 4d on a portion of the surface of the cured film 3 by sputtering.

[0604] Afterwards, if Fig.29 The counter substrate 5 is bonded with an adhesive as shown in FIG. e. The driver IC or other drive element 8 is electrically connected to the light emitting element 2 via the wiring 4c or the wiring 4 and wiring 4e extending in the cured film 3, thereby obtaining a display device 52 having a plurality of light emitting elements 2.

[0605] (Example 51)

[0606] Display device 53 was obtained by the same method as in Example 50 except that resin composition 13 in Example 50 was changed to resin composition 21.

[0607] (Example 52)

[0608] Use as Fig.28 A display device 54 is obtained by carrying out the same method as in Example 50 except that the light-emitting element 2 includes electrodes on discontinuous surfaces as shown.

[0609] (Example 53)

[0610] Display device 55 was obtained by the same method as in Example 52 except that resin composition 13 in Example 52 was changed to resin composition 21.

[0611] As a result, in display devices 1 to 49, 52 to 55, since the transmittance of the cured film 3 is sufficiently low, the cured film 3 hides the wiring 4, which can suppress the glare of the wiring 4 and make it difficult to be seen from the outside, thereby improving the design. In addition, compared with the existing flexible substrate, the thickness of the cured film is small, so it is possible to suppress wiring defects such as wiring short circuits caused by low-profile packaging or short-distance wiring, or achieve low losses, thereby improving high-speed responsiveness. Furthermore, display devices 1 to 20, 22 to 49, 52, and 54 can be finely processed, so tiny light-emitting elements can be applied, and high-density packaging of light-emitting elements can be achieved. In addition, as the partition 15, a cured film containing a resin composition can also be applied, and by forming a partition, it is easy to bond the opposing substrates. Furthermore, in display devices 13, 24-25, 28-29, 41-42, 52-55, since the cured film 3 is black, the cured film 3 hides the wiring 4, suppresses the glare of the wiring 4, and makes it difficult to be seen from the outside, thereby improving the design. In addition, by reducing the reflection of external light or improving the contrast, the visibility can be improved. Furthermore, in display devices 1-33, 36-49, 52-55, since at least a part of the wiring 4c extends on the side of the substrate, the low profile or high-speed responsiveness of the display device itself is improved, and the display device can be made more compact and narrow-framed. In addition, display devices 36 and 37 can suppress light leakage from the light-emitting elements or color mixing between pixels without significantly impairing the light output efficiency by forming a light-shielding layer between the plurality of light-emitting elements, thereby improving the contrast. In display devices 38 and 39, the thickness of the wiring near the bump 10 is thicker than the thickness of the wiring near the light-emitting element 2, so that when the light-emitting element driving substrate 7 is connected using the bump 10, wiring defects can be suppressed, and a display device with high reliability can be obtained. In display devices 46, 52 to 55, since the number of layers of the cured film 3 is one layer, the number of light-emitting elements that can be arranged is limited. In display device 49, since the overall thickness of the cured film exceeds 100 μm, the step flatness is reduced, which causes problems when packaging the light-emitting element.

[0612] (Comparative Examples 1-2)

[0613] Display devices 50 to 51 were obtained by the same method as in Example 1 except that the resin composition 1 in Example 1 was changed to resin compositions 15 to 16.

[0614] As a result, in the display devices 50 to 51 , since the light transmittance of the cured film 3 is sufficiently high, the hiding property including the suppression of the glare of the wiring 4 by the cured film 3 is insufficient.

[0615] Explanation of symbols

[0616] 1 Display device

[0617] 2 Light-emitting element

[0618] 3 Hardening film

[0619] 4, 4c, 4d, 4e wiring

[0620] 4a The thickness of the wiring arranged on the surface of the cured film

[0621] 4b The thickness of the wiring extending in the opening pattern penetrating in the thickness direction of the cured film

[0622] 5 Opposing substrates

[0623] 6 Electrodes

[0624] 7 Light-emitting element driving substrate

[0625] 8 Drive components

[0626] 9 barrier metal

[0627] 10 Bump

[0628] 11a Designated Area A

[0629] 11b Designated Area B

[0630] 12 opening patterns

[0631] 13 Bottom of wiring 4

[0632] 14 The longest length of the bottom part

[0633] 15 Next Door

[0634] 16 External base plate

[0635] 17 Pad

[0636] 18 Support substrate

[0637] 19 Resin film

[0638] 20 Overall thickness of the hardened film

[0639] 21 Hardening film

[0640] 22TFT

[0641] 23 TFT insulation layer

[0642] 24 Contact hole

[0643] 25 Shading layer

[0644] 26 Slanted Edge

[0645] 27 Angle of the inclined side

[0646] 28 Thickness of hardened film 3

[0647] 29 The position where the thickness of the effect film 3 is 1 / 2

Claims

1. A display device comprising at least wiring, a cured film, and a plurality of light-emitting elements, wherein the light-emitting elements include electrodes on two different surfaces, at least one of the electrodes is connected to the plurality of wirings extending in the cured film, the plurality of wirings are electrically insulated by the cured film, the cured film is a film formed by curing a resin composition containing (A) resin, and the transmittance of the cured film at a wavelength of 450 nm at a thickness reference of 1 μm is 0.1% or more and 95% or less.

