Dielectric paste, and method for manufacturing dielectric green sheet and ceramic capacitor

By using a combination of barium titanate-containing dielectric paste and polyalkylene glycol dibenzoate, the problem of peeling and cracking of ceramic capacitors during multi-layer lamination is solved and better interlayer adhesion is achieved and fracture strength, suitable for the manufacture of multilayer ceramic capacitors.

CN118742983APending Publication Date: 2024-10-01SANYO CHEM IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380020383.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-08
Filing Date
2023-02-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Ceramic capacitors are prone to peeling and cracking during the multi-layer lamination process. Existing plasticizers have poor deformability and are difficult to ensure interlayer adhesion.

Method used

A dielectric paste containing barium titanate is used, containing a binder resin and polyalkylene glycol dibenzoate as a plasticizer. The dielectric green sheet is formed through a coating and drying process, and is sintered after laminating the conductor coating. , forming a ceramic capacitor.

Benefits of technology

It effectively suppresses the peeling of dielectric green sheets inside ceramic capacitors, improves interlayer adhesion and fracture strength, and is suitable for multi-layer laminated ceramic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978892350000101
    Figure BDA0004978892350000101
  • Figure BDA0004978892350000111
    Figure BDA0004978892350000111
Patent Text Reader

Abstract

The present invention addresses the problem of providing a dielectric paste for realizing a dielectric green sheet that is not susceptible to structural defects such as peeling when laminated in a plurality of layers inside a ceramic capacitor. The problem is solved by a dielectric paste comprising a barium titanate-containing dielectric (A), a binder resin (B), and a plasticizer (C), wherein the dielectric (A) has a relative dielectric constant of 1000-2000 and the plasticizer (C) comprises a polyalkylene glycol dibenzoate (C1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a dielectric paste, a dielectric green sheet, and a method for producing a ceramic capacitor. Background Art

[0002] Conventionally, there have been restrictions on the use of alkyl phthalates used in the production of ceramic capacitors, and there has also been a demand for thinner ceramic layers of ceramic capacitors.

[0003] As for plasticizers that make the green sheet less likely to break during lamination and compression bonding even in the form of a thin film, dioctyl phthalate is known (Patent Document 1), and as for plasticizers for ceramic substrates, polypropylene glycol diester benzoate (Benzoflex 400) is known (Patent Document 2). However, if the green sheet is multilayered, the layer difference will become larger. In order to achieve tight adhesion, strong compression bonding is required, but existing plasticizers have the problem of poor deformability and easy rupture.

[0004] (Prior art literature)

[0005] Patent Document 1: Japanese Patent Publication No. 2019-197845

[0006] Patent Document 2: Japanese Patent Publication No. 2007-184247 Summary of the invention

[0007] (Problems to be solved by the invention)

[0008] One embodiment of the present invention has been made in view of the above-mentioned problems. An object of one embodiment of the present invention is to provide a dielectric paste for realizing a dielectric green sheet which is unlikely to cause structural defects such as peeling even when the dielectric green sheet is stacked in multiple layers inside a ceramic capacitor.

[0009] (Technical means to solve the problem)

[0010] The inventors of the present invention have conducted intensive research to achieve the above-mentioned purpose, and have completed the present invention as a result. That is, one embodiment of the present invention is a dielectric paste comprising a dielectric (A) containing barium titanate, a binder resin (B) and a plasticizer (C), wherein the relative dielectric constant of the dielectric (A) is 1000 to 2000, and the plasticizer (C) contains a polyalkylene glycol dibenzoate (C1).

[0011] Another aspect of the present invention is a method for producing a dielectric green sheet, comprising the steps of applying and drying the dielectric paste.

[0012] Another aspect of the present invention is a method for producing a ceramic capacitor, comprising the steps of laminating conductive coating green sheets formed by applying a conductive paste on the dielectric green sheets and sintering the laminated sheets.

