Laminated ceramic electronic component
By adding and distributing smaller-diameter ceramic particles in the conductor paste, the problem of thinning and high continuity of the internal electrode layer is solved, the electrostatic capacitance of the laminated ceramic capacitor and the coating rate of the electrode layer are improved, and the The thickness deviation of the ceramic layer and the dielectric layer is eliminated.
Patent Information
- Application Number
- CN202280092337.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-22
- Filing Date
- 2022-08-31
- Publication Date
- 2024-10-01
AI Technical Summary
In laminated ceramic capacitors, it is difficult to achieve thinning and high continuity of internal electrode layers, resulting in reduced electrostatic capacitance and large thickness deviations between ceramic layers and dielectric layers.
By adding smaller-diameter ceramic particles to the conductor paste so that they are concentrated near the center of the thickness direction of the internal electrode layer, the distribution of the ceramic particles is controlled so that the area of the ceramic particles in the area where the Dsp index is below 40 reaches 50 % or more to ensure uniform distribution of ceramic particles and sintering of conductive metal particles.
It achieves thinning and high continuity of the internal electrode layer, while reducing the thickness deviation of the ceramic layer and the dielectric layer, and improving the coating rate and electrostatic capacitance characteristics of the electrode layer.
Smart Images

Figure CN118742982A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated ceramic electronic component having ceramic layers and internal electrode layers laminated alternately. Background Art
[0002] In a multilayer ceramic capacitor, which is an example of a multilayer ceramic electronic component, it is effective to reduce the thickness of an internal electrode layer as an internal conductor film in order to achieve a large capacity and a small size. The internal electrode layer is often formed by simultaneously firing a conductor paste film containing conductive metal particles such as nickel particles, an organic solvent, and an organic binder with a dielectric ceramic sheet.
[0003] In the above-mentioned firing process, the metal component contained in the conductor paste film and the ceramic component contained in the dielectric ceramic sheet generally have different shrinkage behaviors during firing. More specifically, the sintering temperature of the ceramic component is 1000°C or higher, while the sintering temperature of the metal component such as nickel is lower than 1000°C, for example, 600 to 800°C.
[0004] When the internal electrode is thinned, the difference in shrinkage behavior during sintering between the metal component contained in the conductor paste film and the ceramic component contained in the dielectric ceramic sheet can cause problems such as gaps in the internal electrode layer. That is, during the sintering process, the metal component starts sintering before the ceramic component, and the metal component excessively grows grains before the ceramic component reaches the temperature at which sintering starts, which reduces the continuity of the internal electrode layer. The reduction in the continuity of the internal electrode layer leads to a reduction in the electrostatic capacitance of the laminated ceramic capacitor.
[0005] To solve the above problem, a method is adopted in which ceramic particles called inhibitors are added to the conductor paste for forming the internal electrode to inhibit the sintering of the metal component. With the thinning of the internal conductor film in recent years, it is desired that the particle size of these inhibitors be 100 nm or less (see, for example, Patent Document 1).
[0006] However, the smaller the ceramic particles used in the inhibitor, the more significant the cohesion of the ceramic particles. Therefore, in the case of a conductor paste manufactured by applying a mixed dispersion treatment, if the particle size of the ceramic particles contained therein is micronized to, for example, less than 100 nm, it is difficult to evenly arrange the micronized ceramic particles around the conductive metal particles in the conductor paste due to the cohesion of the ceramic particles.
[0007] In this way, if the fine ceramic particles cannot be evenly arranged around the conductive metal particles, it is difficult to sinter the conductive metal particles from the parts where the ceramic particles do not exist, and it is difficult to achieve thinning and high continuity of the internal electrode layer formed using the conductor paste.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2001-110233 Summary of the invention
[0011] Problems to be solved by the invention
[0012] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide a multilayer ceramic electronic component having an internal electrode layer that can be thinned and has high continuity.
[0013] Technical solutions to solve problems
[0014] The inventors of the present invention have conducted in-depth research on stacked ceramic electronic components having internal electrode layers that can achieve thinning and high continuity. As a result, they found that the purpose of the present invention can be achieved by dispersing ceramic particles of smaller particle size while concentrating them near the center in the thickness direction of the internal electrode layer. The present invention has been completed.
[0015] That is, a first aspect of the present invention provides a laminated ceramic electronic component including ceramic layers and internal electrode layers laminated alternately, wherein:
[0016] In the observation range of the cross section intersecting the internal electrode layer,
[0017] The internal electrode layer contains a plurality of inner ceramic particles inside.
[0018] Regarding the relative position of the inner ceramic grains in the inner electrode layer relative to the central position in the thickness direction of the inner electrode layer, let the relative position correspond to the relative position from the central position to the edge position and the relative position be represented by a number from 0 to 100 as Dsp,
[0019] In the internal electrode layer, the area of the inner ceramic grains located in a region where Dsp is 40 or less accounts for 50% or more of the total area of the inner ceramic grains located in the observation range.
[0020] According to the first aspect of the present invention, inside the internal electrode layer, the area of the inner ceramic particles in the region where Dsp is less than 40, preferably less than 30, is more than 50% of the total area of the inner ceramic particles within the observation range. That is, more than half of the inner ceramic particles present in the observation range (more than 50% by area) are present in the region (near the center in the thickness direction) where Dsp is less than 40, preferably less than 30. The inventors of the present invention have confirmed that in a laminated ceramic electronic component having an internal electrode layer of such a structure, both the thinning and high continuity of the internal electrode layer can be satisfied. It has also been confirmed that while the thinning of the internal electrode layer is achieved, the thinning of the ceramic layers (e.g., dielectric layers) laminated in a manner sandwiched by a pair of internal electrode layers is also achieved, and the thickness deviation of these layers is also reduced.
[0021] A second aspect of the present invention provides a multilayer ceramic electronic component comprising ceramic layers and internal electrode layers alternately stacked, wherein:
[0022] In the observation range of the cross section intersecting the internal electrode layer,
[0023] The internal electrode layer contains a plurality of inner ceramic particles inside.
[0024] Regarding the relative position of the inner ceramic grains in the inner electrode layer relative to the central position in the thickness direction of the inner electrode layer, let the relative position correspond to the relative position from the central position to the edge position and the relative position be represented by a number from 0 to 100 as Dsp,
[0025] Inside the internal electrode layer, the area of the inner ceramic grains located in a region where Dsp is 75 or less, preferably 73 or less, accounts for 99% or more of the total area of the inner ceramic grains located in the observation range.
[0026] According to the second aspect of the present invention, inside the internal electrode layer, the area of the inner ceramic particles in the region where Dsp is less than 75, preferably less than 73, is more than 99% of the total area of the inner ceramic particles located within the observation range. That is, almost all (more than 99% by area) of the inner ceramic particles located within the observation range exist in the region where Dsp is less than 75, preferably less than 73. The inventors of the present invention have confirmed that in a laminated ceramic electronic component having an internal electrode layer of such a structure, the thinning and high continuity of the internal electrode layer can be satisfied at the same time. It has also been confirmed that while the thinning of the internal electrode layer is achieved, the thinning of the ceramic layers (such as dielectric layers) laminated in a manner sandwiched by a pair of internal electrode layers is also achieved, and the thickness deviation of these layers is also reduced.