2. The display device according to claim 1, in, The cured film has a transmittance of light of a wavelength of 450 nm at a thickness basis of 5 μm of 0.1% or more and 79% or less.

3. The display device according to claim 1, in, The cured film has a transmittance of light of a wavelength of 450 nm at a thickness basis of 1 μm of 0.1% or more and 25% or less.

4. The display device according to claim 1 or 2, in, The entire cured film has a thickness of 5 μm or more and 100 μm or less.

5. The display device according to claim 1 or 2, in, The number of layers of the cured film is 2 or more and 10 or less.

6. The display device according to claim 1 or 2, wherein the cured film is provided with an opening pattern penetrating in the thickness direction, and the wiring is arranged at least in the opening pattern, and the longest length of the bottom portion of the wiring formed at a position in contact with the light-emitting element is greater than or equal to 2 μm and less than or equal to 20 μm. 7 . The display device according to claim 1 , wherein the cured film covers a surface of the light emitting element other than a light output surface.

8. A display device comprising at least a substrate having wiring and / or a thin film transistor, a cured film, and a plurality of light-emitting elements, wherein the light-emitting elements include electrodes on two different surfaces, at least a portion of the wiring and / or the thin film transistor is in contact with the cured film, the cured film is a film formed by curing a resin composition comprising (A) resin, and the transmittance of the cured film at a wavelength of 450 nm at a thickness reference of 1 μm is greater than 0.1% and less than 95%.

9. The display device according to claim 1 or 8, in, A partition wall having a thickness equal to or greater than that of the light emitting element is provided between the plurality of light emitting elements.

10. The display device according to claim 1 or 8, in, The light emitting element is a light emitting diode having a side length of 5 μm or more and 700 μm or less. 11 . The display device according to claim 1 , further comprising a driving element and a substrate, wherein the driving element is connected to the light emitting element via wiring, and at least a part of the wiring extends on a side surface of the substrate.

12. The display device according to claim 1 or 8, in, A light shielding layer is provided between the plurality of light emitting elements.

13. The display device according to claim 1 or 8, in, The resin (A) includes at least one resin selected from the group consisting of polyimide, a polyimide precursor, polybenzoxazole, a polybenzoxazole precursor, and copolymers thereof.

14. The display device according to claim 1 or 8, in, The resin composition comprising the resin (A) further comprises a photosensitizer (B).

15. The display device according to claim 1 or 8, in, The resin composition containing the resin (A) further contains a colorant (C), and the colorant (C) contains a colorant (C-1) having a maximum absorption in a wavelength range of 400 nm to 490 nm.

16. The display device according to claim 1 or 8, in, The resin composition containing the resin (A) further contains a colorant (C), and the colorant (C) contains a colorant (C-2) having a maximum absorption in a wavelength range of more than 490 nm and 580 nm or less.

17. The display device according to claim 1 or 8, in, The resin composition containing the resin (A) further contains a colorant (C), and the colorant (C) contains a colorant (C-3) having a maximum absorption in a wavelength range of more than 580 nm and 800 nm or less.

18. The display device according to claim 1 or 8, in, The colorant (C) contains (C-1) a colorant having a maximum absorption in a wavelength range of 400 nm to 490 nm, (C-2) a colorant having a maximum absorption in a wavelength range of more than 490 nm to 580 nm, and (C-3) a colorant having a maximum absorption in a wavelength range of more than 580 nm to 800 nm.

19. The display device according to claim 1 or 8, in, The resin composition containing the resin (A) is positive photosensitivity.

Citation Information

Patent Citations

  • Negative photosensitive resin composition, cured film, element provided with cured film, display device and method for producing same

    CN111656277A

  • Light emitting diode packaging assembly

    CN210403726U

  • Display apparatus, glass substrate, and method of manufacturing glass substrate

    US20200135126A1

  • Display system

    WO2003012884A1

  • Photosensitive resin composition, cured film, organic el display, display device, and method for manufacturing cured film