[0013] (Effects of the Invention)

[0014] The dielectric green sheets produced using the dielectric paste according to one embodiment of the present invention are excellently prevented from peeling off when multiple layers are stacked in a ceramic capacitor. DETAILED DESCRIPTION

[0015] A dielectric paste according to one embodiment of the present invention is a dielectric paste for use in a dielectric green sheet for a multi-layered laminated ceramic component.

[0016] A dielectric paste according to one embodiment of the present invention includes: a dielectric (A) containing barium titanate particles; a binder resin (B); and a plasticizer (C).

[0017] The dielectric (A) containing barium titanate (hereinafter sometimes referred to as "dielectric (A)") according to one embodiment of the present invention is used to form a dielectric in a ceramic capacitor. In one embodiment of the present invention, the shape of the dielectric (A) can be particles, rods, etc., but particles are preferred from the viewpoint of the elongation at break of the dielectric green sheet. In addition, when the dielectric (A) is particles, the particle surface of the dielectric (A) containing barium titanate can be covered with at least one surface coating selected from Si compounds, titanium compounds, zirconium compounds, aluminum compounds, yttrium compounds, sulfur compounds and phosphoric acid compounds.

[0018] The relative dielectric constant of the dielectric (A) according to one embodiment of the present invention is 1000 to 2000. The relative dielectric constant of the dielectric (A) is preferably 1200 to 2000, and more preferably 1400 to 2000.

[0019] By setting the relative dielectric constant of the dielectric (A) to 1000 to 2000, it is possible to suppress an increase in the capacitance reduction rate of the obtained dielectric green sheet.

[0020] In addition, in this specification, the relative dielectric constant of the dielectric (A) is a value measured under the following conditions.

[0021] [Determination of relative dielectric constant]

[0022] 2.5 g of the dielectric (A) was mixed with 0.5 g of a 3 wt % aqueous solution of polyvinyl alcohol (Kuraray Poval 5-74LLA, manufactured by Kuraray Co., Ltd.) and the mixture was heated at 100 kg / cm 2The powder was pressed at a pressure of 25 mm to produce a disc-shaped pressed powder body with a diameter of 25 mm and a thickness of 2 mm. Since the pressed powder body contained water, it was placed in dry air at 50°C for 12 hours to adjust the pressed powder body to: the dielectric (A) accounted for 50% by volume, the polyvinyl alcohol accounted for 0.2% by volume, and the remainder was voids.

[0023] For the adjusted compressed powder, the dielectric constant at 10MHz was measured using an impedance analyzer E4991B and a dielectric constant measurement fixture 16453A manufactured by Agilent at room temperature 25°C and humidity 40% RH. The dielectric constant measurement results obtained by this operation include the results caused by the components of dielectric (A), polyvinyl alcohol and voids. Therefore, the logarithmic mixing law is used to calculate the results caused only by dielectric (A) based on the measured values, and the calculated results are used as the relative dielectric constant of dielectric (A).

[0024] From the viewpoint of suppressing peeling, the volume average particle size of the dielectric (A) is preferably 10 to 400 nm, more preferably 10 to 200 nm, and particularly preferably 50 to 200 nm.

[0025] In addition, in this specification, the volume average particle size of a dielectric (A) is a value measured under the following conditions.

[0026] [Measurement of volume average particle size]

[0027] A dispersion prepared by dispersing 0.5 wt % of the dielectric (A) in methyl ethyl ketone was used as a sample and measured using a dynamic light scattering particle size distribution analyzer "ELSZ-2000ZS" (manufactured by Otsuka Electronics Co., Ltd.).

[0028] The dielectric (A) may be a dielectric containing only barium titanate. In addition to barium titanate, it may also contain other components such as zirconate, calcium and strontium. The dielectric (A) may contain 0 to 20% by weight of the other components based on the weight of the dielectric (A).

