Bionic artificial blood vessel with anticoagulant inner layer and preparation method of bionic artificial blood vessel
By forming a uniformly distributed anticoagulant inner layer and enhanced adhesion solution in the artificial blood vessel, the problem of insufficient anticoagulation and anti-leakage of the artificial blood vessel is solved, effective thrombus inhibition and long-term anticoagulant effect are achieved, and the biocompatibility is improved. Tolerance and smoothness.
Patent Information
- Application Number
- CN202410716344.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-08
AI Technical Summary
Existing artificial blood vessels are prone to thrombosis after contact with blood, leading to insufficient anticoagulation, anastomotic intimal hyperplasia and re-obstruction, and the anticoagulant molecules are prone to loss and failure, and have insufficient anti-leakage properties.
Hydrophilic functional molecules with anticoagulant effect are added after cross-linking reaction to form an anticoagulant inner layer evenly distributed in the collagen matrix, and carboxymethyl cellulose is used to enhance the viscosity of the adhesion solution to achieve tight adhesion and Anti-liquid leakage.
Effectively inhibit thrombosis, prolong the anticoagulant effect, reduce the risk of acute thrombosis, improve the biocompatibility and anticoagulant properties of artificial blood vessels, and ensure the patency of the pipeline.
Smart Images

Figure CN118743787A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of artificial blood vessel preparation, and particularly relates to a bionic artificial blood vessel with an anticoagulant inner layer and a preparation method thereof. Background Art
[0002] When preparing artificial blood vessels, the anticoagulant properties of the product are particularly critical. When the anticoagulant properties are insufficient, the artificial blood vessel will be adsorbed and denatured by plasma proteins in a very short time after contact with blood, followed by the adhesion and aggregation of platelets and the formation of a fibrin network. Therefore, the inadequate anticoagulant properties of the artificial blood vessel often lead to problems such as anastomotic intimal hyperplasia and re-blockage, and then acute thrombosis occurs, resulting in transplant failure.
[0003] Some hydrophilic functional molecules with anticoagulant effects are widely used in the field of vascular tissue engineering. They exert anticoagulant effects through various anticoagulant mechanisms. For example, heparin, as a commonly used anticoagulant in clinical practice, exerts anticoagulant effects by inactivating the activity of coagulation factor II and coagulation factor X. It not only has excellent hydrophilicity and anticoagulant properties, but also contains multiple modifiable sites. It is often used as a surface modification molecule or carrier for the construction of artificial vascular stents, and plays the role of anticoagulation, promoting the growth of vascular endothelial cells, and protecting grafts. EDTA, its mechanism is to prevent blood coagulation by forming a stable chelate with calcium ions in the aqueous phase. Oxalate forms calcium oxalate precipitation with calcium ions in the blood through oxalate radicals, making it have no coagulation function. Hirudin has a small molecular weight, has stable anticoagulant factors, has different selective inhibitory effects on different types of thrombin, can more comprehensively inhibit the coagulation process, can covalently bind to the collagen fiber network, and improve the anticoagulant effect. Its excellent biocompatibility is widely used in the field of anticoagulant biomedical materials. However, some current methods of adding anticoagulant molecules to prepare artificial blood vessels have the problem of easy loss and failure of anticoagulant molecules, and there is also room for further improvement in the anti-leakage property of the prepared artificial blood vessels. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a bionic artificial blood vessel with an anticoagulant inner layer.
[0005] (1) Preparation of anticoagulant inner layer
[0006] After adding a crosslinking agent and a catalyst to a dispersion liquid with a collagen concentration of 7.5 to 9.5 mg / mL for crosslinking reaction, a hydrophilic functional molecule with anticoagulant effect is added thereto and stirred to react sufficiently to obtain a uniform composite solution, and the composite solution is naturally air-dried to be used as an anticoagulant inner layer;
[0007] (2) Preparation of the middle layer of artificial blood vessels
[0008] A cross-linking agent and a catalyst are added to a dispersion liquid with a collagen concentration of 5.5 to 7.5 mg / mL to carry out a cross-linking reaction, and the dispersion liquid is naturally air-dried to a non-flowing gel state, and then freeze-dried to obtain an artificial blood vessel middle layer with a dense porous structure;
[0009] (3) Preparation of the outer layer of artificial blood vessels
[0010] A cross-linking agent and a catalyst are added to a dispersion having a collagen concentration of 9.5 to 11.5 mg / mL to perform a cross-linking reaction, and the dispersion is naturally air-dried to form a dense outer layer of an artificial blood vessel;
[0011] (4) Assembly of artificial blood vessels
[0012] Carboxymethyl cellulose and collagen are mixed and dispersed as an adhesion solution. The anticoagulant inner layer obtained in step (1), the artificial blood vessel middle layer obtained in step (2), and the artificial blood vessel outer layer obtained in step (3) are all stacked in a rectangular shape in an alternating manner. The adhesion solution is applied to the contact surface between the anticoagulant inner layer and the artificial blood vessel middle layer and the contact surface between the artificial blood vessel middle layer and the artificial blood vessel outer layer, respectively, and the surfaces are naturally air-dried to achieve tight adhesion to form a two-dimensional plane body. The two-dimensional plane body is wound on the catheter in a state where the edge of the anticoagulant inner layer on the two-dimensional plane body away from the artificial blood vessel middle layer is parallel to the axial direction of the catheter. During the winding process, the adhesion solution is applied between each winding layer. After the winding is completed, the surfaces are naturally air-dried to achieve tight adhesion between each winding layer, and then the catheter is pulled out to leave the artificial blood vessel.
