Ceramic tile renovating coating system and ceramic tile renovating method

By using tile surface treatment agent and water-based tile color-changing coating system during tile renovation, the problems of poor coating adhesion and complex construction are solved, and high adhesion and environmentally friendly construction of tile renovation are achieved, reducing garbage generation .

CN118995324APending Publication Date: 2024-11-22XIAMEN GOOK PAINT GRP CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410924709.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-22

Smart Images

  • Figure BDA0004937776120000041
    Figure BDA0004937776120000041
  • Figure BDA0004937776120000042
    Figure BDA0004937776120000042
  • Figure BDA0004937776120000051
    Figure BDA0004937776120000051
Patent Text Reader

Abstract

The invention relates to a ceramic tile renovating coating system and a ceramic tile renovating method. The coating system comprises a ceramic tile surface treating agent and water-based ceramic tile color-changing paint, the ceramic tile surface treating agent comprises the following raw materials in parts by weight: 90-96 parts of deionized water, 0.5-1.0 part of carboxymethyl cellulose, 0.1-0.3 part of a cleaning agent, 1-4 parts of an alcohol ether solvent, 0.4-0.8 part of a base material wetting agent, 0.3-0.4 part of organic acid and 1-2 parts of fluorine-containing salts. The ceramic tile renovating method adopts the coating system. The renovated coating is good in adhesive force, few in construction procedures, convenient to construct, less in generated construction waste, green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building decoration, and in particular to a ceramic tile renovation coating system and a ceramic tile renovation method. Background Art

[0002] In daily life, when floor and wall tiles become old, most of them are removed and replaced with new ones, which is time-consuming and labor-intensive, and generates a large amount of construction waste that is difficult to handle, and the renovation cost is extremely high. Therefore, recoloring old tiles will become a better choice. However, tiles are usually sintered at high temperatures, and some types of tiles are polished in order to achieve a mirror effect. The resulting dense surface makes general latex paint have very poor adhesion on the surface of the tiles. In addition, in environments such as kitchens and bathrooms, the tile surface is stained with oil or the environment is high in humidity, which can easily cause the tile color-changing coating to fall off. Summary of the invention

[0003] The object of the present invention is to provide a ceramic tile renovation coating system and a ceramic tile renovation method, wherein the ceramic tile renovation coating has good adhesion, is convenient to construct, and generates less construction waste.

[0004] To achieve the above object, the present invention discloses a tile renovation coating system, which comprises: a tile surface treatment agent and a water-based tile color-changing paint;

[0005] The tile surface treatment agent comprises the following raw materials in parts by weight: 90-96 parts of deionized water, 0.5-1.0 parts of carboxymethyl cellulose, 0.1-0.3 parts of detergent, 1-4 parts of alcohol ether solvent, 0.4-0.8 parts of substrate wetting agent, 0.3-0.4 parts of organic acid, and 1-2 parts of fluoride-containing salts.

[0006] Preferably, the organic acid is anhydrous citric acid or citric acid monohydrate, and the fluoride-containing salt is sodium bifluoride.

[0007] Preferably, the water-based tile color-changing paint includes the following raw materials in parts by weight: 7 to 22 parts of deionized water, 0.1 to 0.3 parts of pH regulator, 0.8 to 1.0 parts of wetting and dispersing agent, 0.5 to 0.8 parts of defoaming agent, 20 to 25 parts of inorganic pigments and fillers, 50 to 70 parts of acrylic emulsion, 3 to 4 parts of film-forming aid, 1.0 to 1.5 parts of rheological additive, 0.2 to 0.3 parts of preservative and bactericidal agent, and 0.1 to 0.3 parts of silane coupling agent.

[0008] Preferably, the inorganic pigment filler is one or more of rutile titanium dioxide, barium sulfate, and calcined kaolin; and the rheological additive is at least one of a polyurethane thickener and an alkali swelling thickener.