[0027] Preferably, the ratio of the area of the inner ceramic particles to the total area of the internal electrode layer within the observation range is 2.5% or less, and more preferably 2% or less. According to the laminated ceramic electronic component having the internal electrode layer of such a structure, the coverage of the internal electrode layer relative to the ceramic layer is improved, and the continuity of the internal electrode layer is further improved.
[0028] Preferably, the maximum particle size of the inner ceramic particles within the observation range is 69 nm or less, and more preferably 63 nm or less. The maximum particle size of the inner ceramic particles being less than the specified value indicates that the aggregation of the fine-grained inhibitor particles (ceramic particles before firing) in the paste film for the internal electrode layer is suppressed. As a result of firing the paste film for the internal electrode layer by suppressing the aggregation of the inhibitor particles, the abnormal grain growth of the conductive particles in the paste film is suppressed, which contributes to the thinning of the internal electrode layer and the uniformity of the thickness, and the continuity of the internal electrode layer is further improved.
[0029] Preferably, every 50 μm of the internal electrode layer within the observation range 2 The number of the inner ceramic particles per area is 185 or less, more preferably 170 or less, for example, in the range of 55 to 166. Controlling the number of the inner ceramic particles contributes to thinning, and the coverage of the internal electrode layer relative to the ceramic layer is increased, and the continuity of the internal electrode layer is further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a cross-sectional view of a multilayer ceramic capacitor according to one embodiment of the present invention.
[0031] Figure 2 yes Figure 1 A partially enlarged photograph of a laminated cross section of dielectric layers and internal electrode layers is shown.
[0032] Figure 3 Yes Figure 2 A schematic diagram showing a portion of an internal electrode layer is shown in an enlarged schematic diagram.
[0033] Figure 4 It is used to illustrate Figure 3 Schematic diagram of Dsp of inner ceramic particles contained in a part of the internal electrode layer shown.
[0034] Figure 5 Yes means Figure 2 The graph shown is a graph of the relationship between the Dsp of each inner ceramic particle and the area cumulative frequency of the inner ceramic particles.
[0035] Figure 6 It is used to form Figure 2FIG. 1 is a schematic cross-sectional view of composite particles used in the paste for the internal electrode layer.
[0036] Figure 7 This is an explanatory diagram for measuring the inhibitor coverage rate in composite particles.
[0037] Figure 8 Then Figure 7 An illustration of the method for determining the inhibitor coverage.
[0038] Fig. 9 Then Figure 8 An illustration of the method for determining the inhibitor coverage. DETAILED DESCRIPTION
[0039] Hereinafter, the present invention will be described based on the embodiments shown in the drawings.
[0040] As an example of a laminated ceramic electronic component, a laminated ceramic capacitor 1 according to the present embodiment will be described. Figure 1 As shown, a multilayer ceramic capacitor 1 includes ceramic layers 2 and internal electrode layers 3 substantially parallel to a plane including the X-axis and the Y-axis, and includes a ceramic element body 10 in which the ceramic layers 2 and the internal electrode layers 3 are alternately stacked in the direction of the Z-axis.
[0041] Here, “substantially parallel” means that almost all parts are parallel, but there may be parts that are slightly non-parallel, and the gist of this is that the ceramic layer 2 and the internal electrode layer 3 may have slight irregularities or inclinations.
[0042] The internal electrode layers 3 are stacked in such a manner that each end is alternately exposed on the surface of two end faces that exist opposite to each other along the X-axis of the ceramic body 10. A pair of external electrodes 4 are formed on both end faces of the ceramic body 10 along the X-axis, and are connected to the exposed ends of each of the alternately arranged internal electrode layers 3 to form a capacitor circuit.
[0043] The external electrode conductive material included in the external electrode 4 is not particularly limited, but in this embodiment, cheap Ni, Cu, and alloys thereof can be used. The thickness of the external electrode 4 may be appropriately determined depending on the application, etc., and is usually 10 to 50 μm.
[0044] The thickness of the ceramic layer 2 is not particularly limited, and each layer is preferably 2 μm or less, more preferably 1.5 μm or less, further preferably 0.8 μm or less, and particularly preferably 0.5 μm or less. In addition, the thickness deviation σ of the ceramic layer 2 is preferably within 0.1 μm, further preferably within 0.063 μm, and particularly preferably within 0.05 μm.
[0045] In addition, the thickness of the internal electrode layer 3 is not particularly limited, and each layer is preferably 2 μm or less, more preferably 1.0 μm or less, further preferably 0.5 μm or less, and particularly preferably 0.5 μm or less. The lower limit of the thickness of the internal electrode layer 3 is preferably 0.298 μm or more, and further preferably greater than 0.4 μm. In addition, the thickness deviation σ of the internal electrode layer 3 is preferably within 0.3 μm, further preferably within 0.23 μm, and particularly preferably within 0.1 μm.
[0046] The number of stacked ceramic layers 2 (internal electrode layers 3 ) is not particularly limited, but is preferably 20 or more, and more preferably 50 or more.
[0047] As the material of the ceramic layer 2, for example, BaTiO 3 , CaTiO 3 , SrTiO 3 , CaZrO 3 , (K 1-x Na x )Sr2Nb5O 15 、Ba3TiNb4O 15 、(Ba 1-x Ca x )(Ti 1-y Zr y )O3 and other main components. In addition, auxiliary components such as Mn compounds, Mg compounds, Cr compounds, Co compounds, Ni compounds, rare earth elements, Si compounds, and Li compounds may be added to these main components.
[0048] The conductive component contained in the internal electrode layer 3 of the present embodiment is not particularly limited, and examples thereof include nickel, nickel alloy, copper, copper alloy, silver, and silver alloy, etc., but nickel or nickel alloy is preferred. The internal electrode layer 3 may also contain various trace components such as C, S, N, and O in an amount of about 1 mass % or less.
[0049] like Figure 2 As shown in FIG. 1 , the ceramic layer 2 as an insulating layer has a slight thickness deviation along the Z axis direction, but is almost continuous along the X axis and the Y axis. The internal electrode layer 3 as a conductive layer may also have an electrode discontinuity 3b along the X axis or the Y axis. Figure 2 Within the observation range, the internal electrode layer 3 may be composed of internal electrode portions 3a that appear discontinuous along the X-axis or the Y-axis.
[0050] Furthermore, the inner electrode portion 3a which appears to be discontinuous along the X-axis or the Y-axis is actually Figure 1The other cross sections of the ceramic element body 10 shown are connected, and there will be no poor connection, but the fewer the electrode discontinuities 3b, the higher the coverage of the electrode layer 3 relative to the ceramic layer 2, and the higher the electrostatic capacitance and other properties. Generally speaking, as the internal electrode layer 3 and the ceramic layer 2 are thinned, the electrode discontinuities 3b are easily generated, and there is a tendency for the electrode coverage to decrease.