[0013] Preferably, the dispersion is formed by fully dissolving the crushed collagen sponge in an aqueous glacial acetic acid solution, wherein the solute concentration of the aqueous glacial acetic acid solution is 0.5 mol / L.
[0014] Preferably, the crosslinking agent is dicarbodiimide (EDC) and the catalyst is N-hydroxysuccinimide (NHS), and catalytic crosslinking forms amide bonds between the carboxyl and amino groups of the collagen molecules to increase the tension and stability of the collagen fibers; before being added to each dispersion, the crosslinking agent and the catalyst are first dispersed in deionized water at a concentration of 15 mg / mL, respectively, the mass ratio of the added crosslinking agent to the collagen in each dispersion is 1:5.5-7, and the mass ratio of the crosslinking agent to the catalyst is 0.8-1.5:0.8-1.2; after adding the crosslinking agent and the catalyst to each dispersion, magnetic stirring is performed at 4°C at a stirring speed of 200-800 r / min for 24 hours to achieve a crosslinking reaction.
[0015] Preferably, in step (1), after the dispersion undergoes cross-linking reaction, it is mixed with a solution prepared from hydrophilic functional molecules having an anticoagulant effect at a volume ratio of 8 to 10:1.
[0016] Preferably, in step (1), the hydrophilic functional molecule having an anticoagulant effect is one or a combination of heparin sodium, low molecular weight heparin, EDTA, oxalate, citrate, hirudin, warfarin, phosphorylcholine, and betaine.
[0017] Preferably, in step (1), 60 mL to 100 mL of the composite solution is poured into a square dish with a size of 10 cm×10 cm×1.2 cm and naturally air-dried; in step (3), 60 mL to 100 mL of the dispersion after the cross-linking reaction is poured into a square dish with a size of 10 cm×10 cm×1.2 cm and naturally air-dried.
[0018] Preferably, in step (2), 60 mL to 100 mL of the dispersion after the cross-linking reaction is poured into a square dish with a specification of 10 cm×10 cm×1.2 cm and naturally air-dried to a non-flowing gel state. At this time, the upper surface of the dispersion in the square dish is 1 to 2 mm above the bottom, and 80% to 90% of the water in the dispersion has evaporated. At this time, the dispersion is transferred to an ultra-low temperature refrigerator and frozen at -80°C for 12 hours, and then transferred to a freeze dryer for freeze drying for 8 hours.
[0019] Preferably, in step (4), the adhesion solution is prepared by dispersing carboxymethyl cellulose at a mass fraction of 1% to 2% in water at 18 to 25°C and stirring the solution until it becomes transparent and viscous, then adding collagen at a concentration of 5.5 to 7.5 mg / mL and mixing the mixture for 6 to 12 hours.
[0020] Preferably, in step (4), the outer diameter of the catheter is 3 to 10 mm, and the curling length of the anticoagulant inner layer on the two-dimensional plane is equal to the circumference of the outer diameter of the catheter, that is, it is exactly wrapped around the catheter for one circle, the artificial blood vessel middle layer on the two-dimensional plane is exactly wrapped around the anticoagulant inner layer after winding, and the artificial blood vessel outer layer on the two-dimensional plane is exactly wrapped around the artificial blood vessel middle layer after winding.
[0021] This solution also provides a bionic artificial blood vessel with an anticoagulant inner layer obtained based on the above preparation method.
[0022] The beneficial effects of the present invention are as follows: hydrophilic functional molecules with anticoagulant effect are introduced into the artificial blood vessel through chemical bonds, thereby obtaining a dense inner layer with the function of inhibiting thrombosis, placing it in direct contact with the blood, and effectively exerting its anticoagulant properties; and the anticoagulant molecules are slowly released during the gradual degradation and replacement of the inner collagen matrix (the blood circulating in the blood vessels contains various enzymes, which cause the collagen to be degraded by the enzymes, and the side chains to be hydrolyzed and broken, that is, the covalent bonds connecting the anticoagulant molecules are broken, and the anticoagulant molecules are released. While the artificial blood vessels are degraded, they are replaced by new tissues grown and proliferated based on endothelial cells, smooth muscle cells, etc.), thereby achieving a long-term anticoagulant effect and reducing the risk of acute thrombosis in vascular grafts; the grafting of anticoagulant functional molecules can also further improve the blood compatibility of artificial blood vessel materials and ensure the patency of the artificial blood vessel pipeline, thereby obtaining a bionic artificial blood vessel with excellent biocompatibility and anticoagulant properties, which has broad application prospects.
[0023] This scheme creatively evenly disperses and grafts the anticoagulant functional molecules into the inner layer collagen matrix that has formed a cross-linked connection: this scheme takes into account the fact that the collagen molecules still have good flow dispersibility after catalytic cross-linking. After the inner layer collagen molecules are cross-linked, the anticoagulant molecules are evenly mixed into the inner layer and further air-dried and solidified (the functional groups remaining after the cross-linking reaction on the inner layer collagen matrix form chemical connections such as amide bonds with the anticoagulant molecules, making the dispersion and binding of the anticoagulant molecules in the inner layer more stable). Compared with centrally grafting the anticoagulant functional materials on the surface of the inner wall of the artificial blood vessel, the grafting method of this scheme effectively avoids the problem that the blood in the artificial blood vessel will quickly dissolve the anticoagulant material on the inner wall of the blood vessel, resulting in the anticoagulant effect failing too quickly, and improves the tightness and stability of the anticoagulant molecules in the artificial blood vessel; and compared with mixing the anticoagulant molecules with the collagen molecules first and then cross-linking them together, this scheme effectively avoids the problem that the anticoagulant molecules participate in the cross-linking to a large extent and are too tightly wrapped by the cross-linked collagen matrix and are not easy to be released.