[0009] Preferably, it also includes a water-based topcoat varnish, which includes component A and component B, and the weight ratio of component A to component B is 4 to 6:1; component B is a hydrophilic modified HDI curing agent; and component A is formula 1 or formula 2:

[0010] Formula 1: The A component includes the following raw materials in parts by weight: 45-60 parts of hydroxy acrylic acid dispersion, 35-45 parts of deionized water, 0.2-0.4 parts of wetting agent, 0.5-1.0 parts of rheological additive, 0.1-0.2 parts of defoaming agent, 0.1-0.3 parts of pH regulator, 4-6 parts of film-forming additive, and 0.2-0.4 parts of anti-scratch additive;

[0011] Formula 2: The A component includes the following raw materials in parts by weight: 45-60 parts of hydroxy acrylic dispersion, 25-35 parts of deionized water, 0.2-0.4 parts of wetting agent, 0.5-1.0 parts of rheological additive, 0.1-0.2 parts of defoaming agent, 0.1-0.3 parts of pH regulator, 4-6 parts of film-forming aid, and 8-12 parts of sand grain powder.

[0012] The present invention also discloses a ceramic tile renovation method using any of the ceramic tile renovation coating systems described above, which comprises the following steps:

[0013] S1. Clean the surface of old tiles;

[0014] S2. Apply tile surface treatment agent on the surface of old tiles to clean and roughen the surface of old tiles, then clean and dry them;

[0015] S3. Apply water-based tile color-changing paint on the surface of old tiles and let it dry.

[0016] Preferably, in step S2, the amount of the tile surface treatment agent is 0.05-0.10 kg / m 2 .

[0017] Preferably, in step S3, the amount of the water-based tile color-changing paint is 0.15-0.20 kg / m 2 .

[0018] Preferably, in step S2, the surface of the old ceramic tile is left to stand for 10 to 30 minutes after being coated with the ceramic tile surface treatment agent and then cleaned; in step S3, the applied water-based ceramic tile color-changing paint is dried at a temperature of 20 to 40° C. for 24 to 48 hours.

[0019] Preferably, the step S4 is also included, which is to apply water-based topcoat varnish on the surface of the old ceramic tile coated with water-based ceramic tile color-changing paint, and dry it; the amount of the water-based topcoat varnish is 0.04-0.06kg / m 2 .

[0020] The present invention has the following beneficial effects:

[0021] 1. The present invention does not need to remove the original old tiles, has fewer construction processes, is more convenient to construct, and generates less garbage.

[0022] 2. The present invention firstly performs surface treatment on old tiles by using a tile surface treatment agent, and the adhesion ability of water-based tile color-changing paint can be guaranteed regardless of whether the tile surface has been polished or not.

[0023] 3. The coating system of the present invention is a water-based coating system, which is environmentally friendly and green. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.

[0025] The invention discloses a ceramic tile renovation method comprising the following steps:

[0026] S1. Carry out preliminary cleaning on the surface of old tiles to remove dust attached to the surface of old tiles, so that the subsequent tile surface treatment agent can take effect.

[0027] S2. Apply a layer of tile surface treatment agent on the surface of the old tiles after preliminary cleaning. The amount of tile surface treatment agent is 0.05-0.10kg / m 2 , the tile surface treatment agent can deeply clean and roughen the surface of old tiles. After 15 minutes, clean it with water and a brush and let it dry. After this treatment, the surface of the old tiles is clean and rough, which is conducive to the adhesion of subsequent coatings.

[0028] S3, coating the surface of the old ceramic tile treated in step S2 with water-based ceramic tile color-changing paint, the amount of water-based ceramic tile color-changing paint is 0.15-0.20 kg / m 2 The applied water-based tile color-changing paint is dried at 25°C for 24 to 48 hours. At this time, a layer of water-based tile color-changing paint is attached to the surface of the old tiles.

[0029] S4, apply water-based finishing varnish on the surface of the old tile coated with water-based tile color-changing paint to obtain a water-based finishing varnish coating. The amount of water-based finishing varnish is 0.04-0.06kg / m 2 The applied water-based topcoat varnish can be walked on after drying and curing at 25℃ for 24 hours, and performance testing or putting into use can be carried out after 7 days.

