Preparation method and application of gamma-AlOOH / SiO2 composite film for Cr (VI) adsorption

The γ-AlOOH/SiO2 composite film prepared by the sol-gel method solves the problems of Cr(VI) adsorption performance and separation difficulty in the existing technology, and achieves efficient and low-cost Cr(VI) adsorption and acidic environment Excellent film stability to avoid secondary pollution.

CN118743984AActive Publication Date: 2024-10-08GUANGZHOU UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410980153.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-08
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

It is difficult to prepare γ-AlOOH/SiO2 composite films with good Cr(VI) adsorption performance and easy separation under safe and mild conditions at low cost with the existing technology. Moreover, the preparation process of common methods is complicated and has high equipment costs and high energy consumption. question.

Method used

Using the sol-gel method, cheap pseudo-boehmite and silica are used as aluminum and silicon sources, lactic acid is added as a peptizer and polyvinyl alcohol as a film-forming aid, and γ- is prepared by evenly applying and drying at room temperature. AlOOH/SiO2 composite film.

Benefits of technology

It achieves efficient adsorption of Cr(VI) in an acidic environment, with an adsorption capacity of 23.91mg/g and an adsorption removal rate of 94.67%. The film has good toughness and acid-resistant stability in an acidic environment, making it easy to separate pollutants. Secondary pollution is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743984A_ABST
    Figure CN118743984A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a gamma-AlOOH / SiO2 composite film for adsorbing toxic Cr (VI) in water and application of the gamma-AlOOH / SiO2 composite film. The method comprises the following steps: adding lactic acid to peptize pseudo-boehmite with a certain solid content; sequentially adding silicon dioxide and polyvinyl alcohol; and finally, carrying out tape casting on the composite sol on a substrate, and naturally drying to obtain the gamma-AlOOH / SiO2 composite film. Most of composite films are usually prepared into single sols firstly and then mixed to prepare the composite sol, the composite sol is prepared in one step through the method, safer lactic acid is used for replacing common peptizing agents such as nitric acid, glacial acetic acid and hydrochloric acid, and the method has the advantages of being convenient in raw material source, non-toxic, harmless, simple in preparation process, safe and mild in reaction condition and the like. The gamma-AlOOH / SiO2 composite film prepared by the method has relatively large adsorption capacity and relatively high adsorption rate on Cr (VI) in a water body, and stronger acid resistance and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of developing an adsorbent for treating wastewater containing heavy metal ions, and specifically relates to a preparation method and application of a gamma-AlOOH / SiO2 composite film for Cr(VI) adsorption. Background Art

[0002] Wastewater generated during the production process of electroplating, textile, metal processing and other industries often contains a large amount of heavy metal ions such as Cr(VI), Pb(II), As(V), etc., which are widely sourced, highly toxic, long-lasting, and have certain masking and enrichment properties. If they are discharged directly into the environment without treatment, they will cause serious harm to human health and the ecosystem. Among them, highly soluble Cr(VI) has strong mutagenic and carcinogenic effects after being absorbed through the respiratory tract or skin. At present, the commonly used treatment methods for chromium-containing wastewater include ion exchange, chemical precipitation, membrane separation and adsorption. The adsorption method can remove heavy metal ions in the solution by virtue of the high specific surface area and special functional groups of the adsorbent material. It has the advantages of simple operation, low cost and high adsorption efficiency, and therefore has attracted much attention. Commonly used powder adsorbents include activated carbon, zeolite, clay, metal oxides, SiO2, nanomagnetic particles, synthetic polymers and biomass, but they have more or less disadvantages in their use, such as difficulty in separation after adsorption of pollutants, easy agglomeration, and easy loss leading to secondary pollution of water bodies. In contrast, membrane adsorption materials with integral structures have the advantages of easy regeneration and easy separation after adsorption, and therefore have attracted attention. Considering that most industrial wastewater containing Cr(VI) is acidic, it is necessary to prepare thin film materials that are stable under acidic conditions.