[0051] For example, it is possible to Figure 3 The electrode coverage was determined by the method shown in Figure 2 In the cross-sectional photograph shown, an enlarged schematic diagram of a certain internal electrode layer 3 is shown in Figure 3 .exist Figure 3 As an example, it is assumed that the internal electrode layer 3 having a length L has two electrode discontinuities 3b in the X-axis or Y-axis direction within the observation range of the cross-sectional photograph. The electrode coverage in this case can be obtained by dividing the sum of the lengths L1, L2, and L3 of each electrode portion 3a along the X-axis or Y-axis direction by the total length L of the internal electrode layer 3. The coverage can also be expressed in %. In addition, the coverage can also be calculated for a predetermined number of (for example, more than 10) layers of internal electrode layers 3 within the observation range of the cross-sectional photograph and obtained as their average value.
[0052] In the present embodiment, while maintaining the thinness of the internal electrode layer 3, the electrode coverage is preferably 70% or more, and more preferably 80% or more, within a specified cross-sectional observation range (e.g., 12 μm×8 μm). In addition, in the present embodiment, within a specified cross-sectional observation range (e.g., 12 μm×8 μm), the number of electrode portions 3a (number of electrode divisions) of each internal electrode layer is preferably 5 or less, more preferably 3 or less, and particularly preferably 2 or less.
[0053] like Figure 2 and Figure 4 As shown in FIG. 1 , ceramic particles 36a having a relatively small particle size exist inside the electrode portion 3a of the internal electrode layer 3 of the present embodiment. Figure 2 In FIG. 3 , the ceramic particles 36a are observed as black dots observed inside the gray electrode portion 3a. Figure 2 Although it may not be obvious in the figure, the ceramic layer 2 is actually formed by connecting ceramic particles having a larger particle size than the ceramic particles 36a. In the present embodiment, the ceramic particles 36a observed inside the electrode portion 3a of the internal electrode layer 3 are also referred to as inner ceramic particles 36a in order to distinguish them from the ceramic particles of the ceramic layer 2.
[0054] In the present embodiment, the inner ceramic particles 36a are dispersed inside the internal electrode layer 3 and are located near the center in the thickness direction (approximately parallel to the Z-axis direction) of the internal electrode layer 3. In the present embodiment, the index Dsp is used as an index indicating the thickness direction position of the inner ceramic particles 36a inside the internal electrode layer 3. The index Dsp is obtained, for example, as follows.
[0055] For example, from Figure 2 The cross-sectional photograph shown in FIG. 1 shows an electrode portion 3a of an internal electrode layer 3 extracted and schematically illustrated. Figure 4 .exist Figure 4 For example, focusing on an inner ceramic particle 36a, a vertical line parallel to the thickness direction of the electrode portion 3a (roughly parallel to the Z-axis direction) is drawn through the center of gravity of the particle 36a, and the length from the vertical line to the intersection with the upper edge and the lower edge of the electrode portion 3a is set as the electrode width Z0. Next, the midpoint position (central position) O of the electrode width Z0 is calculated, and the distance Z1 from the midpoint position O to the center of gravity of the particle 36a is calculated. The value obtained by dividing the distance Z1 by the distance Z2 and marking it as a percentage is set as the index Dsp. Among them, the distance Z2 is a value of 1 / 2 of the distance Z0.
[0056] For each ceramic particle 36a, Dsp can be calculated by automatic calculation using an image processing algorithm. Also, for each ceramic particle 36a, each area S0 can be calculated by automatic calculation using an image processing algorithm.
[0057] Dsp can be represented by a number from 0 to 100, and a ceramic particle 36a having a Dsp of 0 refers to a ceramic particle 36a located at the midpoint position O of the vertical line Z0. In addition, a ceramic particle 36a having a Dsp of 100 refers to a ceramic particle 36a located at the upper edge or lower edge of the electrode portion 3a farthest from the midpoint position O of the vertical line Z0. The closer Dsp is to 0, the closer the ceramic particle 36a is to the midpoint position, and conversely, the closer Dsp is to 100, the closer the ceramic particle 36a is to the upper edge or lower edge of the internal electrode layer 3.
[0058] In this embodiment, inside the internal electrode layer 3, the area of the inner ceramic particles 36a in the region where Dsp is less than 40 is more than 50% of the total area of the inner ceramic particles 36a located within the observation range of the cross-sectional photograph (for example, 12μm×8μm). In addition, preferably, the inner ceramic particles 36a in the region where Dsp is less than 30 is more than 50% of the total area of the inner ceramic particles 36a located within the observation range of the cross-sectional photograph (for example, 12μm×8μm).
[0059] Preferably, the inner ceramic grains 36a in the region where Dsp is 75 or less, preferably 73 or less, account for 99% or more of the total area of the inner ceramic grains 36a located within the observation range (eg, 12 μm×8 μm) of the cross-sectional photograph.
[0060] exist Figure 2 In order to determine whether the inner ceramic grains 36a are present in the internal electrode layer 3 in an area where Dsp is less than a predetermined value within the observation range of the cross-sectional photograph shown, for example, the following is performed.
[0061] Figure 5 Yes means Figure 2 The relationship between the Dsp of each inner ceramic particle 36a and the area cumulative frequency of the inner ceramic particles is shown in the graph. For example, image analysis software can be used according to Figure 2 The image shown is automatically calculated. The horizontal axis represents the value of Dsp, and the vertical axis represents the frequency of the area accumulation of the inner ceramic grains 36a within the observation range of the cross-sectional photograph. The area accumulation of the inner ceramic grains 36a is accumulated starting from the area of the inner ceramic grains 36a where Dsp is close to 0.
[0062] exist Figure 5 In the graph, the line connecting the circled plot points represents an embodiment of the present invention, and the × mark represents a comparative example of the present invention. In the embodiment, the value of Dsp at the position of 50% of the area cumulative frequency (Dsp50) is 25, and the value of Dsp at the position of 99% of the area cumulative frequency (Dsp99) is 60.
[0063] That is, according to Figure 5 As shown in the diagram, in the embodiment, since Dsp50 is 25, it can be said that Figure 2 More than half (more than 50% by area) of the inner ceramic particles 36a within the observation range of the cross-sectional photograph shown in FIG. 1 exist in the region (near the center in the thickness direction) where Dsp is 40 or less, preferably 30 or less. In the embodiment, Dsp99 is 60, so it can be said that the inner ceramic particles 36a are located in the region where Dsp is 40 or less, preferably 30 or less. Figure 2 Most (99% or more by area) of the inner ceramic grains 36 a within the observation range of the cross-sectional photograph shown are present in the region where Dsp is 60 or less (near the center in the thickness direction).
[0064] The area cumulative frequency refers to a cumulative relative frequency (0 to 100) obtained by cumulatively accumulating the areas of the ceramic particles 36 a included in the internal electrode layer 3 within the observation range.
[0065] Next, Figure 1 and Figure 2A method for manufacturing the multilayer ceramic capacitor 1 shown will be described.