[0030] In the above steps, a specially designed water-based tile renovation coating system is used, namely, a tile surface treatment agent, a water-based tile color-changing paint and a water-based topcoat varnish. The tile renovation method using the water-based tile renovation coating system is simple and fast to construct, generates almost no construction waste, is more environmentally friendly, and the renovation coating has strong adhesion on the old tiles.

[0031] Specifically, the tile surface treatment agent includes the following raw materials in parts by weight: 90-96 parts of deionized water, 0.5-1.0 parts of carboxymethyl cellulose, 0.1-0.3 parts of detergent, 1-4 parts of alcohol ether solvent, 0.4-0.8 parts of substrate wetting agent, 0.3-0.4 parts of organic acid, and 1-2 parts of fluoride-containing salts. In this case, the substrate wetting agent is 2105-3 substrate wetting agent, which can make the treatment agent spread evenly on the surface of the tile and treat it evenly; the detergent is sodium dodecylbenzene sulfonate detergent, and the alcohol ether solvent is DB solvent. These two ingredients can effectively remove various dirt on the surface of the tile and eliminate the effect of dirt on the adhesion performance between the coatings; the organic acid is citric acid monohydrate, and the fluoride-containing salt is sodium bifluoride. These two ingredients can react quickly with the silicon dioxide on the surface of the tile, reduce the smoothness of the tile interface, and thus improve the adhesion performance of the water-based tile color-changing paint layer and the tile interface.

[0032] Referring to the parameters in Table 1, four embodiments (embodiment A / B / C / D) are set for the tile surface treatment agent. Taking embodiment A as an example, the preparation process of the tile surface treatment agent is described: 94.5 parts of deionized water are added to a stirring container, and 0.6 parts of carboxymethyl cellulose, 0.2 parts of sodium dodecylbenzene sulfonate cleaner, 2 parts of DB solvent, 0.4 parts of 2105-3 substrate wetting agent, 0.3 parts of citric acid monohydrate, and 2 parts of sodium bifluoride are added in sequence under medium-to-low speed stirring, and stirred evenly at medium-to-low speed.

[0033] Table 1

[0034]

[0035] The treatment effect of the tile surface treatment agent obtained by configuring the above four embodiments (embodiments A / B / C / D) was tested, and a blank control group was set up at the same time. The results are shown in Table 2. As can be seen from Table 2, the tile surface treatment agent in the present invention can effectively reduce the mirror effect of the tile glaze surface, improve the hydrophilicity of the tile glaze surface, and thus improve the adhesion performance of the water-based tile color-changing paint to the tile surface (the above experiments all use the water-based tile color-changing paint described in Example E).

[0036] Table 2

[0037]

[0038] The water-based tile color-changing paint includes the following raw materials in parts by weight: 7 to 22 parts of deionized water, 0.1 to 0.3 parts of pH regulator, 0.8 to 1.0 parts of wetting and dispersing agent, 0.5 to 0.8 parts of defoaming agent, 20 to 25 parts of inorganic pigments and fillers, 50 to 70 parts of acrylic emulsion, 3 to 4 parts of film-forming aid, 1.0 to 1.5 parts of rheological additive, 0.2 to 0.3 parts of preservative and bactericidal agent, and 0.1 to 0.3 parts of silane coupling agent. In this case, the pH regulator is 298PH regulator, the wetting and dispersing agent is BD-109 wetting agent and 731A dispersing agent, the defoaming agent is 0602 defoaming agent, the inorganic pigments and fillers are R706 rutile titanium dioxide, barium sulfate, calcined kaolin, the film-forming aid is C-12 film-forming aid, the rheological aid is polyurethane thickener and alkali swelling thickener, and the preservative and bactericidal agent is EG-CT preservative and bactericidal agent. The silane coupling agent contains silane groups that can react with inorganic materials and organic functional groups that can react with organic materials. The silane groups will form silicon-oxygen bonds with the hydroxyl groups on the surface of the tile, while the organic functional groups will combine with the coating to form a stronger bond. This combination can enhance the adhesion performance of the water-based color-changing paint coating and the tile interface, and improve the weather resistance, chemical resistance and mechanical strength of the coating itself.