[0024] In addition to having ideal viscosity, the adhesion solution of this scheme further improves the liquid leakage resistance through the introduction of carboxymethyl cellulose, thereby more effectively eliminating the risk of artificial blood vessel leakage (which may cause internal bleeding under the human skin). BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A schematic diagram of the radial cross-interface layer structure of the artificial blood vessel prepared by the present invention;
[0026] Figure 2 This is a schematic diagram of the operation of winding the two-dimensional plane formed by adhesion layer by layer on the catheter to make an artificial blood vessel in the present invention.
[0027] Among them, 100—artificial blood vessels, 10—anticoagulant inner layer, 20—artificial blood vessel middle layer, 30—artificial blood vessel outer layer, and 50—plastic catheter. DETAILED DESCRIPTION
[0028] The vascular wall of the artificial blood vessel 100 of the present invention is a three-layer structure, which includes an anticoagulant inner layer 10, an artificial blood vessel middle layer 20, and an artificial blood vessel outer layer 30 from the inside to the outside. Figure 1 The artificial blood vessel 100 of the layer structure is prepared by the following operations:
[0029] (1) Preparation of anticoagulant inner layer
[0030] According to the mass ratio of cross-linking agent to collagen of 1:5.5-7 and the mass ratio of cross-linking agent to catalyst of 0.8-1.5:0.8-1.2, a dispersion with a collagen concentration of 7.5-9.5 mg / mL is formed by crushing collagen sponge and fully dissolving it in an aqueous glacial acetic acid solution (solute concentration of 0.5 mol / L), and then a 15 mg / mL cross-linking agent carbodiimide (EDC) aqueous solution and a 15 mg / mL catalyst N-hydroxysuccinimide (NHS) aqueous solution are added, and then magnetic stirring is carried out at a stirring speed of 200-800 r / min at 4°C for 24 hours to achieve a cross-linking reaction, and then a hydrophilic functional molecule with an anticoagulant effect is added thereto and stirred for sufficient reaction to obtain a uniform composite solution, and 60 mL-100 mL of the composite solution is poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to form an anticoagulant inner layer;
[0031] The hydrophilic functional molecule with anticoagulant effect is one or a combination of heparin sodium, low molecular weight heparin, EDTA, oxalate, citrate, hirudin, warfarin, phosphorylcholine, betaine. When added, the cross-linking system and the solution prepared by the hydrophilic functional molecule with anticoagulant effect are mixed in a volume ratio of 8 to 10:1.
[0032] (2) Preparation of the middle layer of artificial blood vessels
[0033] According to the mass ratio of cross-linking agent to collagen of 1:5.5-7 and the mass ratio of cross-linking agent to catalyst of 0.8-1.5:0.8-1.2, a dispersion of 5.5-7.5 mg / mL of collagen prepared by crushing collagen sponge and fully dissolving it in an aqueous solution of glacial acetic acid (solute concentration of 0.5 mol / L) was added with a 15 mg / mL aqueous solution of cross-linking agent carbodiimide (EDC) and a 15 mg / mL aqueous solution of catalyst N-hydroxysuccinimide (NHS), and the mixture was stirred at 200-800 r / min at 4°C. After magnetic stirring for 24 hours at a stirring speed of 10000 g to achieve a cross-linking reaction, 60 mL to 100 mL of the dispersion after the cross-linking reaction was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to a non-flowing gel state. At this time, the height of the upper surface of the dispersion in the square dish from the bottom was 1 to 2 mm, and 80% to 90% of the water in the dispersion evaporated. At this time, the dispersion was transferred to an ultra-low temperature refrigerator and frozen at -80°C for 12 hours, and then transferred to a freeze dryer for freeze drying for 8 hours to obtain an artificial blood vessel middle layer with a dense porous structure;
[0034] (3) Preparation of the outer layer of artificial blood vessels
[0035] According to the mass ratio of the cross-linking agent to the collagen being 1:5.5-7 and the mass ratio of the cross-linking agent to the catalyst being 0.8-1.5:0.8-1.2, a dispersion having a collagen concentration of 9.5-11.5 mg / mL is added to a dispersion having a collagen concentration of 15 mg / mL of an aqueous solution of cross-linking agent carbodiimide (EDC) and a dispersion having a catalyst concentration of 15 mg / mL, wherein the dispersion is fully dissolved in an aqueous solution of glacial acetic acid (solute concentration of 0.5 mol / L) after the collagen sponge is crushed, and then the mixture is magnetically stirred at a stirring speed of 200-800 r / min for 24 hours at 4°C to achieve a cross-linking reaction, and 60 mL-100 mL of the dispersion having undergone the cross-linking reaction is poured into a square dish having a specification of 10 cm×10 cm×1.2 cm and naturally air-dried to form a dense outer layer of an artificial blood vessel;
[0036] (4) Assembly of artificial blood vessels
[0037] Disperse carboxymethyl cellulose at a mass fraction of 1% to 2% in water at 18 to 25°C and stir until it becomes transparent and viscous, then add collagen at a concentration of 5.5 to 7.5 mg / mL and mix and stir for 6 to 12 hours to prepare an adhesion solution, lay the anticoagulant inner layer obtained in step (1), the artificial blood vessel middle layer obtained in step (2), and the artificial blood vessel outer layer obtained in step (3) in a rectangular shape, alternately and flatly stack them in sequence, and apply the adhesion solution on the contact surface between the anticoagulant inner layer and the artificial blood vessel middle layer and the contact surface between the artificial blood vessel middle layer and the artificial blood vessel outer layer, and dry them naturally to achieve tight adhesion, and then prepare a two-dimensional plane body with a two-dimensional structure. When the edge of the anticoagulant inner layer on the two-dimensional plane body away from the middle layer of the artificial blood vessel is parallel to the axial direction of the catheter with an outer diameter of 3 to 10 mm, the two-dimensional plane body is wound on the catheter, and the curling length of the anticoagulant inner layer on the two-dimensional plane body is equal to the circumference of the outer diameter of the catheter, that is, it is just wound around the catheter for one circle, the artificial blood vessel middle layer on the two-dimensional plane body is just wound around the anticoagulant inner layer after winding, and the artificial blood vessel outer layer on the two-dimensional plane body is just wound around the artificial blood vessel middle layer after winding. During the winding process, an adhesion solution is applied between each winding layer. After the winding is completed, it is naturally dried to achieve close adhesion between the winding layers, and then the catheter is pulled out to leave the artificial blood vessel.