[0029] The binder resin (B) according to one embodiment of the present invention includes polyvinyl butyral, polyacrylate, ethyl cellulose, and mixtures thereof. From the viewpoint of thin film formation, polyvinyl butyral or ethyl cellulose is preferred, polyvinyl butyral is more preferred, and polyvinyl butyral having a number average molecular weight of 10,000 to 60,000 is particularly preferred.

[0030] In the present specification, the number average molecular weight (may be abbreviated as Mn) of the binder resin (B) and the polyalkylene glycol dibenzoate (C1) described later is a value measured under the following conditions using gel permeation chromatography.

[0031] [Determination of number average molecular weight]

[0032] Device: "HLC-8120GPC" [TOSOH Co., Ltd.]

[0033] Column: "Guardcolumn HXL-H" (1 column), "TSKgel GMHXL" (2 columns) [both manufactured by TOSOH Corporation]

[0034] Sample solution: 0.25 wt% tetrahydrofuran solution

[0035] Solution injection volume: 100μL

[0036] Flow rate: 1mL / min

[0037] Measuring temperature: 40℃

[0038] Detection device: Refractive index detector

[0039] Reference material: Standard polystyrene

[0040] The plasticizer (C) according to one embodiment of the present invention contains a polyalkylene glycol dibenzoate (C1).

[0041] Examples of the polyalkylene glycol dibenzoate (C1) include: diethylene glycol dibenzoate, triethylene glycol dibenzoate, polyethylene glycol dibenzoate having a molecular weight of 400 or more, etc., which are polyalkylene glycol dibenzoates (polyethylene glycol dibenzoates) containing only an ethylene oxide chain; dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, polypropylene glycol dibenzoate having a molecular weight of 400 or more, etc., which are polyalkylene glycol dibenzoates (polypropylene glycol dibenzoates) containing only a propylene oxide chain; diesters formed from diols of random or block copolymers of ethylene oxide and propylene oxide and benzoic acid, etc., which are polyalkylene glycol dibenzoates containing ethylene oxide chains and propylene oxide chains; and the like.

[0042] Among them, from the viewpoint of thin film formation of the raw sheet, the polyalkylene glycol dibenzoate (C1) is preferably a polyalkylene glycol dibenzoate containing an ethylene oxide chain, more preferably a polyalkylene glycol dibenzoate containing an ethylene oxide chain having a number average molecular weight of 400 to 700, preferably polyethylene glycol dibenzoate having a number average molecular weight of 400 to 700, and further preferably polyethylene glycol dibenzoate having a number average molecular weight of 400 to 550.

[0043] The plasticizer (C) may contain a plasticizer other than the polyalkylene glycol dibenzoate (C1). Specific examples of the plasticizer other than the polyalkylene glycol dibenzoate (C1) include ethylene glycol dibenzoate, propylene glycol dibenzoate, and phthalic acid diesters.

[0044] From the viewpoint of adhesion when the green sheet is thinned, the content of the polyalkylene glycol dibenzoate (C1) is preferably 50 wt % or more, more preferably 80 wt % or more, particularly preferably 90 wt %, and most preferably 100 wt %, based on the weight of the plasticizer (C).

[0045] From the viewpoint of thinning the raw sheet, in the dielectric paste involved in one embodiment of the present invention, the content of the barium titanate-containing dielectric (A) is preferably 70 to 95% by weight, more preferably 80 to 95% by weight, and particularly preferably 80 to 90% by weight, based on the total weight of the barium titanate-containing dielectric (A), the binding resin (B) and the plasticizer (C).

[0046] From the viewpoint of thinning the raw sheet, in the dielectric paste involved in one embodiment of the present invention, the content of the binding resin (B) is preferably 4 to 20 wt %, more preferably 4 to 15 wt %, and particularly preferably 8 to 15 wt %, based on the total weight of the barium titanate-containing dielectric (A), the binding resin (B) and the plasticizer (C).

