Nano tungsten oxide and preparation method thereof
By using a specific molar ratio of ammonium tungsten oxide and ammonium chloride to react in hydrogen peroxide during the preparation process of nano-tungsten oxide, and adding propylene glycol for hydrothermal treatment, the uneven particle size distribution of nano-tungsten oxide in the existing technology is solved. Solving the problem of unsatisfactory morphology, we have achieved efficient and controllable preparation of nanometer tungsten oxide, improving its application performance in energy storage, photocatalysis and other fields.
Patent Information
- Application Number
- CN202410971007.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-08
AI Technical Summary
Among the existing methods for producing nanometer tungsten oxide, the solid-phase method is difficult to control the reaction conditions and parameters, resulting in uneven particle size distribution and unsatisfactory morphology. The liquid-phase method has harsh equipment factors and reaction conditions, making it difficult to control the particle size and affecting the nanometer size. Properties and applications of tungsten oxide.
A specific molar ratio of ammonium tungstate and ammonium chloride is used to react in hydrogen peroxide, propylene glycol is added for hydrothermal treatment, and one-dimensional nanotubular tungsten oxide is formed by controlling the roasting temperature and rate to ensure the controllability of the reaction system and the product Efficient preparation.
It achieves efficient and controllable preparation of nano-tungsten oxide, improves the purity and specific surface area of the product, and broadens its application potential in energy storage, photocatalysis, gas sensing and other fields.
Smart Images

Figure CN118745005A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tungsten oxides, and in particular relates to nano tungsten oxide and a preparation method thereof. Background Art
[0002] As an important functional material, nano-tungsten oxide has shown broad application prospects in the fields of energy storage, photocatalysis, gas sensing, etc. The existing methods for producing nano-tungsten oxide include solid-phase method and liquid-phase method. Due to the difficulty in controlling the reaction conditions and parameters of the solid-phase method, the particle size distribution of the obtained nano-tungsten oxide particles is uneven or the morphology is not ideal. Impurities will be introduced or amorphous structures will be produced during the preparation process, affecting the performance and application of nano-tungsten oxide. Its further application in some application fields is limited. Due to equipment factors and harsh reaction conditions, the liquid-phase method is difficult to control the particle size and there are challenges in post-processing, which affects the performance and application of nano-tungsten oxide. Summary of the invention
[0003] The purpose of the present invention is to solve the above-mentioned shortcomings and provide a nano tungsten oxide and a preparation method thereof.
[0004] In the first aspect, a method for preparing nano tungsten oxide adopts the following technical solution:
[0005] A method for preparing nano tungsten oxide comprises the following steps:
[0006] Step 1, mixing and dissolving ammonium tungstate and ammonium chloride, adding hydrogen peroxide to react, and obtaining a tungstate precursor solution;
[0007] Step 2, adding propylene glycol to the tungstate precursor solution, keeping warm and stirring to obtain a sol;
[0008] Step 3, subjecting the sol to a hydrothermal reaction, cooling, solid-liquid separation, and drying to obtain a tungsten oxide precursor;
[0009] Step 4: calcining the tungsten oxide precursor and cooling it to obtain the nano tungsten oxide.
[0010] By adopting the above technical solution, ammonium chloride, NH4 + and Cl - The tungsten oxide crystal nuclei in the reaction system grow along a specific direction to form a one-dimensional product; the organic solvent propylene glycol is adsorbed on the tungstic acid precursor through hydrogen bonds and physical effects, acting as both a co-solvent and a reaction auxiliary agent, selectively controlling the morphology of the tungsten oxide precursor to obtain nano-tubular tungsten oxide, which is then calcined to obtain nano-tungsten oxide.
[0011] Furthermore, in step 1, the molar ratio of ammonium tungstate to ammonium chloride is 1:1 to 1:1.5.