[0066] First, a ceramic green sheet containing a ceramic material for forming the ceramic element body 10 is prepared. Next, a conductor paste is applied to the ceramic green sheet to form a conductive pattern corresponding to the internal electrode layer 3. The conductor paste of this embodiment contains, for example, Figure 6 The composite particles 32 shown in the figure are preferably kneaded relatively smoothly in order to maintain the structure of the composite particles 32, preferably by using a rotary mixer. Figure 6 The details of the composite particles 32 shown will be described later.
[0067] The conductor paste can be applied by various printing methods such as screen printing. However, since the conductor paste of the present embodiment contains composite particles 32, it is preferably applied by screen printing or gravure printing in order to maintain the structure of the composite particles 32.
[0068] A mother laminate is produced by sequentially stacking a plurality of ceramic green sheets without a conductive pattern, a ceramic green sheet with a conductive pattern, and a plurality of ceramic green sheets without a conductive pattern and punching them in a stacking direction.
[0069] By cutting the mother laminate, a plurality of green ceramic bodies are produced. In addition, the cutting of the mother laminate can be performed by cutting or trimming. Furthermore, the green ceramic body can also be subjected to drum grinding or the like to round off the ridges or corners.
[0070] Before firing, the green chip is subjected to a debinding treatment. As debinding conditions, the heating rate is preferably set to 5 to 300°C / hour, the holding temperature is preferably set to 180 to 800°C, and the temperature holding time is preferably set to 0.5 to 24 hours. In addition, the debinding atmosphere is set to air or a reducing atmosphere. The heating rate during firing is not particularly limited, but is preferably 50 to 500°C / hour, and more preferably 200 to 300°C / hour.
[0071] The holding temperature during calcination is preferably 1200-1350° C., more preferably 1220-1300° C., and the holding time is preferably 0.5-8 hours, more preferably 2-3 hours. The calcination atmosphere is preferably a reducing atmosphere, and as the atmosphere gas, for example, a humidified mixed gas of N2 and H2 can be used.
[0072] The oxygen partial pressure during firing may be appropriately determined according to the type of conductive material in the conductor paste. However, when a base metal such as Ni or a Ni alloy is used as the conductive material, the oxygen partial pressure in the firing atmosphere is preferably set to 10 -14 ~10 -10 The temperature drop rate is preferably 50 to 500°C / hour.
[0073] The ceramic body 10 may be annealed after being fired in a reducing atmosphere. The oxygen partial pressure in the annealing atmosphere is set to 10 -9 ~10 -5 MPa, the holding temperature during annealing is set to 950 to 1150° C., and the holding time is set to 0 to 20 hours. In addition, as the atmosphere gas for annealing, for example, humidified N 2 gas can be used.
[0074] In the above-mentioned binder removal treatment, firing and annealing, a humidifier may be used to humidify the N2 gas or the mixed gas. In this case, the water temperature is preferably about 5 to 75° C. The binder removal treatment, firing and annealing may be performed continuously or independently.
[0075] The ceramic element body 10 obtained as described above is subjected to end surface grinding by, for example, barrel grinding or sandblasting, and then coated with an external electrode paste and fired to form an external electrode 4. Then, as required, a coating layer is formed on the surface of the external electrode 4 by plating or the like. In addition, the external electrode paste contains a known binder or solvent in addition to the external electrode conductive particles constituting the external electrode conductive material after firing.
[0076] The multilayer ceramic capacitor 1 of the present embodiment manufactured in this manner is mounted on a printed circuit board or the like by soldering or the like, and is used in various electronic devices or the like.
[0077] Next, based on Figure 6 to Figure 9 The composite particles 32 will be described.
[0078] like Figure 6 As shown in FIG. 1 , the composite particles 32 of the present embodiment include conductive particles 34 and inhibitor particles 36 attached to the surface of the conductive particles 34 and having a smaller particle size than the conductive particles 34. The conductive particles 34 are contained in the conductive paste printing pattern and become Figure 1 and Figure 2 The material of the internal electrode layer 3 is not particularly limited, but is preferably at least one selected from Ni, Ni alloy, Cu, Cu alloy, Ag and Ag alloy, and more preferably Ni or Ni alloy. In addition, the conductive particles 34 may contain various trace components such as C, S, N and O in an amount of about 1 mass % or less.
[0079] In the present embodiment, as the conductive particles 34 , a plurality of conductive particles 34 made of the same material may be used, or a plurality of conductive particles 34 made of different materials may be mixed.
[0080] The particle size (R) of the conductive particles 34 of this embodiment is preferably 20 nm or more and 300 nm or less, preferably 25 nm or more and 150 nm or less. In this embodiment, since the inhibitor particles 36 are attached to the surface of the conductive particles 34 even if the conductive particles 34 are relatively fine, the sintering start temperature can be shifted to the high temperature side. In addition, by making R within the above range, it is easy to achieve thinning of the internal electrode layer 3. From the above viewpoint, R is preferably less than at least 1 / 5 of the thickness of the internal electrode layer 3.
[0081] exist Figure 2 and Figure 4 In the embodiment, the inhibitor particles 36 are the ceramic particles 36a in the internal electrode layer 3 after firing. The material thereof is not particularly limited, but is preferably a material having the effect of shifting the sintering start temperature of the internal electrode layer 3 to the high temperature side, more preferably an oxide, and further preferably insulating. Specific examples of the material having the effect of shifting the sintering start temperature of the internal electrode layer 3 to the high temperature side, being an oxide and being insulating include barium titanate, barium calcium titanate, barium strontium titanate, (Ba 1-x Ca x )(Ti 1-y Zr y ) At least one of O3, silicon oxide, titanium oxide, zirconium oxide and aluminum oxide, preferably barium titanate or silicon oxide, more preferably barium titanate.
[0082] The inhibitor particles 36 of this embodiment preferably have crystallinity. This can shift the sintering start temperature of the internal electrode layer 3 to a higher temperature. For example, the crystallinity can be confirmed by a scanning transmission electron microscope (STEM) or an X-ray diffraction method (XRD).
[0083] In addition, the inhibitor particles 36 of this embodiment are smaller than the conductive particles 34. In addition, the particle size (r) of the inhibitor particles 36 is 2 nm to 30 nm, preferably 5 nm to 20 nm. When r is within the above range, the inhibitor particles can be easily dispersed.
[0084] In the present embodiment, when the particle size of the conductive particles 34 is represented by R and the particle size of the inhibitor particles 36 attached to the conductive particles 34 is represented by r, (r / R) is preferably 0.01 or more and 0.17 or less, and more preferably 0.03 or more and 0.15 or less. By setting r / R within the above range, the inhibitor particles 36 are less likely to fall off from the conductive particles 34.
[0085] In the present embodiment, as the inhibitor particles 36 , a plurality of inhibitor particles 36 made of the same material may be used, or inhibitor particles obtained by mixing a plurality of inhibitor particles 36 made of different materials may be used.