[0047] From the perspective of interlayer adhesion of the thin film of the raw sheet, in the dielectric paste involved in one embodiment of the present invention, based on the total weight of the barium titanate-containing dielectric (A), the adhesive resin (B) and the plasticizer (C), the content of the plasticizer (C) is preferably 1 to 10 weight %, more preferably 1 to 8 weight %, and particularly preferably 2 to 5 weight %.

[0048] Regarding the method for manufacturing the dielectric paste involved in one embodiment of the present invention, for example, there can be cited a method of pre-preparing the dielectric paste by placing various components in a mixing container and stirring them until they are uniform, and kneading them with a mixer such as a bead mill to obtain the dielectric paste. However, it is not limited to this method. In the kneading method, other kneading machines include a three-roller type, a vibration mill type, a high-speed rotary blade type mixer, a multi-axis rotary mixer, and other kneading machines with high shear force.

[0049] A method for producing a dielectric green sheet according to one embodiment of the present invention includes the step of applying the dielectric paste and drying it.

[0050] Specifically, first, a dielectric paste is applied to a support such as PET that has been subjected to a release treatment using a doctor blade, an extrusion coater, a wire rod coater, or a screen printer, a gravure printer, etc. Then, a volatile component is removed from the slurry composition on the support by a drying treatment to form a film, thereby obtaining a dielectric green sheet.

[0051] A method for manufacturing a ceramic capacitor according to an embodiment of the present invention comprises the steps of applying a conductor paste described below on the dielectric green sheets to obtain conductor-coated green sheets, laminating and pressing the conductor-coated green sheets, and then sintering them.

[0052] Specifically, a conductive paste to be an internal electrode is printed on a dielectric green sheet by screen printing, gravure printing, etc. and dried, and then the ceramic green sheet with electrodes is peeled off from the support. A plurality of ceramic green sheets with electrodes are stacked and heat-pressed to produce a laminate, and then the laminate is cut and ground into a predetermined shape to obtain a dielectric green chip. The obtained dielectric green chip is heat-treated to vaporize the solvent and the like, and to thermally decompose organic components such as the adhesive resin, and then the ceramic is sintered at a high temperature to obtain a laminated ceramic capacitor.

[0053] The conductive paste according to one embodiment of the present invention contains at least nickel particles (D) as a conductor, and preferably contains a dielectric (A) containing barium titanate, a binder resin (B), a plasticizer (C), and the like.

[0054] Examples of the barium titanate-containing dielectric (A), the binder resin (B), and the plasticizer (C) in the conductive paste include the same ones as those in the above-described dielectric paste.

[0055] Examples of the nickel particles (D) include nickel particles having a volume average particle size of 10 to 300 nm.

[0056] Nickel used for the nickel particles (D) includes nickel, nickel-tin alloys, nickel-silver alloys, etc. The particle surfaces of the nickel particles (D) may be covered with at least one selected from titanium oxide and barium compounds.

[0057] The conductive paste according to one embodiment of the present invention may contain, in addition to the dielectric (A) containing barium titanate, the binder resin (B), the plasticizer (C) and the nickel particles (D), a solvent capable of dissolving the binder resin (B) or the plasticizer (C). In addition, additives such as a dispersant and an antioxidant may be contained within the range that does not hinder the effect of the present invention.

[0058] Examples of the solvent include ethanol, toluene, and terpineol.

[0059] Examples of the dispersant, particularly those having a carboxyl group, include ether carboxylic acid surfactants and polycarboxylic acid amine salts.

[0060] Examples of the antioxidant include hindered amine antioxidants, hindered phenol antioxidants, phosphoric acid antioxidants and the like.

[0061] From the viewpoint of thinning the green sheet, the content of the dielectric (A) containing barium titanate in the conductive paste is preferably 1 to 10% by weight based on the weight of the conductive paste.

[0062] From the viewpoint of thinning, the content of the binder resin (B) in the conductive paste is preferably 4 to 20 wt %, more preferably 4 to 15 wt %, particularly preferably 8 to 15 wt %, based on the weight of the conductive paste.