[0038] Example 1
[0039] (1) Preparation of anticoagulant inner layer
[0040] A collagen sponge made of New Zealand beef tendon was crushed into 40 meshes and dispersed in a 0.5 mol / L glacial acetic acid aqueous solution at a concentration of 8 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6, and then incubated at 4°C. The cross-linking reaction was completed by magnetic stirring at a stirring speed of 300 r / min for 24 hours; a sodium heparin aqueous solution with a concentration of 1 mg / mL was prepared using PBS buffer (pH=7.4) as a solvent, and the collagen dispersion that completed the cross-linking reaction and the sodium heparin aqueous solution were mixed at a volume ratio of 10:1 to obtain a uniform composite solution, and 80 mL of the composite solution was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to fully form a film as an anticoagulant inner layer;
[0041] (2) Preparation of the middle layer of artificial blood vessels
[0042] A collagen sponge made of New Zealand beef tendon was crushed to 40 meshes and dispersed in a 0.5 mol / L glacial acetic acid aqueous solution at a concentration of 6 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6.5, and the mixture was incubated at 300 r / mi at 4°C. n stirring speed and magnetic stirring for 24 h to complete the cross-linking reaction; pouring 100 mL of the collagen dispersion after the cross-linking reaction into a square dish with a specification of 10 cm×10 cm×1.2 cm, and naturally air-drying until the collagen dispersion in the square dish is in a non-flowing gel state (at this time, the height of the upper surface of the collagen dispersion in the square dish from the bottom is 1 mm), transferring it to an ultra-low temperature refrigerator at -80°C and freezing it for 12 h, and then transferring it to a freeze dryer and freeze-drying it for 8 h to obtain an artificial blood vessel middle layer with a dense porous structure;
[0043] (3) Preparation of the outer layer of artificial blood vessels
[0044] A collagen sponge made of New Zealand beef tendon was crushed into 40 meshes, and then dispersed in an aqueous glacial acetic acid solution with a solute concentration of 0.5 mol / L at a concentration of 10 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:7, and then magnetically stirred at 480 r / min at 4°C for 24 hours to complete the cross-linking reaction; 120 mL of the collagen dispersion after the cross-linking reaction was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to form a dense outer layer of the artificial blood vessel;
[0045] (4) Assembly of artificial blood vessels
[0046] Dispersing carboxymethyl cellulose at a mass fraction of 1% in deionized water at 20° C. and stirring until transparent and viscous, adding collagen made from New Zealand beef tendon at a concentration of 6 mg / mL, and blending and stirring for 8 hours to obtain an adhesion solution;
[0047] The anticoagulant inner layer obtained in step (1) and the artificial blood vessel middle layer obtained in step (2) are cut into rectangular films of 8 cm × 1.9 cm, and the artificial blood vessel outer layer obtained in step (3) is cut into rectangular films of 8 cm × 2.3 cm. Figure 2The outer layer of the artificial blood vessel obtained by cutting was laid flat with its 8 cm side as the side, and the left half of the bottom surface of the middle layer of the artificial blood vessel obtained by cutting was contacted with the surface and the adhesion solution (0.25 L / m 2 ), and then the anticoagulant inner layer obtained by cutting was laid flat with its 8 cm edge as the side edge, which was in surface contact with the right half of the top surface of the flattened artificial blood vessel middle layer, and the above-mentioned adhesion solution (0.25 L / m 2 ), and after natural air drying, a two-dimensional plane body is obtained; in a state where the side of the anticoagulant inner layer on the two-dimensional plane body that is 8 cm away from the middle layer of the artificial blood vessel is parallel to the axial direction of the catheter, the two-dimensional plane body is wound on a plastic catheter 50 with an outer diameter (diameter) of 6 mm. During the winding process, the above-mentioned adhesion solution (0.25 L / m 2 ), after the winding is completed and the artificial blood vessel is left, the plastic catheter is removed after it is naturally dried. Figure 1 .