[0086] When the inhibitor particles 36 are composed of two or more inhibitor particles 36 of different materials, the average particle size of the inhibitor particles 36 composed of a certain material and the average particle size of the inhibitor particles 36 composed of another material may be different.
[0087] In addition, the particle diameters of the conductive particles 34 and the inhibitor particles 36 and the coverage of the inhibitor particles 36 with respect to the conductive particles 34 according to the present embodiment are measured in the following manner.
[0088] The liquid containing the composite particles 32 is dropped onto a scanning electron microscope (SEM) or a STEM stage and air-dried. Next, a SEM image or the like is taken. Figure 7 Schematic diagram showing a SEM image. The field of view of the SEM image or the like is not particularly limited, but when the average particle size of the conductive particles 34 is represented by R, it may be approximately (R×8)×(R×6).
[0089] Next, “conductive particles 34 whose outlines can be confirmed” are screened from the SEM image or the like. Figure 8 In the middle, the bold line indicates Figure 7 The outline of the "conductive particles 34 whose outlines can be confirmed" is shown in FIG. 1 , and the outline of the "inhibitor particles 36 whose outlines can be confirmed" attached to the "conductive particles 34 whose outlines can be confirmed" is also shown in bold. In addition, the "conductive particles 34 whose outlines can be confirmed" means that the entire outline is included in the SEM image, etc., and the conductive particles 34 that exist in the front in the SEM image, etc. Therefore, even if a part is missing, the conductive particles 34 will not become "conductive particles 34 whose outlines can be confirmed". In addition, in the case where a part exists behind (on the back side) of other conductive particles 34, the conductive particles 34 will not become "conductive particles 34 whose outlines can be confirmed".
[0090] Regarding the "conductive particles 34 whose outlines can be confirmed" confirmed by the above method and the "inhibitor particles 36 whose outlines can be confirmed" attached to the "conductive particles 34 whose outlines can be confirmed", the equivalent circle diameters are calculated respectively, and the particle size (R) of the conductive particles 34 and the average particle size (r) of the particles 36 are calculated respectively using the equivalent circle diameter as the particle size.
[0091] Moreover, if Fig. 9As shown in FIG. 1 , the center of gravity G of each of the "conductive particles 34 whose outlines can be confirmed" is obtained, and a circle with a radius of "0.25×the particle diameter (Ra) of the conductive particles" is drawn from the center of gravity G, and the circle is taken as the virtual circle 38. In addition, the "particle diameter Ra" refers to the particle diameter of each conductive particle 34, not the average particle diameter. The total area of the inhibitor particles 36 contained in the virtual circle 38 relative to the area of the virtual circle 38 is set as the coverage rate. Figure 7 and Figure 8 The coverage ratios of all the “conductive particles 34 whose outlines can be confirmed” are calculated, and the average value thereof is defined as the average coverage ratio.
[0092] In the present embodiment, the average coverage of the inhibitor particles 36 with respect to the conductive particles 34 is preferably 3% or more and 50% or less, and more preferably 5% or more and 30% or less. In addition, the coverage deviation represented by the standard deviation of the coverage is preferably 0% or more and 20% or less, and more preferably 0% or more and 5% or less. In the present embodiment, the inhibitor particles 36 are attached to the conductive particles 34 by electrostatic adsorption described later, thereby suppressing the aggregation of the inhibitor particles 36, and thus the coverage deviation can be suppressed to be low.
[0093] In the present embodiment, the ratio of the number of composite particles 32 with a coverage of 0% to the number of composite particles 32 observed, that is, the ratio of composite particles 32 with a coverage of 0%, is preferably 60% or less, and more preferably 10% or less.
[0094] In the present embodiment, for example, when r / R=0.07 to 0.09, the number of inhibitor particles 36 included in the imaginary circle 38 is preferably 0 or more and 20 or less, and more preferably 1 or more and 15 or less. In addition, “the inhibitor particles 36 included in the imaginary circle 38” do not include inhibitor particles 36 that are partially missing.
[0095] In the present embodiment, the number of aggregated inhibitor particles 36 in the field of view of (R×80)×(R×60) is preferably 3 or less, more preferably 1 or less, and further preferably 0. In the present embodiment, the content of the inhibitor particles 36 relative to the conductive particles 34 is preferably 1 vol% or more and 23 vol% or less, and more preferably 2 vol% or more and 15 vol% or less.
[0096] Next, Figure 6 A method for producing the composite particles 32 shown will be described.
[0097] First, in this embodiment, the conductive particles 34 and the inhibitor particles 36 are prepared, and the inhibitor particles 36 are attached to the surfaces of the conductive particles 34 to produce a Figure 6The composite particles 32 shown. The method for attaching the inhibitor particles 36 to the surface of the conductive particles 34 is not particularly limited. For example, the inhibitor particles 36 may be attached to the surface of the conductive particles 34 by electrostatic adsorption, by a chemical kinetic method, by a method in which the inhibitor particles 36 are precipitated on the surface of the conductive particles 34 by synthesis, or by an organic material such as a resin.
[0098] In the present embodiment, it is preferred that the inhibitor particles 36 be attached to the surface of the conductive particles 34 by electrostatic adsorption. The reason for this is that, in the case of electrostatic adsorption, the inhibitor particles 36 can be attached to the surface of the conductive particles 34 with low energy. In addition, in the case of electrostatic adsorption, the inhibitor particles 36 can be adsorbed to the conductive particles 34 in a state close to monodisperse.
[0099] Furthermore, in the case of electrostatic adsorption, a separately synthesized "material with high crystallinity", "material with high heat resistance" and / or "material close to spherical shape" can be used as the inhibitor particles 36, thereby maximizing the inhibitor effect of the inhibitor particles 36. In addition, the closer the inhibitor particles 36 are to spherical shapes, the smaller the specific surface area (a sphere is the smallest), and there is a tendency to increase the sintering start temperature by reducing the surface free energy.
[0100] Furthermore, in the case of electrostatic adsorption, it is possible to reduce aggregation of inhibitor particles 36. Aggregation of inhibitor particles 36 may reduce the number of inhibitor particles 36 that effectively function as inhibitors, and may become a cause of the starting point of electrode discontinuity.
[0101] Furthermore, since the thickness of electrostatic adsorption can be changed by changing the particle size of the inhibitor particles 36, it is easy to control the adsorption thickness of the inhibitor (inhibitor particles 36) on the surface of the conductive particles 34. Furthermore, in the case of electrostatic adsorption, there is also an advantage that after the conductive particles 34 and the inhibitor particles 36 are respectively charged with opposite charges, it is easy to control the amount of the inhibitor particles 36 attached to the conductive particles 34 due to adsorption.
[0102] For the above reasons, by attaching the inhibitor particles 36 to the surfaces of the conductive particles 34 by electrostatic adsorption, the effect of shifting the sintering start temperature of the composite particles 32 to the high temperature side can be further enhanced.
[0103] The oxide nanoparticles used as the inhibitor particles 36 have hydroxyl groups on the outermost surface, so they are basically well dispersed in highly hydrophilic water or highly polar solvents such as ethanol or ethylene glycol. Although it depends on the preparation method or dispersion method, the oxide nanoparticles have a negative surface charge in most cases and can be used for composite formation. A trace amount of additives may also be present to stabilize the dispersion.