[0063] From the viewpoint of interlayer adhesion when thinning, the content of the plasticizer (C) in the conductive paste is preferably 1 to 10 wt %, more preferably 1 to 8 wt %, and particularly preferably 2 to 5 wt %, based on the weight of the conductive paste.

[0064] From the viewpoint of thinning, the content of the nickel particles (D) in the conductor paste is preferably 69 to 79% by weight based on the weight of the conductor paste.

[0065] The method for producing a conductive paste according to one embodiment of the present invention is the same as the method for producing the dielectric paste except that nickel particles (D) are mixed.

[0066] <Others>

[0067] The present invention may include the following aspects.

[0068] <1>

[0069] A dielectric paste comprises a dielectric (A) containing barium titanate, an adhesive resin (B), and a plasticizer (C), wherein the relative dielectric constant of the dielectric (A) is 1000 to 2000, and the plasticizer (C) comprises polyalkylene glycol dibenzoate (C1).

[0070] <2>

[0071] according to <1> In the dielectric paste, the dielectric (A) containing barium titanate is in the form of particles, and the volume average particle size of the particles is 10 to 400 nm.

[0072] <3>

[0073] according to <1> or <2> In the dielectric paste, the adhesive resin (B) is a mixture of polyacrylate and ethyl cellulose or polyvinyl butyral.

[0074] <4>

[0075] according to <1> ~ <3> The dielectric paste described in any one of the above aspects, wherein the polyalkylene glycol dibenzoate (C1) has a number average molecular weight of 400 to 700.

[0076] <5>

[0077] according to <1> ~ <4> The dielectric paste described in any one of the above aspects, wherein the polyalkylene glycol dibenzoate (C1) is a polyalkylene glycol dibenzoate containing an ethylene oxide chain.

[0078] <6>

[0079] according to <1> ~ <5> The dielectric paste described in any one of the preceding claims, wherein, based on the total weight of the barium titanate-containing dielectric (A), the binding resin (B) and the plasticizer (C), the content of the barium titanate-containing dielectric (A) is 70 to 95% by weight, the content of the binding resin (B) is 4 to 20% by weight, and the content of the plasticizer (C) is 1 to 10% by weight.

[0080] <7>

[0081] A method for manufacturing a dielectric green sheet, comprising: <1> ~ <6> A step of applying and drying the dielectric paste described above.

[0082] <8>

[0083] A method for manufacturing a ceramic capacitor, comprising the following steps: <7> The conductor-coated green sheets are obtained by applying a conductor paste on the dielectric green sheets, and the conductor-coated green sheets are stacked and pressed, and then sintered.

[0084] [Example]

[0085] Hereinafter, the present invention will be further described by way of examples, but the present invention is not limited to these examples.

[0086] <Production Example 1>

[0087] 100 parts by weight of polyethylene glycol (PEG-1000, manufactured by Sanyo Chemical Industries, Ltd.), 20 parts by weight of benzoic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts by weight of diisopropoxytitanium terephthalate were mixed at 80° C., and then dehydrated at 80° C. under reduced pressure to obtain polyethylene glycol dibenzoate having a number average molecular weight of 1200.

[0088] <Production Example 2>

[0089] 85 parts by weight of butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), 5 parts by weight of methyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), 6 parts by weight of butyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), 2 parts by weight of hydroxyethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), 2 parts by weight of dimethylaminoethyl methacrylate, 0.02 parts by weight of V-65 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and 300 parts by weight of toluene were mixed under a nitrogen atmosphere, and then the solvent was distilled off to prepare a polyacrylate solution having a number average molecular weight of 10,000 (butyl methacrylate: methyl methacrylate: butyl acrylate: hydroxyethyl methacrylate: dimethylaminoethyl methacrylate = 85:5:6:2:2).