[0003] According to the different membrane materials, membranes are mainly divided into four types: inorganic membranes, bio-based membranes, functionalized polymer-based membranes, and mixed matrix membranes. Inorganic membrane materials that have been reported for the adsorption and removal of heavy metal pollutants include NaA-type zeolites, MCM-41, MCM-48, and zeolite molecular sieves. However, in the above cases, the chromium in most solutions exists in the form of chromate anions, and the above adsorption membranes are obviously not very suitable; efficient adsorption membranes should provide abundant binding sites for the adsorption of heavy metal ions. Compared with the preparation methods of membrane materials such as chemical vapor deposition, spray thermal decomposition, thermal evaporation, electron beam evaporation, magnetron sputtering, and anodization, the sol-gel method has the advantages of low-temperature liquid phase preparation, simple process, and easy regulation of product composition and pore structure. Adding a suitable cross-linking agent in the process of forming the sol also helps to form a membrane material with high cross-linking degree and good stability.

[0004] Pseudo-boehmite (γ-AlOOH·nH2O) has excellent properties such as high specific surface area, environmental friendliness, porosity and rich hydroxyl groups; amorphous SiO2 is a porous material with high specific surface area, good thermal stability, rich surface hydroxyl groups and good modifiability. Both are adsorbent materials with great potential for industrial wastewater treatment. Tu et al. (Tu WJ, Cai WQ, Jiang YH, et al. Facile synthesis of novel rare earth elements modified SiO2 films for effective Cr(VI)removal from electroplating effluent [J]. Journal of Chemical and Engineering Data, 2019, 64, 2677-2685.) successfully prepared a rare earth element modified SiO2 film with a smooth surface and no cracks by using solvent evaporation induced self-assembly method. Since the hydroxyl groups on the rare earth elements can undergo ion exchange and electrostatic adsorption with Cr(VI) in the solution, Cr(VI) can be effectively adsorbed and reduced to low-toxic Cr(III) on the film surface. However, rare earth elements are relatively expensive and block the pores when introduced, resulting in a decrease in the specific surface area and pore volume of the film. Most of the studies reported so far mainly prepare γ-AlOOH films or SiO2 films by doping modification, introduction of surfactants, hydrothermal treatment, and electrospinning. While the preparation cost increases, the doped materials may block the pores, resulting in a decrease in the specific surface area and pore volume of the film; or new impurity ions are introduced, affecting the purity of the sol. Miao et al. (Miao YE, Wang R, Chen D, et al. Electrospun self-standing membrane of hierarchical SiO2@γ-AlOOH (boehmite) core / sheath fibers for water remediation [J]. ACS Applied Materials & Interfaces, 2012, 4 (10), 5353-5359.) based on the combination of electrospinning and hydrothermal reaction, anchored γ-AlOOH nanosheets uniformly on the surface of SiO2 fibers to prepare hierarchical SiO2@γ-AlOOH core / sheath self-supporting membranes, which provided a direct contact area between pseudo-boehmite and the solution, were easy to handle and recycle, and had an adsorption capacity of 21.3 mg / g for Congo red. However, the hydrothermal treatment would generate a certain amount of energy consumption, and the electrospinning method had high equipment cost and low productivity. In addition, the preparation process was carried out under high pressure, which was dangerous.In addition, the silicon source and aluminum source used in the study are mostly organic substances such as tetraethyl orthosilicate, aluminum isopropoxide, and aluminum sec-butoxide, and the hydrolysis process is complicated and has many influencing factors; when aluminum nitrate, aluminum chloride, etc. are used as aluminum sources, it is often necessary to first filter to obtain a precipitate, and then add a certain amount of nitric acid, hydrochloric acid or acetic acid to prepare a sol, and the steps are numerous and the added acid has a certain corrosiveness. CN110064358B discloses a method for preparing a SiO2 / γ-AlOOH composite film for toxic Cr(VI) adsorption using aluminum nitrate nonahydrate as an aluminum source and tetraethyl orthosilicate as a silicon source, but it is necessary to first prepare a SiO2 sol and a γ-AlOOH sol separately, and then mix them with an acidified PVA solution in a certain proportion, and the steps are relatively cumbersome.