[0104] The nickel powder used as the conductive particles 34 has a very weak positive or negative charge, although it also depends on the production method. It can be changed to a strong positive charge by using a polymer electrolyte such as polydimethyl ammonium chloride (PDDA) and polyethyleneimine (PEI), and can be composited with negative oxide nanoparticles (inhibitor particles 36).
[0105] When BaTiO 3 is used as the inhibitor particles 36 , for example, the composite is formed by the following method: First, Ni particles (conductive particles 34 ) having a positive surface charge are introduced into an organic solvent to prepare a “dispersion liquid containing Ni particles having a positive surface charge”.
[0106] Furthermore, a "dispersion liquid containing BaTiO3 with a negatively charged surface" is also prepared. The reason for using an organic solvent is that if the solvent is water, the surface ions of BaTiO3 will be eluted into the water. In addition, as a solvent for the BaTiO3 solution, ethanol, ethylene glycol, ketone, etc. can be used.
[0107] The “dispersion liquid containing Ni particles having a positive surface charge” and the “dispersion liquid containing BaTiO 3 particles having a negative surface charge” are mixed, and the BaTiO 3 particles are adsorbed on the Ni particles by electrostatic adsorption, thereby obtaining composite particles 32 .
[0108] The internal electrode layers 3 of the multilayer ceramic capacitor 1 of the present embodiment can be formed of, for example, a conductor paste containing composite particles 32. The composite particles 32 are fine, and thus can meet the requirement for a thinner multilayer ceramic capacitor 1.
[0109] In addition, the inhibitor particles 36 have the effect of shifting the sintering start temperature of the composite particles 32 to the high temperature side, and the composite particles 32 are structures in which the inhibitor particles 36 are attached to the surface of the conductive particles 34. According to the conductor paste having the composite particles 32 of this embodiment, the sintering start temperature of the composite particles 32 can be efficiently shifted to the high temperature side and can be close to the sintering start temperature of the ceramic layer 2. As a result, cracks in the ceramic layer 2 caused by the difference in thermal shrinkage behavior between the internal electrode layer 3 and the ceramic layer 2 can be prevented, and electrode discontinuity in the internal electrode layer 3 can be prevented.
[0110] Furthermore, as described above, the composite particles 32 of this embodiment can efficiently shift the sintering start temperature of the internal electrode layer 3 to the high temperature side, so the inhibitor content can be reduced compared to conventional conductor pastes. This can reduce the influence of the inhibitor on the ceramic layer 2.
[0111] In addition, by using the composite particles 32 of the present embodiment, for example Figure 2 As shown, ceramic particles 36a composed of sintered inhibitor particles 36 are often located near the center in the thickness direction of the internal electrode layer 3, and the area ratio of ceramic particles 36a in the region where Dsp is below a predetermined value increases to above a predetermined value.
[0112] In this embodiment, the Figure 2 More than half (more than 50% by area) of the inner ceramic particles 36a within the observation range of the cross-sectional photograph shown are present in the region (near the center in the thickness direction) where Dsp is 40 or less, preferably 30 or less. In the laminated ceramic capacitor 1 having the internal electrode layer 3 of such a structure, both thinning and high continuity of the internal electrode layer 3 can be achieved. In addition, while thinning of the internal electrode layer 3 is achieved, thinning of the ceramic layer 2 (e.g., dielectric layer) laminated in a manner sandwiched by a pair of internal electrode layers 3 is also achieved, and the thickness deviation of these layers is reduced.
[0113] In addition, in this embodiment, Figure 2 Almost all of the inner ceramic particles 36a within the observation range of the cross-sectional photograph shown (more than 99% by area) exist in the region where Dsp is less than 75, preferably less than 73. In the laminated ceramic capacitor 1 having the internal electrode layer 3 of such a structure, both thinning and high continuity of the internal electrode layer 3 can be achieved. In addition, while thinning the internal electrode layer 3 is achieved, thinning of the ceramic layer 2 (e.g., dielectric layer) laminated in a manner sandwiched by a pair of internal electrode layers 3 is also achieved, and the thickness deviation of these layers is also reduced.
[0114] In addition, the ratio of the total area of the inner ceramic particles 36a to the total area of the internal electrode layer located in the observation range is preferably 2.5% or less, and more preferably 2% or less. According to the laminated ceramic capacitor 1 having the internal electrode layer 3 of such a structure, the coverage of the internal electrode layer 3 with respect to the ceramic layer 2 is improved, and the continuity of the internal electrode layer 3 is further improved.
[0115] Moreover, in this embodiment, the maximum particle size of the inner ceramic particles 36a within the observation range is 69 nm or less, and more preferably 63 nm or less. The maximum particle size of the inner ceramic particles 36a is less than the specified value, indicating that the inhibitor particles (e.g. Figure 6 The aggregation of the inhibitor particles 36 shown in FIG. 1 is suppressed. As a result of suppressing the aggregation of the inhibitor particles 36 and firing the internal electrode layer paste film, the paste film Figure 6 The abnormal grain growth of the conductive particles 34 is suppressed. Figure 2 This contributes to the thinning and uniformity of the thickness of the internal electrode layer 3 shown, and the continuity of the internal electrode layer 3 is further improved.
[0116] In addition, for example, Figure 2 The internal electrode layer 3 has a thickness of 50 μm in the observation range of the cross-sectional photograph shown. 2 The number of the inner ceramic particles 36a per area is 185 or less, more preferably 170 or less, for example, in the range of 55 to 166. By suppressing the number of the inner ceramic particles 36a, the thinning of the internal electrode layer 3 is contributed to, and the coverage of the internal electrode layer 3 with respect to the ceramic layer 2 is improved, and the continuity of the internal electrode layer 3 is further improved.
[0117] In addition, the present invention is not limited to the above-mentioned embodiment, and various changes can be made within the scope of the present invention.
[0118] For example, the electronic components of this embodiment are not limited to laminated ceramic capacitors, but can be applied to other electronic components. Other electronic components include all electronic components in which ceramic layers are laminated via internal electrode layers, such as bandpass filters, inductors, laminated three-terminal filters, piezoelectric elements, PTC thermistors, NTC thermistors, varistors, etc.
[0119] The internal electrode layer 3 of the present embodiment can also be obtained by sintering a combination of conductive particles and inhibitors having a structure other than the composite particles 32. The material of the conductive particles is not particularly limited, and Ni, Ni-based alloys, Cu, Cu-based alloys, etc. can be used.
[0120] In addition, the internal electrode layer 3 may include ceramic particles 36a not derived from the inhibitor particles 36. The ceramic particles 36a not derived from the inhibitor particles 36 may not be derived from the conductor paste as part of the composite particles 32, but may be derived from particles included in another form. The material of the particles not derived from the inhibitor particles 36 is not particularly limited, but in order to reduce the influence on the composition of the ceramic layer 2, it is preferably the same as the material of any component constituting the ceramic layer 2.