[0039] Referring to the parameters in Table 3, four embodiments (Embodiment E / F / G / H) are set for water-based tile color-changing paint. Taking Embodiment E as an example, the preparation process of water-based tile color-changing paint is described as follows: 21.6 parts of deionized water are added to a stirring container, and 0.7 parts of 731A dispersant, 0.1 parts of BD-109 wetting agent, 0.3 parts of 0602 defoaming agent, and 0.1 parts of 298PH regulator are added in sequence under medium-low speed stirring; appropriately increase the temperature. Add 22 parts of R706 rutile titanium dioxide, barium sulfate and calcined kaolin (inorganic pigment and filler) in turn at a higher speed and disperse at high speed until the fineness is qualified; reduce the speed and add 50 parts of acrylic emulsion, 3 parts of C-12 film-forming aid, 0.3 parts of 0602 defoamer, 1 part of polyurethane thickener, 0.4 parts of alkali swelling thickener (rheological additive), 0.3 parts of EG-CT preservative and bactericidal agent, and 0.2 parts of silane coupling agent in turn, and stir at medium or low speed until evenly mixed.

[0040] Table 3

[0041]

[0042] The water-based tile color-changing paint obtained by configuring the above four embodiments (Embodiments E / F / G / H) was tested for performance, and the results are shown in Table 4. As can be seen from Table 4, the water-based tile color-changing paint of the present invention has good stability, short drying time, excellent performance, and is particularly suitable for occasions such as renovation that require high construction time. Compared with oil-based paint, the present invention is environmentally friendly, has no irritating odor, and is particularly suitable for indoor use; compared with UV light-curing paint, the present invention can be dried naturally, does not require special treatment, and is simple to operate.

[0043] Table 4

[0044]

[0045] The water-based topcoat varnish comprises component A and component B, wherein the weight ratio of component A to component B is 4 to 6:1; component B is a hydrophilic modified HDI curing agent; component A is formula 1 (wear-resistant type) or formula 2 (anti-slip type), specifically:

[0046] Formula 1: Component A includes the following raw materials in parts by weight: 45-60 parts of hydroxy acrylic dispersion, 35-45 parts of deionized water, 0.2-0.4 parts of wetting agent, 0.5-1.0 parts of rheological additive, 0.1-0.2 parts of defoaming agent, 0.1-0.3 parts of PH regulator, 4-6 parts of film-forming agent, 0.2-0.4 parts of anti-scratch agent. The wetting agent is 2105-3 substrate wetting agent, the rheological additive is polyurethane thickener, the defoaming agent is BYK022 defoaming agent, the PH regulator is triethanolamine PH regulator, the film-forming agent is DPnB film-forming agent, and the anti-scratch agent is DC51 anti-scratch agent.

[0047] Formula 2: Component A includes the following raw materials in parts by weight: 45-60 parts of hydroxy acrylic dispersion, 25-35 parts of deionized water, 0.2-0.4 parts of wetting agent, 0.5-1.0 parts of rheological additive, 0.1-0.2 parts of defoaming agent, 0.1-0.3 parts of PH regulator, 4-6 parts of film-forming aid, 8-12 parts of sand grain powder. The wetting agent is 2105-3 substrate wetting agent, the rheological additive is polyurethane thickener, the defoaming agent is BYK022 defoaming agent, the PH regulator is triethanolamine PH regulator, and the film-forming aid is DPnB film-forming aid.