[0005] In summary, the use of a relatively simple preparation process under safe and mild conditions to develop a silicon-aluminum oxide composite film based on the excellent properties of environmentally friendly γ-AlOOH and SiO2, which is stable in acidic aqueous solution, has good adsorption performance for toxic Cr(VI) and is easy to separate from water, has important scientific significance and application prospects. The successful implementation of the research will provide new ideas for the development of composite oxide membrane materials that are easy to separate solid / liquid and the treatment of toxic heavy metal ion wastewater. Summary of the invention

[0006] The technical problem to be solved by the present invention is: using low-priced, conveniently sourced and environmentally friendly pseudo-boehmite and silica as aluminum source and silicon source respectively, selecting suitable peptizing agents and film-forming aids, and synthesizing a γ-AlOOH / SiO2 composite film with good adsorption performance for toxic Cr(VI) and easy separation through a sol-gel method under mild and simple conditions.

[0007] In order to solve the above technical problems, the primary purpose of the present invention is to provide a method for preparing a γ-AlOOH / SiO2 composite film for Cr(VI) adsorption.

[0008] Another object of the present invention is to provide a γ-AlOOH / SiO2 composite film prepared by the above method.

[0009] Another object of the present invention is to provide applications of the above-mentioned γ-AlOOH / SiO2 composite film.

[0010] The technical problem to be solved by the present invention is achieved through the following technical solutions:

[0011] A method for preparing a γ-AlOOH / SiO2 composite film for adsorbing toxic Cr(VI) in water: first, dispersing pseudo-boehmite powder in water at room temperature, adding lactic acid for degumming, and obtaining a suspension; then, uniformly dispersing nano-silicon dioxide powder in the suspension, adding a film-forming aid polyvinyl alcohol, and stirring uniformly at room temperature to obtain a composite sol; finally, uniformly applying the composite sol on a substrate, casting it, and drying it at room temperature to obtain a γ-AlOOH / SiO2 composite film.

[0012] The ratio of the pseudo-boehmite powder to lactic acid is based on the mass ratio: m (lactic acid) / m (pseudo-boehmite) = 0.15-0.75, and the preferred ratio is m (lactic acid) / m (pseudo-boehmite) = 0.45-0.75.

[0013] The mass ratio of the pseudo-boehmite powder to the silicon dioxide powder is (2-6):1.

[0014] The mass fraction of pseudo-boehmite in the suspension is 2-8 wt %.

[0015] The added amount of the polyvinyl alcohol is (0.1-0.8 g) polyvinyl alcohol / 10 mL of the composite sol.

[0016] The preparation method specifically comprises the following steps:

[0017] (1) dispersing 0.8 to 3.2 parts by weight of pseudo-boehmite powder in deionized water at room temperature, and then rapidly adding 0.12 to 2.4 parts by weight of lactic acid to perform debonding;

[0018] (2) adding 0.133 to 1.600 parts by weight of nano-silicon dioxide powder to the solution obtained in step (1), stirring at room temperature for a certain period of time to obtain a composite sol;

[0019] (3) Take the composite sol in step (2), add polyvinyl alcohol, stir for 2 hours, and finally apply the γ-AlOOH / SiO2 composite sol on the substrate for tape casting. After drying for 48 hours at room temperature and static air, peel off the film to obtain the γ-AlOOH / SiO2 composite film.

[0020] In step (1), the mass of the aluminum sol is maintained at 40 g, that is, the sum of the mass parts of the pseudo-boehmite powder, lactic acid and deionized water is 40 parts.

[0021] The stirring time in step (2) is 8 hours.

[0022] The γ-AlOOH / SiO2 composite film prepared by the above method can be used to adsorb Cr(VI) in water.

[0023] When the γ-AlOOH / SiO2 composite film is used to adsorb Cr(VI) solution with a pH of 2 and a concentration of 50 mg / L, the maximum adsorption amount of Cr(VI) is 23.91 mg / g. In comparison, the adsorption amounts of Cr(VI) by a single γ-AlOOH film and a SiO2 film are 19.42 mg / g and 20.37 mg / g, respectively.

[0024] In addition, the γ-AlOOH / SiO2 composite film obtained by the above preparation method has strong toughness and elasticity in an acidic environment. After immersing the composite film in a pH = 1 aqueous solution for 5 hours, it was found that: the mass of the γ-AlOOH film lost 28.16%; although the mass of the SiO2 film only lost 3.85%, the brittleness of the film was very large; and the γ-AlOOH / SiO2 composite film did not crack after being pulled and could rebound, not only retaining the toughness of the γ-AlOOH film, but also only losing 12.75% of its mass, and significantly enhancing its acid resistance and stability.