[0048] Example 2
[0049] (1) Preparation of anticoagulant inner layer
[0050] A collagen sponge made of New Zealand beef tendon was crushed into 40 meshes and dispersed in a 0.5 mol / L glacial acetic acid aqueous solution at a concentration of 7.5 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6.5. The mixture was stirred for 4 hours. ℃ and 420r / min stirring speed for 24h to complete the cross-linking reaction; using physiological saline as solvent to prepare 10mg / mL EDTA-2Na aqueous solution, the collagen dispersion that has completed the cross-linking reaction and the EDTA-2Na aqueous solution are mixed in a volume ratio of 8:1 to form a uniform composite solution, and 75mL of the composite solution is poured into a square dish with a specification of 10cm×10cm×1.2cm for natural air drying to form a film as an anticoagulant inner layer;
[0051] (2) Preparation of the middle layer of artificial blood vessels
[0052] A collagen sponge made of New Zealand beef tendon was crushed to 40 meshes and dispersed in a 0.5 mol / L glacial acetic acid aqueous solution at a concentration of 5.5 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6, and the mixture was stirred at 420 r / min at 4°C. The cross-linking reaction was completed by magnetic stirring at a stirring speed of 1000 μl for 24 h; 110 mL of the cross-linked collagen dispersion was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm, and naturally air-dried until the collagen dispersion in the square dish was in a non-flowing gel state (at this time, the height of the upper surface of the collagen dispersion in the square dish from the bottom was 1.5 mm), and then transferred to an ultra-low temperature refrigerator at -80°C for freezing for 12 h, and then transferred to a freeze dryer for freeze drying for 8 h to obtain an artificial blood vessel middle layer with a dense porous structure;
[0053] (3) Preparation of the outer layer of artificial blood vessels
[0054] A collagen sponge made of New Zealand beef tendon was crushed into 40 meshes, and then dispersed in an aqueous glacial acetic acid solution with a solute concentration of 0.5 mol / L at a concentration of 9.5 mg / mL as a collagen dispersion. A 15 mg / mL EDC aqueous solution and a 15 mg / mL NHS aqueous solution were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6, and then magnetically stirred at 480 r / min at 4°C for 24 hours to complete the cross-linking reaction; 110 mL of the collagen dispersion after the cross-linking reaction was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to form a dense outer layer of the artificial blood vessel;
[0055] (4) Assembly of artificial blood vessels
[0056] Dispersing carboxymethyl cellulose at a mass fraction of 1.5% in deionized water at 23° C. and stirring until transparent and viscous, adding collagen made from New Zealand beef tendon at a concentration of 5.5 mg / mL, and blending and stirring for 12 hours to obtain an adhesion solution;
[0057] The anticoagulant inner layer obtained in step (1) and the artificial blood vessel middle layer obtained in step (2) are cut into rectangular films of 6 cm × 3.2 cm, and the artificial blood vessel outer layer obtained in step (3) is cut into rectangular films of 6 cm × 4.2 cm. Figure 2The outer layer of the artificial blood vessel obtained by cutting was laid flat with its 6 cm side as the side, and the left half of the bottom surface of the middle layer of the artificial blood vessel obtained by cutting was contacted with the surface and the adhesion solution (0.25 L / m 2 ), and then the anticoagulant inner layer obtained by cutting was laid flat with its 6 cm edge as the side edge, which was in surface contact with the right half of the top surface of the flattened artificial blood vessel middle layer, and the above-mentioned adhesion solution (0.25 L / m 2 ), and after natural air drying, a two-dimensional plane body is obtained; in a state where the side of the anticoagulant inner layer on the two-dimensional plane body that is 6 cm away from the middle layer of the artificial blood vessel is parallel to the axial direction of the catheter, the two-dimensional plane body is wound on a plastic catheter 50 with an outer diameter (diameter) of 10 mm. During the winding process, the above-mentioned adhesion solution (0.25 L / m 2 ), after the winding is completed and the artificial blood vessel is left, the plastic catheter is removed after it is naturally dried. Figure 1 .
[0058] Comparative Example 1
[0059] Before the collagen dispersion in step (1) undergoes cross-linking reaction, heparin sodium is added thereto, and the remaining operations are the same as those in Example 1:
[0060] (1) Preparation of anticoagulant inner layer
[0061] The collagen sponge made of New Zealand beef tendon was crushed into 40 meshes and dispersed in an aqueous solution of 0.5 mol / L glacial acetic acid at a concentration of 8 mg / mL as a collagen dispersion. A sodium heparin aqueous solution with a concentration of 1 mg / mL was prepared using PBS buffer (pH = 7.4) as a solvent. EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6 by mass ratio was added to the collagen dispersion. After adding 15 mg / mL of EDC aqueous solution and 15 mg / mL of NHS aqueous solution, the collagen dispersion with EDC and NHS added was fully mixed with the above-mentioned sodium heparin aqueous solution at a volume ratio of 10:1, and magnetically stirred at a stirring speed of 300 r / min at 4°C for 24 hours to complete the cross-linking reaction; 80 mL of the above-mentioned cross-linked solution system was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to fully form a film as an anticoagulant inner layer;
[0062] (2) Preparation of the middle layer of artificial blood vessels
[0063] A collagen sponge made of New Zealand beef tendon was crushed to 40 meshes and dispersed in a 0.5 mol / L glacial acetic acid aqueous solution at a concentration of 6 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6.5, and the mixture was incubated at 300 r / mi at 4°C. n stirring speed and magnetic stirring for 24 h to complete the cross-linking reaction; pouring 100 mL of the collagen dispersion after the cross-linking reaction into a square dish with a specification of 10 cm×10 cm×1.2 cm, and naturally air-drying until the collagen dispersion in the square dish is in a non-flowing gel state (at this time, the height of the upper surface of the collagen dispersion in the square dish from the bottom is 1 mm), transferring it to an ultra-low temperature refrigerator at -80°C and freezing it for 12 h, and then transferring it to a freeze dryer and freeze-drying it for 8 h to obtain an artificial blood vessel middle layer with a dense porous structure;
[0064] (3) Preparation of the outer layer of artificial blood vessels