[0048] Referring to the parameters in Table 5, four embodiments (embodiment I / J / K / L) are set for the wear-resistant water-based topcoat varnish. Taking embodiment I as an example, the preparation process of the wear-resistant water-based topcoat varnish is described: 43.7 parts of deionized water are added to a stirring container, and 0.2 parts of triethanolamine pH regulator, 0.2 parts of 2105-3 substrate wetting agent, 0.2 parts of BYK022 defoamer, 50 parts of hydroxy acrylic acid dispersion, 0.5 parts of polyurethane thickener (rheological additive), 5 parts of DPnB film-forming additive, and 0.2 parts of DC51 anti-scratch additive are added in sequence under medium-low speed stirring, and the A component of the wear-resistant water-based topcoat varnish is obtained by stirring evenly. Then, the paint is prepared according to component A: component B = 5:1 to obtain the wear-resistant water-based topcoat varnish.

[0049] Table 5

[0050]

[0051] The wear-resistant water-based top varnish obtained by configuring the above four embodiments (embodiments I / J / K / L) was subjected to performance tests, and the results are shown in Table 6. As can be seen from Table 6, the wear-resistant water-based top varnish coating film of the present invention has high hardness and good wear resistance, and is suitable for use in areas such as living rooms that require high wear resistance.

[0052] Table 6

[0053]

[0054]

[0055] Referring to the parameters in Table 7, four embodiments (embodiment M / N / O / P) are set for the anti-slip water-based topcoat varnish. Taking embodiment M as an example, the preparation process of the anti-slip water-based topcoat varnish is described: 34.3 parts of deionized water are added to a stirring container, and 0.2 parts of triethanolamine pH regulator, 0.3 parts of 2105-3 substrate wetting agent, 0.2 parts of BYK022 defoamer, and 50 parts of hydroxy acrylic acid dispersion are added in sequence under medium-low speed stirring, 9 parts of sand grain powder are added at a high speed, and the fineness is qualified, and the speed is reduced to add 1 part of polyurethane thickener (rheological additive) and 5 parts of DPnB film-forming aid in sequence, and stir evenly to obtain component A of the anti-slip water-based topcoat varnish. Then, the paint is prepared according to component A: component B = 4.5:1 to obtain the anti-slip water-based topcoat varnish.

[0056] Table 7

[0057]

[0058] The performance test of the anti-skid water-based topcoat varnish obtained by configuring the above four embodiments (embodiments M / N / O / P) is carried out, and the results are shown in Table 8. As can be seen from Table 8, the anti-skid water-based topcoat varnish coating film of the present invention has good anti-skid performance and is suitable for use in areas such as kitchens and bathrooms that require high anti-skid performance.

[0059] Table 8

[0060]

[0061]

[0062] According to the above-mentioned ceramic tile renovation method, four embodiments (embodiment 1 / embodiment 2 / embodiment 3 / embodiment 4) are set up to test the performance of ceramic tiles renovated by the renovation method of the present invention, and the results are shown in Table 9. Among them, embodiment 1 uses the ceramic tile surface treatment agent of embodiment A, the water-based ceramic tile color-changing paint of embodiment E, and the wear-resistant water-based topcoat varnish of embodiment I; embodiment 2 uses the ceramic tile surface treatment agent of embodiment A, the water-based ceramic tile color-changing paint of embodiment F, and the wear-resistant water-based topcoat varnish of embodiment J; embodiment 3 uses the ceramic tile surface treatment agent of embodiment C, the water-based ceramic tile color-changing paint of embodiment E, and the anti-slip water-based topcoat varnish of embodiment M; embodiment 4 uses the ceramic tile surface treatment agent of embodiment C, the water-based ceramic tile color-changing paint of embodiment H, and the anti-slip water-based topcoat varnish of embodiment O.

[0063] Table 9

[0064]

[0065]

[0066] It can be seen from Table 9 that the renovation coating obtained by the tile renovation method of the present invention meets the standard requirements, has excellent performance, good coating effect, and can also select wear-resistant or anti-slip effects as needed, which is suitable for promotion and application.

[0067] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered by the protection scope of the present invention.

Claims

1. A tile renovation coating system, characterized in that: include: Tile surface treatment agent and water-based tile color-changing paint; The tile surface treatment agent comprises the following raw materials in parts by weight: 90-96 parts of deionized water, 0.5-1.0 parts of carboxymethyl cellulose, 0.1-0.3 parts of detergent, 1-4 parts of alcohol ether solvent, 0.4-0.8 parts of substrate wetting agent, 0.3-0.4 parts of organic acid, and 1-2 parts of fluoride-containing salts.