[0090] <Example 1>

[0091] <Preparation of Dielectric Paste>

[0092] A dielectric paste (Y-1) was prepared by stirring 80 parts by weight of barium titanate particles (10 nm barium titanate, manufactured by Toda Kogyo Co., Ltd.) having a volume average particle size of 10 nm as a dielectric (A), 15 parts by weight of polyvinyl butyral (BL-10, manufactured by Sekisui Chemical Co., Ltd.) having a number average molecular weight of 10,000 as a binder resin (B), 5 parts by weight of polyethylene glycol dibenzoate (EB-200, manufactured by Sanyo Chemical Industries, Ltd.) having a number average molecular weight of 400 as a plasticizer (C), 1 part by weight of an ether carboxylic acid surfactant (Viewlight LCA-25NH, manufactured by Sanyo Chemical Industries, Ltd.) as a dispersant, and 20 parts by weight of a toluene-ethanol mixed solution (toluene:ethanol=1:1 (weight ratio)) as a solvent using a bead mill for 3 hours.

[0093] <Production of Dielectric Green Sheet>

[0094] While the coating head was moved along the demolding PET sheet (thickness 50 μm), the dielectric paste (Y-1) was squeezed out from the coating head to apply a coating layer with a thickness of 60 μm, and then dried at 150°C for 30 minutes, thereby producing a dielectric green sheet (S-1) with a thickness of 50 μm.

[0095] <Examples 2 to 19 and Comparative Examples 1 to 3>

[0096] Dielectric pastes (Y-2) to (Y-19) and (RY-1) to (RY-3) were prepared in the same manner as in Example 1, except that the barium titanate-containing dielectric (A), adhesive resin (B), plasticizer (C) and dispersant described in Tables 1 and 2 were used.

[0097] Except for replacing the dielectric paste (Y-1) with dielectric pastes (Y-2) to (Y-19) and (RY-1) to (RY-3), the same method as Example 1 was followed to produce dielectric raw sheets (S-2) to (S-19) and (RS-1) to (RS-3) with a thickness of 50 μm.

[0098] The raw materials in Tables 1 and 2 are as follows.

[0099] Barium titanate particles with a volume average particle size of 5 nm (10 nm barium titanate, manufactured by Toda Industries, Ltd., relative dielectric constant 500)

[0100] Barium titanate particles with a volume average particle size of 10 nm (10 nm barium titanate, manufactured by Toda Industries, Ltd., relative dielectric constant 1000)

[0101] Barium titanate particles with a volume average particle size of 50 nm (10 nm barium titanate, manufactured by Toda Industries, Ltd., relative dielectric constant 1200)

[0102] Barium titanate particles with a volume average particle size of 100 nm (BT-HP9DX, manufactured by Kyoritsu Materials Co., Ltd., relative dielectric constant 1400)

[0103] Barium titanate particles with a volume average particle size of 200 nm (BT-HP9DX, manufactured by Kyoritsu Materials Co., Ltd., relative dielectric constant 2000)

[0104] Barium titanate particles with a volume average particle size of 400 nm (UQBT, manufactured by Fuji Titanium Industry Co., Ltd., relative dielectric constant 2000)

[0105] Barium titanate particles with a volume average particle size of 600 nm (HPBT, manufactured by Fuji Titanium Industry Co., Ltd., relative dielectric constant 2200)

[0106] Polyvinyl butyral with Mn 10000 (BL-10, manufactured by Sekisui Chemical Co., Ltd., relative dielectric constant 2000)

[0107] Polyvinyl butyral with Mn 60000 (BH-S, manufactured by Sekisui Chemical Co., Ltd.)

[0108] Ethyl cellulose (ETHOCEL STD-45 (Mw 140,000), manufactured by Dow Chemical Co., Ltd.)

[0109] Polyethylene glycol dibenzoate with Mn 400 (EB-200, manufactured by Sanyo Chemical Industries, Ltd.)