[0065] A collagen sponge made of New Zealand beef tendon was crushed into 40 meshes, and then dispersed in an aqueous glacial acetic acid solution with a solute concentration of 0.5 mol / L at a concentration of 10 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:7, and then magnetically stirred at 480 r / min at 4°C for 24 hours to complete the cross-linking reaction; 120 mL of the collagen dispersion after the cross-linking reaction was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to form a dense outer layer of the artificial blood vessel;
[0066] (4) Assembly of artificial blood vessels
[0067] Dispersing carboxymethyl cellulose at a mass fraction of 1% in deionized water at 20° C. and stirring until transparent and viscous, adding collagen made from New Zealand beef tendon at a concentration of 6 mg / mL, and blending and stirring for 8 hours to obtain an adhesion solution;
[0068] The anticoagulant inner layer obtained in step (1) and the artificial blood vessel middle layer obtained in step (2) are cut into rectangular films of 8 cm × 1.9 cm, and the artificial blood vessel outer layer obtained in step (3) is cut into rectangular films of 8 cm × 2.3 cm. Figure 2The outer layer of the artificial blood vessel obtained by cutting was laid flat with its 8 cm side as the side, and the left half of the bottom surface of the middle layer of the artificial blood vessel obtained by cutting was contacted with the surface and the adhesion solution (0.25 L / m 2 ), and then the anticoagulant inner layer obtained by cutting was laid flat with its 8 cm edge as the side edge, which was in surface contact with the right half of the top surface of the flattened artificial blood vessel middle layer, and the above-mentioned adhesion solution (0.25 L / m 2 ), and after natural air drying, a two-dimensional plane body is obtained; in a state where the side of the anticoagulant inner layer on the two-dimensional plane body that is 8 cm away from the middle layer of the artificial blood vessel is parallel to the axial direction of the catheter, the two-dimensional plane body is wound on a plastic catheter 50 with an outer diameter (diameter) of 6 mm. During the winding process, the above-mentioned adhesion solution (0.25 L / m 2 ), after the winding is completed and the artificial blood vessel is left, the plastic catheter is removed after it is naturally dried. Figure 1 .
[0069] Comparative Example 2
[0070] In the adhesion solution, "collagen" of equal concentration was used instead of "carboxymethyl cellulose", and the rest of the operations were the same as in Example 1:
[0071] (1) Preparation of anticoagulant inner layer
[0072] A collagen sponge made of New Zealand beef tendon was crushed into 40 meshes and dispersed in a 0.5 mol / L glacial acetic acid aqueous solution at a concentration of 8 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6, and then incubated at 4°C. The cross-linking reaction was completed by magnetic stirring at a stirring speed of 300 r / min for 24 hours; a sodium heparin aqueous solution with a concentration of 1 mg / mL was prepared using PBS buffer (pH=7.4) as a solvent, and the collagen dispersion that completed the cross-linking reaction and the sodium heparin aqueous solution were mixed at a volume ratio of 10:1 to obtain a uniform composite solution, and 80 mL of the composite solution was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to fully form a film as an anticoagulant inner layer;
[0073] (2) Preparation of the middle layer of artificial blood vessels
[0074] A collagen sponge made of New Zealand beef tendon was crushed to 40 meshes and dispersed in a 0.5 mol / L glacial acetic acid aqueous solution at a concentration of 6 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:6.5, and the mixture was incubated at 300 r / mi at 4°C. n stirring speed and magnetic stirring for 24 h to complete the cross-linking reaction; pouring 100 mL of the collagen dispersion after the cross-linking reaction into a square dish with a specification of 10 cm×10 cm×1.2 cm, and naturally air-drying until the collagen dispersion in the square dish is in a non-flowing gel state (at this time, the height of the upper surface of the collagen dispersion in the square dish from the bottom is 1 mm), transferring it to an ultra-low temperature refrigerator at -80°C and freezing it for 12 h, and then transferring it to a freeze dryer and freeze-drying it for 8 h to obtain an artificial blood vessel middle layer with a dense porous structure;
[0075] (3) Preparation of the outer layer of artificial blood vessels
[0076] A collagen sponge made of New Zealand beef tendon was crushed into 40 meshes, and then dispersed in an aqueous glacial acetic acid solution with a solute concentration of 0.5 mol / L at a concentration of 10 mg / mL as a collagen dispersion. A 15 mg / mL aqueous solution of EDC and a 15 mg / mL aqueous solution of NHS were added to the collagen dispersion at a mass ratio of EDC: N-hydroxysuccinimide (NHS): collagen (in the collagen dispersion) = 1:1:7, and then magnetically stirred at 480 r / min at 4°C for 24 hours to complete the cross-linking reaction; 120 mL of the collagen dispersion after the cross-linking reaction was poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying to form a dense outer layer of the artificial blood vessel;
[0077] (4) Assembly of artificial blood vessels
[0078] Collagen made from New Zealand beef tendon was dispersed in deionized water at 20°C at a mass fraction of 1.6% and stirred until transparent and viscous to prepare an adhesion solution;
[0079] The anticoagulant inner layer obtained in step (1) and the artificial blood vessel middle layer obtained in step (2) are cut into rectangular films of 8 cm × 1.9 cm, and the artificial blood vessel outer layer obtained in step (3) is cut into rectangular films of 8 cm × 2.3 cm. Figure 2The outer layer of the artificial blood vessel obtained by cutting was laid flat with its 8 cm side as the side, and the left half of the bottom surface of the middle layer of the artificial blood vessel obtained by cutting was contacted with the surface and the adhesion solution (0.25 L / m 2 ), and then the anticoagulant inner layer obtained by cutting was laid flat with its 8 cm edge as the side edge, which was in surface contact with the right half of the top surface of the flattened artificial blood vessel middle layer, and the above-mentioned adhesion solution (0.25 L / m 2 ), and after natural air drying, a two-dimensional plane body is obtained; in a state where the side of the anticoagulant inner layer on the two-dimensional plane body that is 8 cm away from the middle layer of the artificial blood vessel is parallel to the axial direction of the catheter, the two-dimensional plane body is wound on a plastic catheter 50 with an outer diameter (diameter) of 6 mm. During the winding process, the above-mentioned adhesion solution (0.25 L / m 2 ), after the winding is completed and the artificial blood vessel is left, the plastic catheter is removed after it is naturally dried. Figure 1 .