[0012] The specific molar ratio of ammonium tungstate and ammonium chloride helps control the growth of tungsten oxide nuclei in the reaction system and promotes the formation of one-dimensional products, thereby improving the consistency and purity of the products. In addition, it helps to optimize the reaction conditions, improve the reaction efficiency and product performance, and achieve a more efficient and controllable nano-tungsten oxide preparation process, thereby improving the quality and application potential of the final product.
[0013] Furthermore, in step 1, the concentration of hydrogen peroxide is 30wt% to 40wt%, and the molar ratio of the added amount of hydrogen peroxide to ammonium tungstate is 1:1 to 1:1.5.
[0014] As an oxidant, hydrogen peroxide promotes the formation of tungstic acid precursors in the reaction. Appropriate concentration and addition amount can ensure the full progress of the reaction while avoiding excessive side reactions or over-oxidation of the product. This helps to improve the purity and morphology control of the product, thereby improving the performance of nano-tungsten oxide.
[0015] Furthermore, in step 1, the reaction temperature is 75°C to 85°C, and the reaction time is 3.5h to 4.5h.
[0016] The appropriate reaction temperature can accelerate the reaction rate, improve efficiency, and ensure the controllability of the reaction process; ensure that the formation and conversion of the tungstic acid precursor reach the optimal state, thereby affecting the particle size, morphology and performance of the final nano-tungsten oxide, and achieving product consistency and repeatability of the preparation process.
[0017] Furthermore, in step 2, the added amount of propylene glycol is 40wt% to 70wt% of the ammonium tungstate.
[0018] As an organic solvent, propylene glycol can be adsorbed on the tungstic acid precursor through hydrogen bonding and physical action, which helps to control the morphology of the tungsten oxide precursor and promote the formation of nano-tungsten oxide with a specific structure, such as a tubular structure; the appropriate amount of propylene glycol added helps to reduce the presence of impurities and improve the purity of the final nano-tungsten oxide. The amount of propylene glycol added can affect the viscosity and fluidity of the reaction system, thereby optimizing the conditions of subsequent steps such as hydrothermal reaction, which is conducive to the formation and separation of products. By controlling the amount of propylene glycol added, the physical and chemical properties of nano-tungsten oxide, such as specific surface area and pore structure, can be affected.
[0019] Furthermore, in step 2, the insulation temperature is 75° C. to 85° C., and the insulation time is 3 h to 4 h.
[0020] During the heat preservation process, the interaction between the organic solvent propylene glycol and the tungstate precursor helps to control the morphology and structure of the product and promotes the formation of a tubular structure.
[0021] Furthermore, in step 3, the hydrothermal reaction temperature is 150°C to 250°C, and the reaction time is 10h to 12h.
[0022] The hydrothermal reaction is carried out under high temperature and high pressure conditions, which promotes the transformation of tungstate precursor to tungsten oxide and the growth of crystal nuclei. + , Cl - The presence of propylene glycol makes the tungsten oxide crystal nucleus grow along a specific direction to form the desired nano one-dimensional tubular structure.
[0023] Furthermore, in step 4, the heating rate is 4.5°C / min to 5.5°C / min, the calcination temperature is 500°C to 800°C, and the calcination time is 1h to 3h.
[0024] Appropriate calcination temperature and time promote the complete transformation of tungsten oxide precursor to nano tungsten oxide, and improve the crystallinity and purity of the product. The heating rate and calcination temperature affect the morphology of the product, such as maintaining the stability of tubular structure or other one-dimensional structure. The appropriate heating rate helps to reduce the damage of thermal stress to the product, avoid morphological damage and uneven particle size distribution.
[0025] Furthermore, in step 4, the cooling rate is 9.5°C / min to 10.5°C / min.
[0026] The cooling rate helps to reduce the impact of thermal stress on nano-tungsten oxide and prevent crystal defects, morphology damage or internal stress accumulation caused by rapid cooling. Slow cooling helps to promote the improvement of the crystallinity of nano-tungsten oxide and reduce the generation of impurities, thereby improving the purity of the product.
[0027] In the second aspect, a nano tungsten oxide adopts the following technical solution:
[0028] A nano tungsten oxide is prepared by any of the above-mentioned methods for preparing nano tungsten oxide, wherein the particle size of the nano tungsten oxide is 100nm to 300nm.