2. The tile renovation coating system according to claim 1, characterized in that: The organic acid is anhydrous citric acid or citric acid monohydrate, and the fluorine-containing salt is sodium bifluoride.

3. The tile renovation coating system according to claim 1, characterized in that: The water-based tile color-changing paint includes the following raw materials in parts by weight: 7 to 22 parts of deionized water, 0.1 to 0.3 parts of a pH regulator, 0.8 to 1.0 parts of a wetting and dispersing agent, 0.5 to 0.8 parts of a defoaming agent, 20 to 25 parts of an inorganic pigment and filler, 50 to 70 parts of an acrylic emulsion, 3 to 4 parts of a film-forming aid, 1.0 to 1.5 parts of a rheological aid, 0.2 to 0.3 parts of an antiseptic and bactericidal agent, and 0.1 to 0.3 parts of a silane coupling agent.

4. The tile renovation coating system according to claim 3, characterized in that: The inorganic pigment filler is one or more of rutile titanium dioxide, barium sulfate and calcined kaolin; the rheological additive is at least one of a polyurethane thickener and an alkali swelling thickener.

5. The tile renovation coating system according to claim 1, characterized in that: It also includes a water-based topcoat varnish, which includes a component A and a component B, wherein the weight ratio of the component A to the component B is 4 to 6:1; the component B is a hydrophilic modified HDI curing agent; the component A is formula one or formula two: Formula 1: The A component includes the following raw materials in parts by weight: 45-60 parts of hydroxy acrylic acid dispersion, 35-45 parts of deionized water, 0.2-0.4 parts of wetting agent, 0.5-1.0 parts of rheological additive, 0.1-0.2 parts of defoaming agent, 0.1-0.3 parts of pH regulator, 4-6 parts of film-forming additive, and 0.2-0.4 parts of anti-scratch additive; Formula 2: The A component includes the following raw materials in parts by weight: 45-60 parts of hydroxy acrylic dispersion, 25-35 parts of deionized water, 0.2-0.4 parts of wetting agent, 0.5-1.0 parts of rheological additive, 0.1-0.2 parts of defoaming agent, 0.1-0.3 parts of pH regulator, 4-6 parts of film-forming aid, and 8-12 parts of sand grain powder.

6. A method for renovating a tile using the tile renovation coating system according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Clean the surface of old tiles; S2. Apply tile surface treatment agent on the surface of old tiles to clean and roughen the surface of old tiles, then clean and dry them; S3. Apply water-based tile color-changing paint on the surface of old tiles and let it dry.

7. The ceramic tile renovation method according to claim 6, characterized in that: In step S2, the amount of the tile surface treatment agent is 0.05-0.10 kg / m 2 .

8. The ceramic tile renovation method according to claim 6, characterized in that: In step S3, the amount of the water-based tile color-changing paint is 0.15-0.20 kg / m 2 .

9. The ceramic tile renovation method according to claim 6, characterized in that: In step S2, the surface of the old ceramic tile is left to stand for 10 to 30 minutes after being coated with the ceramic tile surface treatment agent and then washed; in step S3, the applied water-based ceramic tile color-changing paint is dried at a temperature of 20 to 40° C. for 24 to 48 hours.

10. The ceramic tile renovation method according to claim 6, characterized in that: The method further comprises step S4, which is to apply water-based topcoat varnish on the surface of the old ceramic tile coated with water-based ceramic tile color-changing paint, and then air-dry the surface; the amount of the water-based topcoat varnish is 0.04-0.06 kg / m 2 .

Citation Information

Cited By

  • Environment-friendly indoor renovating surface treating agent, renovating color-changing paint and renovating construction method

    CN121022263A

  • Water replenishing solution for electric porcelain insulator, and preparation method and use method of water replenishing solution

    CN122187506A

  • A composite coating for tile renovation and its preparation method and application

    CN122878786A