[0121] Furthermore, when forming the external electrode 4, instead of forming by firing the paste, the external electrode 4 may be formed from a resin containing the composite particles 32. That is, the external electrode 4 may be a resin electrode containing the composite particles 32.
[0122] Example
[0123] Hereinafter, the present invention will be described based on more detailed examples, but the present invention is not limited to these examples.
[0124] Example 1
[0125] D50: In an ethanol dispersion of 100 nm nickel powder (initial zeta potential of +8 mV), 400 ppm of polymer electrolyte polyethyleneimine (PEI) was prepared relative to the weight of nickel and dissolved in ethanol. The zeta potential of the dissolved nickel was measured (Zetasizer Nano manufactured by Malvern) and showed +30 mV, thus confirming that the nickel surface had a negative potential due to PEI.
[0126] Next, an ethanol dispersion of barium titanate (inhibitor particles) (D50: 10 nm) was prepared as oxide nanoparticles. The zeta potential of the dispersion of barium titanate was measured by the same apparatus as above, showing -20 mV. Thus, it was confirmed that the zeta potential of the nickel surface was positive, and the zeta potential of the untreated barium titanate surface was negative.
[0127] Next, the two dispersions were mixed, dispersed for 10 minutes using an ultrasonic homogenizer, and then dried at 100°C for 1 hour. The dried composite powder was mixed with a solvent (pinene alcohol) and a binder (ethyl cellulose) to complete a paste containing composite particles. At this time, the weight of barium titanate was set to 5 parts by weight (5PHP) relative to 100 parts by weight of nickel particles (conductive particles). In addition, the volume % of barium titanate was 6.9 vol%.
[0128] In the conductor paste thus obtained, when the entire paste was 100 parts by mass, the composite particles accounted for 45 parts by mass, the ethyl cellulose accounted for 3 parts by mass, and the solvent accounted for 52 parts by mass.
[0129] In addition, composite particles different from the composite particles contained in the conductive paste are added to ethanol at a ratio of 0.5 mass %, and mixed by a vortex oscillator for 1 minute. Let it stand for 1 to 2 hours to allow the composite particles to settle. Remove the supernatant by decantation, and add ethanol again and mix. Drop the liquid containing the obtained composite particles on the SEM workbench, air-dry it, and observe it under SEM. Determine the coverage rate of the inhibitor particles relative to the conductive particles. The results are shown in Table 1. The average inhibitor coverage rate is 30%.
[0130] Next, a conductor paste is applied to a ceramic green sheet mainly composed of BaTiO3 to form a conductive pattern corresponding to the internal electrode layer 3. A plurality of ceramic green sheets without conductive patterns, ceramic green sheets with conductive patterns, and a plurality of ceramic green sheets without conductive patterns are sequentially stacked and punched in the stacking direction to produce a mother laminate.
[0131] The mother laminated body is cut to produce a plurality of pre-fired ceramic bodies (green chips). The green chips are then subjected to a binder removal treatment, firing and annealing under the following conditions to obtain a laminated ceramic fired body (ceramic body).
[0132] The binder removal treatment conditions were as follows: a temperature increase rate of 25° C. / hour, a holding temperature of 500° C., a temperature holding time of 8 hours, and an atmosphere of a humidified N 2 +H 2 mixed gas.
[0133] The firing conditions were set to a heating rate of 200°C / hour, a holding temperature of 1200-1350°C, and a holding time of 1 hour. The cooling rate was set to 200°C / hour. In addition, the atmosphere gas was set to a humidified N2+H2 mixed gas, and the oxygen partial pressure was set to 10 -12 MPa.
[0134] The annealing conditions were as follows: heating rate: 200°C / hour, holding temperature: 1000°C, temperature holding time: 2 hours, cooling rate: 200°C / hour, atmosphere gas: humidified N2 gas (oxygen partial pressure: 10 -7 MPa).
[0135] In addition, a humidifier is used to humidify the atmospheric gas during firing and annealing.
[0136] Next, the end faces of the obtained ceramic body were polished by sandblasting, and then Cu was applied as external electrodes to obtain Figure 1 The size of the obtained capacitor sample was 1.0 mm×0.5 mm×0.5 mm.
[0137] The capacitor sample was cut into a cross section parallel to the Z axis, and the cross section was observed by SEM. The cross section observation range was 8 μm×12 μm or more, which was the range in which more than 10 internal electrode layers 3 were observed. Figure 2 The cross section shown in the figure is image processed, thereby, through the above Figure 4 The method shown in the figure measures the Dsp of at least 50 or more inner ceramic particles 36a located inside each inner electrode layer 3. In addition, the area of the inner ceramic particles 36a for which the Dsp is measured is measured in association with the value of Dsp and cumulatively added, and the relationship between the ratio (area cumulative frequency) to the total area of all observed inner ceramic particles 36a and Dsp is calculated. Figure 5 The line connecting the dots represents the data in the form of a graph of the relationship.
[0138] According to Figure 5The Dsp50 and Dsp99 are obtained from the graph represented by the line connecting the dots or the raw data of the graph. The results are shown in Table 1. As shown in Table 1, in Example 1, Dsp50 is 25 and Dsp99 is 60. In addition, Dsp50 refers to the value of Dsp at the position of 50% of the area cumulative frequency as described above, and Dsp99 refers to the value of Dsp at the position of 99% of the area cumulative frequency.
[0139] In addition, for example, by Figure 2 The cross section shown in FIG. 1 is subjected to image processing, and the inner ceramic particles with the largest particle size are detected in at least 50 or more inner ceramic particles 36a located inside each internal electrode layer 3, and their area is calculated. The results are shown in Table 1. In addition, for example, the area existing in Figure 2 The internal electrode layer 3 has a thickness of 50 μm in the observation range of the cross-sectional photograph shown. 2 The number of inner ceramic particles 36a in the area. The results are shown in the column of the number of ceramic particles in Table 1.
[0140] Moreover, in Figure 2 In the observed range of the cross section shown, the average value and the variation σ of the thickness of the dielectric layer 2 and the average value and the variation σ of the thickness of the internal electrode layer 3 were measured by image processing.
[0141] In addition, according to Figure 2 By observing the cross section shown in FIG. 1 , the electrode coverage of the internal electrode layer 2, the number of electrode divisions, and the area ratio of the ceramic particles are measured and obtained. Figure 3 The electrode coverage is calculated by the method shown in the figure. The number of electrode divisions is calculated by dividing the total number of electrode portions 3a observed in the cross-sectional SEM images of the internal electrode layers 3 observed 10 or more times by the total number of the internal electrode layers 3, for example.
[0142] The area ratio of the ceramic particles was determined by calculating the ratio of the total area of the ceramic particles 36a to the total area of the electrode portion 3a in the cross-sectional SEM image of the internal electrode layer observed for 10 or more times, and the ratio was defined as the area ratio.