[0029] The nano tungsten oxide prepared by the above-mentioned preparation method of nano tungsten oxide has a nano particle size, which makes the tungsten oxide have a higher specific surface area, improves the activity of nano tungsten oxide in applications such as catalysis and sensing, and its excellent product performance broadens its application in energy storage, photocatalysis, gas sensing and other fields.
[0030] Beneficial effects of the present invention:
[0031] The preparation method of nano tungsten oxide provided by the present invention accurately controls the reaction conditions, additive ratio and heat treatment steps, improves the purity of nano tungsten oxide and controls its morphology. The prepared nano tungsten oxide has a higher specific surface area and excellent performance, and broadens the application market space of tungsten oxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a photo of the morphology of nano tungsten oxide prepared by the method of Example 1. DETAILED DESCRIPTION
[0033] The following is a further specific description of a nano tungsten oxide and a preparation method thereof described in the present invention in conjunction with an embodiment. For the sake of simplicity of description, this document cannot list all the alternative technical features and implementation schemes contained in the present invention. Therefore, those skilled in the art should know that any technical features and implementation schemes in this embodiment do not limit the scope of protection of the present invention, which includes any alternative technical features and implementation schemes adopted by all those skilled in the art without creative labor. Specifically, the implementation schemes obtained by replacing any technical feature in the present invention or combining any two or more technical features provided by the present invention should be within the scope of protection of the present invention.
[0034] If no specific techniques and conditions are specified in the examples, the procedures are carried out according to the techniques and conditions described in the literature in the art or according to the product instructions. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0035] Example
[0036] Example 1
[0037] Embodiment 1 provides a method for preparing nano tungsten oxide, comprising the following steps:
[0038] Step 1, ammonium tungstate and ammonium chloride are mixed and dissolved in a molar ratio of 1:1, and 40wt% hydrogen peroxide solution is added in a molar ratio of ammonium tungstate to hydrogen peroxide of 1:1 to react at a reaction temperature of 85°C and a reaction time of 3.5h to obtain a tungstic acid precursor solution;
[0039] Step 2, adding propylene glycol to the tungstate precursor solution, wherein the amount of propylene glycol added is 40wt% of ammonium tungstate, and stirring at 85° C. for 4 hours to obtain a sol;
[0040] Step 3, subjecting the sol to a hydrothermal reaction at a temperature of 150° C. for a reaction time of 12 h, cooling, solid-liquid separation, and drying to obtain a tungsten oxide precursor;
[0041] Step 4, calcining the tungsten oxide precursor at 500°C for 3h, with a heating rate of 4.5°C / min, and cooling at a cooling rate of 9.5°C / min to obtain nano tungsten oxide. The morphology of the nano tungsten oxide is shown in FIG. Figure 1 .
[0042] The nano tungsten oxide provided in Example 1 has a purity of 99 wt % and a particle size of 120-290 nm.
[0043] Example 2
[0044] Embodiment 2 provides a method for preparing nano tungsten oxide, comprising the following steps:
[0045] Step 1, ammonium tungstate and ammonium chloride are mixed and dissolved in a molar ratio of 1:1.5, and a 30wt% hydrogen peroxide solution is added in a molar ratio of ammonium tungstate to hydrogen peroxide of 1:1.5 to react at a reaction temperature of 75°C and a reaction time of 4.5h to obtain a tungstic acid precursor solution;
[0046] Step 2, adding propylene glycol to the tungstate precursor solution, wherein the amount of propylene glycol added is 70wt% of ammonium tungstate, and stirring at 75° C. for 3 hours to obtain a sol;
[0047] Step 3, subjecting the sol to a hydrothermal reaction at a temperature of 250° C. for a reaction time of 10 h, cooling, solid-liquid separation, and drying to obtain a tungsten oxide precursor;
[0048] Step 4, calcining the tungsten oxide precursor at 800° C. for 1 h at a heating rate of 5.5° C. / min, and cooling at a cooling rate of 10.5° C. / min to obtain nano tungsten oxide.