[0025] The principle underlying the technical solution of the present invention is that the surfaces of γ-AlOOH and SiO2 are both rich in hydroxyl groups. After being peptized with lactic acid, they react with the film-forming agent polyvinyl alcohol by forming hydrogen bonds and covalent bonds. In the subsequent drying process, polyvinyl alcohol, silicon dioxide, and pseudo-boehmite undergo cross-linking reactions to form a uniform composite film. Polyvinyl alcohol provides good mechanical properties for the composite film, making it easy to separate after adsorbing Cr(VI). As active components of the adsorbent, silicon dioxide and pseudo-boehmite provide more adsorption sites for the adsorption of Cr(VI) ions.

[0026] Compared with other Cr(VI) adsorbents, the γ-AlOOH / SiO2 composite film prepared by the present invention has the following advantages:

[0027] (1) Using cheap and non-toxic commercial pseudo-boehmite powder as the aluminum source instead of toxic and expensive aluminum alcohol;

[0028] (2) Innovative use of organic acid lactic acid as a peptizer, replacing conventional corrosive strong acids, which is non-toxic and safe to operate;

[0029] (3) The sol-gel method used has low equipment requirements, mild preparation conditions and simple operation;

[0030] (4) The prepared γ-AlOOH / SiO2 composite film has a certain adsorption capacity for Cr(VI). When the initial concentration of Cr(VI) is 50 mg / L, the maximum adsorption amount of Cr(VI) is 23.91 mg / g, and the adsorption removal rate is as high as 94.67%.

[0031] (5) The prepared γ-AlOOH / SiO2 composite film has good toughness in an acidic environment and is not easy to crack;

[0032] (6) The prepared γ-AlOOH / SiO2 composite film is easy to separate after adsorbing pollutants and will not cause secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The adsorption kinetic curve of Cr(VI) by the γ-AlOOH / SiO2 composite film prepared in Example 1-7;

[0034] Figure 2 The adsorption kinetic curves of the γ-AlOOH / SiO2 composite film (BSPM) prepared in Example 1, the γ-AlOOH film (BPM) prepared in Example 8, and the SiO2 film (SPM) prepared in Example 9;

[0035] Figure 3 XRD patterns of the γ-AlOOH / SiO2 composite film (BSPM) prepared in Example 1, the γ-AlOOH film (BPM) prepared in Example 8, and the SiO2 film (SPM) prepared in Example 9;

[0036] Figure 4 SEM photos of the γ-AlOOH / SiO2 composite film (BSPM) prepared in Example 1, the γ-AlOOH film (BPM) prepared in Example 8, and the SiO2 film (SPM) prepared in Example 9;

[0037] Figure 5 This is a photo of the γ-AlOOH / SiO2 composite film prepared in Example 1;

[0038] Figure 6 This is a photo of the toughness of the γ-AlOOH / SiO2 composite film prepared in Example 3 after adsorbing Cr(VI);

[0039] Figure 7 This is a comparison chart of the γ-AlOOH / SiO2 composite film prepared in Example 1 before and after adsorption of Cr(VI). DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. For process parameters not specifically noted, conventional techniques may be used.

[0041] Embodiment 1:

[0042] (1) 3.2 g of pseudo-boehmite powder was dispersed in 34.4 g of water at room temperature, and 2.4 g of lactic acid was slowly added dropwise for debonding to obtain a suspension; then 1.6 g of nano-silica powder was evenly dispersed in the above suspension, and the γ-AlOOH / SiO2 composite sol was obtained after stirring for 8 h.

[0043] (2) Take 10 mL of the composite sol in step (1), add 8 g of 10 wt% polyvinyl alcohol, stir for 2 h, and finally apply the γ-AlOOH / SiO2 composite sol on a 2 cm×6 cm polytetrafluoroethylene plate to form a tape-casting film. After drying at room temperature and static air for 48 h, peel off the film to obtain the γ-AlOOH / SiO2 composite film.

[0044] (3) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH / SiO2 composite film, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH / SiO2 composite film is shown in Figure 1 The adsorption removal rate of Cr(VI) is 94.67%, and the adsorption amount is 23.91 mg / g.