[0110] Polyethylene glycol dibenzoate with Mn 550 (EB-300, manufactured by Sanyo Chemical Industries, Ltd.)

[0111] Polyethylene glycol dibenzoate with Mn 700 (EB-400, manufactured by Sanyo Chemical Industries, Ltd.)

[0112] Dioctyl phthalate (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0113] Polypropylene glycol dibenzoate with Mn 550 (Benzoflex 400, manufactured by Eastman Co., Ltd.)

[0114] [Breaking Strength and Tensile Elongation of Dielectric Green Sheet]

[0115] The breaking strength and tensile elongation of the dielectric green sheets (S-1) to (S-19) and (RS-1) to (RS-3) were evaluated by the following methods. The results are shown in Table 1 or 2.

[0116] A test piece with a width of 5 mm and a length of 20 mm was cut, and a standard line was drawn on the test piece at intervals of 15 mm from the center along the long side direction using an automatic tracer measuring instrument ("AUTOGRAPH AGX-V" manufactured by Shimadzu Corporation). A clamp was clamped at the standard line, and the test piece was stretched at a tensile speed of 1 mm / min in an atmosphere of 25°C. The breaking strength and tensile elongation of the test piece at break were then calculated using the following formula.

[0117] Breaking strength (mPa) = tensile load value / cross-sectional area of ​​test piece

[0118] Tensile elongation (%) = 100 × (L-Lo) / Lo

[0119] Lo: Length of the test piece before the test

[0120] L: Length of the test piece when it breaks

[0121] [Table 1]

[0122]

[0123] [Table 2]

[0124]

[0125] <Preparation of Conductive Paste>

[0126] <Production Example 3>

[0127] Using a bead mill, 5 parts by weight of barium titanate particles with a volume average particle size of 10 nm as a dielectric (10 nm barium titanate, manufactured by Toda Industry Co., Ltd.), 75 parts by weight of nickel particles with a volume average particle size of 10 nm as a dielectric (i-nan S, manufactured by Nippon Steel Corporation), 15 parts by weight of polyvinyl butyral with a number average molecular weight of 10,000 as a binder resin (BL-10, manufactured by Sekisui Chemical Co., Ltd.), 5 parts by weight of polyethylene glycol dibenzoate with a number average molecular weight of 400 as a plasticizer (EB-200, manufactured by Sanyo Chemical Industries, Ltd.), 1 part by weight of an ether carboxylic acid surfactant as a dispersant (Viewlight LCA-25NH, manufactured by Sanyo Chemical Industries, Ltd.), and 20 parts by weight of pineneol (manufactured by Tokyo Chemical Industry Co., Ltd.) as a solvent were stirred for 3 hours to prepare a conductive paste (Z-1).

[0128] <Production of Ceramic Capacitors>

[0129] <Example 20>

[0130] While the coating head was moved along the de-patterned PET sheet (thickness 50 μm), the dielectric paste (Y-1) was squeezed out from the coating head to apply a coating layer with a thickness of 3.5 μm, and then dried at 150° C. for 30 minutes to prepare a dielectric green sheet with a thickness of 3 μm, which was then cut into a square of 1 cm×1 cm. Ten similar dielectric green sheets were prepared.

[0131] On the dielectric green sheet obtained, a conductor paste (Z-1) with a thickness of 1.5 μm was printed so that a 0.5 mm non-coated line appeared every 2 mm from the end of the green sheet, and a dielectric paste (Y-1) was printed on the margin to obtain a conductor-coated green sheet. Nine conductor-coated green sheets of the same type were produced.

[0132] Nine conductor-coated green sheets were stacked in the same direction, and then a dielectric green sheet was overlapped on the surface coated with the conductor and pressed. Then, a debonding resin treatment was performed at 500°C for 1 hour in a nitrogen atmosphere, and then sintered at 1200°C for 2 hours to obtain a ceramic laminate. A 50 μm thick copper paste for external electrodes (TCU-101G, manufactured by Daiken Chemical Industry Co., Ltd.) was applied to the mutually opposing surfaces of the obtained ceramic laminate, and sintered at 850°C for 1 hour in a nitrogen atmosphere to obtain a ceramic capacitor (W-1).