[0143] Embodiments 2 to 6
[0144] Capacitor samples were prepared in the same manner as in Example 1 except that the weight of barium titanate in the conductor paste was 7 parts by weight (7PHP), 9PHP, 11PHP, 13PHP, and 15PHP relative to 100 parts by weight of the nickel particles. The inhibitor coverage of the composite particles used in each of Examples 2 to 6 was measured in the same manner as in Example 1. The results are shown in Table 1.
[0145] In addition, Dsp50, Dsp99, the maximum diameter of ceramic particles, the number of ceramic particles, the average value of dielectric thickness and its deviation σ, the average value of the thickness of the internal electrode layer (electrode thickness) and its deviation σ, the electrode coverage, the number of electrode divisions, and the ceramic particle area ratio of the capacitor sample of each embodiment were obtained in the same manner as in Example 1. These results are shown in Table 1 or Table 2.
[0146] Comparative Example 1
[0147] A capacitor sample was manufactured in the same manner as in Example 1, except that nickel particles (conductive particles) and barium titanate (inhibitor particles) were prepared separately instead of composite particles, and these were mixed and dispersed with a solvent (pinene alcohol) and a binder (ethyl cellulose) to prepare a conductor paste. The inhibitor coverage of the inhibitor particles on the surface of the conductive particles in the conductor paste used in Comparative Example 1 was measured in the same manner as in Example 1. The results are shown in Table 1.
[0148] In addition, the Dsp50, Dsp99, the maximum diameter of the ceramic particles, the number of ceramic particles, the average value of the dielectric thickness and its deviation σ, the average value of the thickness of the internal electrode layer (electrode thickness) and its deviation σ, the electrode coverage, the number of electrode divisions, and the ceramic particle area ratio of the capacitor sample of Comparative Example 1 were obtained in the same manner as in Example 1. These results are shown in Table 1 or Table 2.
[0149] Comparative Examples 2 to 6
[0150] Capacitor samples were produced in the same manner as in Comparative Example 1, except that composite particles were not produced and the weight of barium titanate in the conductor paste was set to 7 parts by weight (7PHP), 9PHP, 11PHP, 13PHP, and 15PHP relative to 100 parts by weight of nickel particles. The inhibitor coverage of the inhibitor particles in the conductor paste used in each of Comparative Examples 2 to 6 on the surface of the conductive particles was measured in the same manner as in Comparative Example 1. The results are shown in Table 1.
[0151] In addition, Dsp50, Dsp99, the maximum diameter of ceramic particles, the number of ceramic particles, the average value of dielectric thickness and its deviation σ, the average value of the thickness of the internal electrode layer (electrode thickness) and its deviation σ, the electrode coverage, the number of electrode divisions, and the ceramic particle area ratio of the capacitor samples of each comparative example were obtained in the same manner as in comparative example 1. These results are shown in Table 1 or Table 2.
[0152] Rating 1
[0153] It can be confirmed that, compared with Comparative Examples 1 to 6, in Examples 1 to 6, the electrode continuity is excellent, and the electrode thickness deviation σ of the internal electrode layer and the dielectric thickness deviation σ of the dielectric layer are small and the thinning is excellent. In addition, according to the results shown in Tables 1 and 2, it can be confirmed that when Dsp50 is 40 or less, preferably 30 or less, the electrode coverage is improved, the number of electrode divisions is also reduced, the electrode continuity is improved, the thickness deviation σ is also reduced, and the thinning is excellent. In addition, it can be confirmed that when Dsp99 is 80 or less, preferably 73 or less, the electrode coverage is improved, the number of electrode divisions is also reduced, the electrode continuity is improved, the thickness deviation σ is also reduced, and the thinning is excellent.
[0154] It was confirmed that when the maximum particle size of the inner ceramic particles is 69 nm or less, more preferably 63 nm or less, the electrode continuity of the internal electrode layer is excellent, and the electrode thickness deviation σ of the internal electrode layer and the dielectric thickness deviation σ of the dielectric layer are small.
[0155] In addition, it can be confirmed that every 50 μm of the internal electrode layer 2 When the number of inner ceramic particles per area is 185 or less, more preferably 170 or less, for example, in the range of 55 to 166, the electrode continuity of the internal electrode layer is excellent, and the electrode thickness deviation σ of the internal electrode layer and the dielectric thickness deviation σ of the dielectric layer are small.
[0156] It can be confirmed that when the total area ratio of the inner ceramic particles is 2.5% or less, more preferably 2% or less, the electrode continuity of the internal electrode layer is excellent, and the electrode thickness deviation σ of the internal electrode layer and the dielectric thickness deviation σ of the dielectric layer are small.
[0157] [Table 1]
[0158]
[0159]
[0160] [Table 2]
[0161]
[0162] DESCRIPTION OF SYMBOLS 1 ...Multilayer ceramic capacitor 2 ...Ceramic layer (dielectric layer) 3 ...Internal electrode layer
[0163] 3a…Electrode part
[0164] 3b…Electrode discontinuity
[0165] 32…Composite particles
[0166] 34…Conductive particles
[0167] 36…Inhibitor particles
[0168] 36a...Inner ceramic particles 38...Imaginary circle
[0169] 4: External electrode 10: Ceramic body.
Claims
1. A laminated ceramic electronic component comprising ceramic layers and internal electrode layers laminated alternately, wherein: In the observation range of the cross section intersecting the internal electrode layer, The internal electrode layer contains a plurality of inner ceramic particles inside. Regarding the relative position of the inner ceramic grains in the inner electrode layer relative to the central position in the thickness direction of the inner electrode layer, let the relative position correspond to the relative position from the central position to the edge position and the relative position be represented by a number from 0 to 100 as Dsp, In the internal electrode layer, the area of the inner ceramic grains located in a region where Dsp is 40 or less accounts for 50% or more of the total area of the inner ceramic grains located in the observation range.
2. A laminated ceramic electronic component comprising ceramic layers and internal electrode layers laminated alternately, wherein: In the observation range of the cross section intersecting the internal electrode layer, The internal electrode layer contains a plurality of inner ceramic particles inside. Regarding the relative position of the inner ceramic grains in the inner electrode layer relative to the central position in the thickness direction of the inner electrode layer, let the relative position correspond to the relative position from the central position to the edge position and the relative position be represented by a number from 0 to 100 as Dsp, In the internal electrode layer, the area of the inner ceramic grains located in a region where Dsp is 75 or less accounts for 99% or more of the total area of the inner ceramic grains located in the observation range.
3. The multilayer ceramic electronic component according to claim 1 or 2, wherein: A ratio of the total area of the inner ceramic particles to the total area of the internal electrode layers located within the observation range is 2.5% or less.
4. The multilayer ceramic electronic component according to any one of claims 1 to 3, wherein The maximum particle size of the inner ceramic particles within the observation range is 69 nm or less.
5. The multilayer ceramic electronic component according to any one of claims 1 to 4, wherein Every 50 μm of the internal electrode layer within the observation range 2 The number of the inner ceramic particles per area is 185 or less.
Citation Information
Patent Citations
Conductive paste for forming internal electrode as well as laminated ceramic electronic parts
JP2001110233A