[0045] Embodiment 2:

[0046] (1) 2 g of pseudo-boehmite powder was dispersed in 37.1 g of water at room temperature, and 0.9 g of lactic acid was slowly added dropwise for debonding to obtain a suspension; then 1 g of nano-silica powder was evenly dispersed in the above suspension, and the γ-AlOOH / SiO2 composite sol was obtained after stirring for 8 h.

[0047] (2) Take 10 mL of the composite sol in step (1), add 5 g of 10 wt% polyvinyl alcohol, stir for 2 h, and finally apply the γ-AlOOH / SiO2 composite sol on a 2 cm×6 cm polytetrafluoroethylene plate to form a tape-casting film. After drying at room temperature and static air for 48 h, peel off the film to obtain the γ-AlOOH / SiO2 composite film.

[0048] (3) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH / SiO2 composite film sample, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH / SiO2 composite film is shown in Figure 1 The adsorption removal rate of Cr(VI) is 91.75%, and the adsorption amount is 23.41 mg / g.

[0049] Embodiment 3:

[0050] (1) 0.8 g of pseudo-boehmite powder was dispersed in 38.84 g of water at room temperature, and 0.36 g of lactic acid was slowly added dropwise for debonding to obtain a suspension; then 0.13 g of nano-silica powder was evenly dispersed in the above suspension, and the γ-AlOOH / SiO2 composite sol was obtained after stirring for 8 h.

[0051] (2) Take 10 mL of the composite sol in step (1), add 8 g of 10 wt% polyvinyl alcohol, stir for 2 h, and finally apply the γ-AlOOH / SiO2 composite sol on a 2 cm×6 cm polytetrafluoroethylene plate to form a tape-casting film. After drying at room temperature and static air for 48 h, peel off the film to obtain the γ-AlOOH / SiO2 composite film.

[0052] (3) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH / SiO2 composite film, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH / SiO2 composite film is shown in Figure 1 The adsorption removal rate of Cr(VI) is 85.57%, and the adsorption amount is 22.05 mg / g.

[0053] Embodiment 4:

[0054] (1) 0.8 g of pseudo-boehmite powder was dispersed in 38.6 g of water at room temperature, and 0.6 g of lactic acid was slowly added dropwise for debonding to obtain a suspension; then 0.2 g of nano-silica powder was evenly dispersed in the above suspension, and the γ-AlOOH / SiO2 composite sol was obtained after stirring for 8 h.

[0055] (2) Take 10 mL of the composite sol in step (1), add 5 g of 10 wt% polyvinyl alcohol, stir for 2 h, then apply the γ-AlOOH / SiO2 composite sol on a 2 cm×6 cm polytetrafluoroethylene plate to form a tape-casting film, and then dry it at room temperature in static air for 48 h before peeling off the film to obtain the γ-AlOOH / SiO2 composite film.

[0056] (3) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH / SiO2 composite film sample, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH / SiO2 composite film is shown in Figure 1The adsorption removal rate of Cr(VI) is 87.63%, and the adsorption amount is 21.91 mg / g.

[0057] Embodiment 5:

[0058] (1) 2 g of pseudo-boehmite powder was dispersed in 37.7 g of water at room temperature, and 0.3 g of lactic acid was slowly added dropwise for debonding to obtain a suspension; then 0.5 g of nano-silica powder was evenly dispersed in the above suspension, and the γ-AlOOH / SiO2 composite sol was obtained after stirring for 8 h.

[0059] (2) Take 10 mL of the composite sol in step (1), add 8 g of 10 wt% polyvinyl alcohol, stir for 2 h, and finally apply the γ-AlOOH / SiO2 composite sol on a 2 cm×6 cm polytetrafluoroethylene plate to form a tape-casting film. After drying at room temperature and static air for 48 h, peel off the film to obtain the γ-AlOOH / SiO2 composite film.

[0060] (3) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH / SiO2 composite film sample, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH / SiO2 composite film is shown in Figure 1 The adsorption removal rate of Cr(VI) is 90.21%, and the adsorption amount is 22.55 mg / g.