[0080] Anticoagulant molecule sustained release experiment:
[0081] The anticoagulant inner layer obtained in step (1) of the above-mentioned Example 1, the anticoagulant inner layer obtained in step (1) of Example 2, and the anticoagulant inner layer obtained in step (1) of Comparative Example 1 were immersed in PBS buffer solution (pH=7.4) at a ratio of 1 g / 15 mL, and placed in an incubator at 37° C. for standing. At each time point of the 1st, 2nd, 5th, 7th, 9th, 11th, 13th, 17th, 19th, 21st, 25th and 28th day, 3 mL of supernatant was taken from the immersion solution of each anticoagulant inner layer sample, and the absorbance value (A2) of the anticoagulant molecule therein at a specific ultraviolet absorption wavelength (the ultraviolet absorption wavelength of heparin sodium is 260 nm (heparin sodium needs to add the color developer Azure A), and the ultraviolet absorption wavelength of EDTA-2Na is 240 nm) was detected by UV3802 ultraviolet-visible spectrophotometer. After the test, the supernatant was poured back into the original immersion solution (the operation was repeated three times for the immersion solution of each anticoagulant inner layer sample, and the average was taken). According to the absorbance value A2 measured above, the corresponding concentration of the anticoagulant molecule in the immersion solution is calculated, and finally the cumulative release rate of the anticoagulant molecule is calculated:
[0082] A1 / C1=A2 / C2
[0083]
[0084] In the formula: C1 is the known anticoagulant molecule concentration value, A1 is the absorbance value corresponding to the known anticoagulant molecule concentration value (C1), A2 is the absorbance value measured in real time, C2 is the anticoagulant molecule concentration corresponding to A2, V is the volume of the solution with the known anticoagulant molecule concentration value (C1) (known), M is the mass of the anticoagulant inner layer immersed in the PBS buffer solution as a sample, V1 is the volume of the PBS buffer solution taken out each time for measuring the absorbance (3 mL), V0 is the total volume of the PBS buffer solution used for immersion (15 mL), Ci and Cn are the concentrations of the anticoagulant molecules in the immersion solution detected and calculated at the sampling time node.
[0085] The cumulative release rate of anticoagulant molecules at 28 days is as follows:
[0086] Example 1 90..76% Example 2 92..31% Comparative Example 1 24..78%
[0087] From the above table, it can be seen that in Comparative Example 1, the anticoagulant molecules are cross-linked with the collagen molecules, which significantly increases the degree of participation of the anticoagulant molecules in the cross-linking and causes them to be too tightly wrapped by the cross-linked collagen matrix, resulting in the release activity of the anticoagulant molecules being significantly lower than the anticoagulant inner layer prepared in this scheme.
[0088] Samples with an axial length of 3 cm were cut from the middle section of the artificial blood vessel obtained in step (4) of the above-mentioned Example 1, the artificial blood vessel obtained in step (4) of Example 2, and the artificial blood vessel obtained in step (4) of Comparative Example 2, and used for the in vitro liquid leakage test of the artificial blood vessel:
[0089] The two ends of the artificial blood vessel sample are coaxially connected with a dense and impermeable plastic catheter, and the connection is ensured to be tight and leak-proof as an experimental channel (i.e., the artificial blood vessel is simulated to be sutured between two natural blood vessels to play a connecting role). A glycerol aqueous solution with a mass concentration of 40% (simulated plasma) is continuously perfused into the experimental channel from one of the ports of the experimental channel through a pressure syringe for 3 minutes (the perfusion pressure of the pressure syringe is 10 kPa, equivalent to an average systolic pressure of 75 mmHg). At the same time, the liquid flowing out only from the other port of the experimental channel is collected, and the weight of the liquid is recorded to calculate the passing rate:
[0090] Passage rate (%) = the total volume of liquid collected from the experimental channel port / the total volume of liquid injected into the experimental channel during continuous perfusion for 3 minutes × 100%. The greater the pass rate, the better the anti-leakage effect of the artificial blood vessel; conversely, the smaller the pass rate, the more liquid overflows from the wall of the artificial blood vessel sample in the experimental channel during transmission, that is, the worse the anti-leakage effect.
[0091] Each sample was measured three times and the average value was taken. The specific results are shown in the following table:
[0092] Example 1 98.69±2.75% Example 2 99.15±2.81% Comparative Example 2 91.27±2.42%
[0093] From the above table, compared with Comparative Example 2 which uses pure collagen matrix as the adhesion solution, the introduction of carboxymethyl cellulose in this solution further improves the liquid leakage resistance, thereby more effectively eliminating the risk of artificial blood vessel leakage (which may cause internal bleeding under the human skin).