[0133] <Examples 21 to 38 and Comparative Examples 4 to 6>

[0134] Except for replacing the dielectric paste (Y-1) with dielectric pastes (Y-2) to (Y-19) and (RY-1) to (RY-3), the same method as in Example 20 was followed to produce ceramic capacitors (W-2) to (W-19) and (RW-1) to (RW-3).

[0135] [Check for peeling]

[0136] The fired laminate was cut to obtain a WT plane (cross section), and 1000 locations between ceramic layers were observed using a microscope to check for peeling. The number of peelings of 1 μm or more between ceramic layers was counted, and the results are shown in Table 3.

[0137] [Thermal shock test]

[0138] Thermal shock: The fired laminate was kept at -55°C for 30 minutes, then heated to 125°C with a high temperature recovery time of 5 minutes, kept at 125°C for 30 minutes, and then cooled to -55°C with a low temperature recovery time of 5 minutes, and then entered the next cycle. This series of operations was repeated 100 times. The electrostatic capacitance of the laminate before and after the thermal shock was measured using an LCR meter (IM3536, manufactured by Hioki Electric Co., Ltd.) under the conditions of 1MHz / 1Vrms, and the electrostatic capacitance reduction rate before and after (electrostatic capacitance after thermal shock / electrostatic capacitance before thermal shock) was evaluated.

[0139] [Table 3]

[0140] (Industrial Applicability)

[0141] The dielectric green sheet obtained by using the dielectric paste of the present invention has excellent breaking strength and breaking elongation, and the occurrence of peeling when stacked in multiple layers inside a ceramic capacitor is excellently suppressed. Furthermore, it is also suitable as a material for various inductors, ceramic package components, piezoelectric elements, etc.

Claims

1. A dielectric paste comprising: A dielectric (A) containing barium titanate; a binder resin (B); and Plasticizer (C), in, The dielectric (A) has a relative dielectric constant of 1000 to 2000, and the plasticizer (C) comprises polyalkylene glycol dibenzoate (C1).

2. The dielectric paste according to claim 1, in, The dielectric (A) containing barium titanate is in the form of particles, and the volume average particle size of the particles is 10 to 400 nm.

3. The dielectric paste according to claim 1, in, The adhesive resin (B) is a mixture of polyacrylate and ethyl cellulose or polyvinyl butyral.

4. The dielectric paste according to claim 1, in, The number average molecular weight of the polyalkylene glycol dibenzoate (C1) is 400-700.

5. The dielectric paste according to claim 1, in, The polyalkylene glycol dibenzoate (C1) is a polyalkylene glycol dibenzoate containing an ethylene oxide chain.

6. The dielectric paste according to claim 1, in, Based on the total weight of the barium titanate-containing dielectric (A), the binding resin (B) and the plasticizer (C), the content of the barium titanate-containing dielectric (A) is 70 to 95% by weight, the content of the binding resin (B) is 4 to 20% by weight, and the content of the plasticizer (C) is 1 to 10% by weight.

7. A method for manufacturing a dielectric green sheet, comprising: A step of applying and drying the dielectric paste according to any one of claims 1 to 6.

8. A method for manufacturing a ceramic capacitor, comprising the following steps: A conductor-coated green sheet is obtained by applying a conductor paste on the dielectric green sheet according to claim 7, and the conductor-coated green sheets are stacked and pressed, and then sintered.

9. The method for manufacturing a ceramic capacitor according to claim 8, in, The conductive paste contains nickel particles (D).

10. The method for manufacturing a ceramic capacitor according to claim 9, in, The conductive paste further includes the barium titanate-containing dielectric (A), the binder resin (B), and the plasticizer (C).