[0061] Embodiment 6:

[0062] (1) 0.8 g of pseudo-boehmite powder was dispersed in 39.08 g of water at room temperature, and 0.12 g of lactic acid was slowly added dropwise for debonding to obtain a suspension; then 0.4 g of nano-silicon dioxide was uniformly dispersed in the above suspension, and the γ-AlOOH / SiO2 composite sol was obtained after stirring for 8 h.

[0063] (2) Take 10 mL of the composite sol in step (1), add 1 g of 10 wt% polyvinyl alcohol, stir for 2 h, and finally apply the γ-AlOOH / SiO2 composite sol on a 2 cm×6 cm polytetrafluoroethylene plate to form a tape-casting film. After drying at room temperature and static air for 48 h, peel off the film to obtain the γ-AlOOH / SiO2 composite film.

[0064] (3) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH / SiO2 composite film sample, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH / SiO2 composite film is shown in Figure 1 The adsorption removal rate of Cr(VI) is 76.63%, and the adsorption amount is 18.97 mg / g.

[0065] Embodiment 7:

[0066] (1) 3.2 g of pseudo-boehmite powder was dispersed in 36.32 g of water at room temperature, and 0.48 g of lactic acid was slowly added dropwise for debonding to obtain a suspension; then 0.53 g of nano-silica powder was uniformly dispersed in the above suspension, and the γ-AlOOH / SiO2 composite sol was obtained after stirring for 8 h.

[0067] (2) Take 10 mL of the composite sol in step (1), add 5 g of 10 wt% polyvinyl alcohol, stir for 2 h, and finally apply the γ-AlOOH / SiO2 composite sol on a 2 cm×6 cm polytetrafluoroethylene plate to form a tape-casting film. After drying at room temperature and static air for 48 h, peel off the film to obtain the γ-AlOOH / SiO2 composite film.

[0068] (3) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH / SiO2 composite film sample, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH / SiO2 composite film is shown in Figure 1 The adsorption removal rate of Cr(VI) is 64.95%, and the adsorption amount is 16.40 mg / g.

[0069] Embodiment 8:

[0070] In order to compare the adsorption performance of γ-AlOOH / SiO2 composite film and γ-AlOOH film, γ-AlOOH film was also prepared. The relevant steps and adsorption performance test process are as follows:

[0071] (1) 3.2 g of pseudo-boehmite powder was dispersed in 34.4 g of water at room temperature, and 2.4 g of lactic acid was slowly added for debonding. After stirring for 8 h, 10 mL of γ-AlOOH sol was taken, and 8 g of 10 wt% polyvinyl alcohol was added. The mixture was stirred for 2 h. Finally, the γ-AlOOH sol was smeared on a 2 cm × 6 cm polytetrafluoroethylene plate to form a film, and the film was peeled off after drying at room temperature in static air for 48 h.

[0072] (2) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of γ-AlOOH film sample, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of Cr(VI) by γ-AlOOH film is shown in Figure 2 The adsorption removal rate of Cr(VI) is 77.66%, and the adsorption amount is 19.97 mg / g.

[0073] Embodiment 9:

[0074] In order to compare the adsorption performance of γ-AlOOH / SiO2 composite film and SiO2 film, SiO2 film was also prepared. The relevant steps and adsorption performance test process are as follows:

[0075] (1) 1.6 g of nano-silica powder was uniformly dispersed in 40 g of water at room temperature and stirred for 8 h to obtain SiO2 sol. Then 10 mL of SiO2 sol was stirred with 8 g of 10 wt% polyvinyl alcohol for 2 h, and finally smeared on a 2 cm × 6 cm polytetrafluoroethylene plate for tape casting, and dried at room temperature in static air for 48 h before peeling off the film.

[0076] (2) Adsorption of 50 mL, 50 mg / L Cr(VI) solution: Adjust the pH to 2 with 0.1 mol / L HCl solution, then add 0.1 g of SiO2 film, and set the parameters of the constant temperature oscillation box to 25°C and 150 r / min. The adsorption kinetics curve of SiO2 composite film on Cr(VI) is shown in Figure 2 The adsorption removal rate of Cr(VI) is 82.30%, and the adsorption amount is 20.37 mg / g.

[0077] Embodiment 10:

[0078] In order to detect the acid resistance of the γ-AlOOH / SiO2 composite film, 0.1 g of the film samples in "Example 1", "Example 8" and "Example 9" were taken respectively, added into a solution with 50 mL of HCl solution adjusted to pH = 1, and the parameters of the constant temperature oscillation box were set to 25°C, 150 r / min, and the oscillation time was 5 h.