[0094] Viscosity characteristics test of adhesion solution:
[0095] The viscosity characteristics of the adhesion solution obtained in step (4) of the above-mentioned Example 1, the adhesion solution obtained in step (4) of Example 2, and the adhesion solution obtained in step (4) of Comparative Example 2 were analyzed using a Malvern rotational rheometer of model KINEXUS PRO. The test conditions were set to be measured after keeping warm for 30 minutes at 25°C, and the rotation speed was 50r / min. Each sample was measured three times and the average was taken. The test data are shown in the following table:
[0096] Example 1 143.58±3.42 Example 2 164.91±3.68 Comparative Example 2 97.45±2.64
Claims
1. A method for preparing a bionic artificial blood vessel with an anticoagulant inner layer, Features: The preparation method is: (1) Preparation of the anticoagulant inner layer After adding a crosslinking agent and a catalyst to a dispersion liquid with a collagen concentration of 7.5 to 9.5 mg / mL for crosslinking reaction, a hydrophilic functional molecule with anticoagulant effect is added thereto and stirred to react sufficiently to obtain a uniform composite solution, and the composite solution is naturally air-dried to obtain the anticoagulant inner layer; (2) Preparation of the middle layer of artificial blood vessels Adding a crosslinking agent and a catalyst to a dispersion having a collagen concentration of 5.5 to 7.5 mg / mL to carry out a crosslinking reaction, naturally air-drying to a non-flowing gel state, and then freeze-drying to obtain the artificial blood vessel middle layer having a dense porous structure; (3) Preparation of the outer layer of artificial blood vessels Adding a crosslinking agent and a catalyst to a dispersion having a collagen concentration of 9.5 to 11.5 mg / mL to carry out a crosslinking reaction, and then naturally air-drying the dispersion to form a dense outer layer of the artificial blood vessel; (4) Assembly of artificial blood vessels Carboxymethyl cellulose and collagen are mixed and dispersed as an adhesion solution. The anticoagulant inner layer obtained in step (1), the artificial blood vessel middle layer obtained in step (2), and the artificial blood vessel outer layer obtained in step (3) are all stacked in a rectangular shape in an alternating manner. The adhesion solution is applied to the contact surface between the anticoagulant inner layer and the artificial blood vessel middle layer, and the contact surface between the artificial blood vessel middle layer and the artificial blood vessel outer layer, respectively, and naturally air-dried to achieve tight adhesion to form a two-dimensional plane body. The two-dimensional plane body is wound on the catheter in a state where the edge of the anticoagulant inner layer on the two-dimensional plane body away from the artificial blood vessel middle layer is parallel to the axial direction of the catheter. During the winding process, the adhesion solution is applied between each winding layer. After the winding is completed, the catheter is pulled out after natural air-drying to achieve tight adhesion between each winding layer, thereby leaving the artificial blood vessel.
2. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: The dispersion is formed by fully dissolving the crushed collagen sponge in an aqueous glacial acetic acid solution, wherein the solute concentration of the aqueous glacial acetic acid solution is 0.5 mol / L.
3. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: The cross-linking agent is carbodiimide, and the catalyst is N-hydroxysuccinimide. Before adding them to each of the dispersions, the cross-linking agent and the catalyst are first dispersed in deionized water at a concentration of 15 mg / mL, respectively. The mass ratio of the added cross-linking agent to the collagen in each of the dispersions is 1:5.5-7, and the mass dosage ratio of the cross-linking agent to the catalyst is 0.8-1.5:0.8-1.
2. After adding the cross-linking agent and the catalyst to each of the dispersions, magnetic stirring is carried out at 4°C with a stirring speed of 200-800 r / min for 24 hours to achieve the cross-linking reaction.
4. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: In step (1), after the cross-linking reaction, the dispersion is mixed with the solution prepared by the hydrophilic functional molecules with anticoagulant effect at a volume ratio of 8 to 10:1 for reaction.
5. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: In step (1), the hydrophilic functional molecule with anticoagulant effect is one or a combination of heparin sodium, low molecular weight heparin, EDTA, oxalate, citrate, hirudin, warfarin, phosphorylcholine, and betaine.
6. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: In step (1), 60 mL to 100 mL of the composite solution is poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying; in step (3), 60 mL to 100 mL of the dispersion after the cross-linking reaction is poured into a square dish with a specification of 10 cm×10 cm×1.2 cm for natural air drying.
7. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: In step (2), 60 mL to 100 mL of the dispersion after the cross-linking reaction is poured into a square dish with a specification of 10 cm×10 cm×1.2 cm and naturally air-dried until it becomes a non-flowing gel, then transferred to an ultra-low temperature refrigerator and frozen at -80°C for 12 hours, and then transferred to a freeze dryer for freeze drying for 8 hours.
8. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: In step (4), the preparation process of the adhesion solution is to disperse carboxymethyl cellulose at a mass fraction of 1% to 2% in water at 18 to 25°C and stir until it becomes transparent and viscous, then add collagen at a concentration of 5.5 to 7.5 mg / mL and mix and stir for 6 to 12 hours.
9. The method for preparing the bionic artificial blood vessel with an anticoagulant inner layer according to claim 1, Features: In step (4), the outer diameter of the catheter is 3 to 10 mm, and the curling length of the anticoagulant inner layer on the two-dimensional plane is equal to the circumference of the outer diameter of the catheter, that is, it is exactly wrapped around the catheter once, and the artificial blood vessel middle layer on the two-dimensional plane is exactly wrapped around the anticoagulant inner layer after winding, and the artificial blood vessel outer layer on the two-dimensional plane is exactly wrapped around the artificial blood vessel middle layer after winding.
10. A bionic artificial blood vessel with an anticoagulant inner layer obtained by the preparation method according to any one of claims 1 to 9.