[0079] The results show that the γ-AlOOH film has a certain toughness, but its mass loss is 28.16%; the mass loss of the SiO2 film is only 3.85%, but the film is very brittle; while the γ-AlOOH / SiO2 composite film does not crack after being pulled and can rebound, while the γ-AlOOH film only loses 12.75% of its mass while retaining good toughness, and its acid resistance stability is significantly enhanced.

[0080] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A γ-AlOOH / SiO for Cr(VI) adsorption 2 Preparation method of composite film, Features The following steps are involved: Firstly, pseudo-boehmite powder is dispersed in water at room temperature, and lactic acid is added to debond the powder to obtain a suspension; Subsequently, the nano-silicon dioxide powder is evenly dispersed in the above suspension, and a film-forming aid polyvinyl alcohol is added, and the composite sol is obtained after being stirred evenly at room temperature; finally, the composite sol is evenly applied on a substrate to be cast, and γ-AlOOH / SiO is obtained after being dried at room temperature. 2 Composite film.

2. The γ-AlOOH / SiO2 for Cr(VI) adsorption according to claim 1 2 Preparation method of composite film, It is characterized in that The mass ratio of the lactic acid to the pseudo-boehmite powder is 0.15-0.75:

1.

3. The γ-AlOOH / SiO2 for Cr(VI) adsorption according to claim 1 2 Preparation method of composite film, It is characterized in that The mass ratio of the lactic acid to the pseudo-boehmite powder is 0.45-0.75:

1.

4. The γ-AlOOH / SiO2 for Cr(VI) adsorption according to claim 1 2 Preparation method of composite film, It is characterized in that The mass ratio of the pseudo-boehmite powder to the nano-silicon dioxide powder is (2-6):1; the mass fraction of the pseudo-boehmite in the suspension is 2-8wt%.

5. The γ-AlOOH / SiO2 for Cr(VI) adsorption according to claim 1 2 Preparation method of composite film, It is characterized in that The added amount of the polyvinyl alcohol is (0.1-0.8 g) polyvinyl alcohol / 10 mL of the composite sol.

6. The γ-AlOOH / SiO2 for Cr(VI) adsorption according to claim 1 2 Preparation method of composite film, It is characterized in that The preparation method specifically comprises the following steps: (1) dispersing 0.8 to 3.2 parts by weight of pseudo-boehmite powder in deionized water at room temperature, and then rapidly adding 0.12 to 2.4 parts by weight of lactic acid to perform debonding; (2) adding 0.133 to 1.6 parts by weight of silicon dioxide powder to the solution obtained in step (1), stirring at room temperature for a certain period of time to obtain a composite sol; (3) Take the composite sol in step (2), add polyvinyl alcohol in a ratio of (0.1-0.8 g) polyvinyl alcohol / 10 mL composite sol, stir for 2 h, and finally γ-AlOOH / SiO 2 The composite sol is coated on a substrate and cast into a film. After drying for 48 hours under static air at room temperature, the film is peeled off to obtain the γ-AlOOH / SiO 2 Composite film.

7. The γ-AlOOH / SiO2 for Cr(VI) adsorption according to claim 1 2 Preparation method of composite film, It is characterized in that The stirring time in step (2) is 8 hours.

8. A γ-AlOOH / SiO prepared by the method according to any one of claims 1 to 7 2 Composite film.

9. The γ-AlOOH / SiO according to claim 8 2 Application of composite films in Cr(VI) adsorption.

Citation Information

Patent Citations

  • Hydrotalcite pseudoboehmite composite film as well as preparation method and application thereof

    CN110711553A

  • Lithium ion battery diaphragm, preparation method thereof and lithium ion battery

    CN113394516A

  • Production of a nano-corundum used in the production of aluminum oxide sintered products uses chlorine-free inorganic precursors as starting material in a liquid medium to form a sol which is subsequently hydrolyzed

    DE19922492A1

  • Platy Ceramic Stacking Organic-Inorganic Composite Coating Method using Sol-Gel Binder with Boehmite Sol and Electrophoretic Deposition

    KR1020160034050A