[0049] The nano tungsten oxide provided in Example 2 has a purity of 99 wt % and a particle size of 100-270 nm.
[0050] Example 3
[0051] Embodiment 3 provides a method for preparing nano tungsten oxide, comprising the following steps:
[0052] Step 1, ammonium tungstate and ammonium chloride are mixed and dissolved in a molar ratio of 1:1.2, and a 35wt% hydrogen peroxide solution is added in a molar ratio of ammonium tungstate to hydrogen peroxide of 1:1.2 to react at a reaction temperature of 80°C and a reaction time of 4h to obtain a tungstic acid precursor solution;
[0053] Step 2, adding propylene glycol to the tungstate precursor solution, wherein the amount of propylene glycol added is 65wt% of ammonium tungstate, and stirring at 80°C for 3.5h to obtain a sol;
[0054] Step 3, subjecting the sol to a hydrothermal reaction at a temperature of 200° C. for a reaction time of 11 h, cooling, solid-liquid separation, and drying to obtain a tungsten oxide precursor;
[0055] Step 4, calcining the tungsten oxide precursor at 650° C. for 2 h with a heating rate of 5° C. / min, and cooling with a cooling rate of 10° C. / min to obtain nano tungsten oxide.
[0056] The nano tungsten oxide provided in Example 3 has a purity of 99 wt % and a particle size of 150-300 nm.
[0057] Comparative Example
[0058] Comparative Example 1
[0059] Comparative Example 1 provides a method for preparing nano tungsten oxide, which differs from Example 3 in that an equal amount of ammonium chloride is replaced by hydrochloric acid.
[0060] Comparative Example 2
[0061] Comparative Example 2 provides a method for preparing nano tungsten oxide, which differs from Example 3 in that an equal amount of ammonium chloride is replaced by ammonium sulfate.
[0062] Comparative Example 3
[0063] Comparative Example 3 provides a method for preparing nano tungsten oxide, which differs from Example 3 in that an equal amount of hydrogen peroxide is replaced by water.
[0064] Comparative Example 4
[0065] Comparative Example 4 provides a method for preparing nano tungsten oxide, which differs from Example 3 in that an equal amount of propylene glycol is replaced by propylene glycol.
[0066] Comparative Example 5
[0067] Comparative Example 5 provides a method for preparing nano tungsten oxide, which differs from Example 3 in that propylene glycol is replaced by propanol in an equal amount.
[0068] Comparative Example 6
[0069] Comparative Example 6 provides a method for preparing nano tungsten oxide. The difference from Example 3 is that step 2 is not performed in Comparative Example 6, which is as follows:
[0070] A method for preparing nano tungsten oxide comprises the following steps:
[0071] Step 1, ammonium tungstate and ammonium chloride are mixed and dissolved in a molar ratio of 1:1.2, and a 35wt% hydrogen peroxide solution is added in a molar ratio of ammonium tungstate to hydrogen peroxide of 1:1.2 to react at a reaction temperature of 80°C and a reaction time of 4h to obtain a tungstic acid precursor solution;
[0072] Step 2, subjecting the tungstic acid precursor solution to a hydrothermal reaction at a temperature of 200° C. for a reaction time of 11 h, cooling, solid-liquid separation, and drying to obtain a tungsten oxide precursor;
[0073] Step 3, calcining the tungsten oxide precursor at 650° C. for 2 h with a heating rate of 5° C. / min, and cooling with a cooling rate of 10° C. / min to obtain nano tungsten oxide.
[0074] Comparative Example 7
[0075] Comparative Example 7 provides a method for preparing nano tungsten oxide, which differs from Example 3 in that, in step 4, the heating rate is 6.5° C. / min.
[0076] Comparative Example 8
[0077] Comparative Example 8 provides a method for preparing nano tungsten oxide, which is different from Example 3 in that, in step 4, the cooling rate is 15°C / min.
[0078] The purity and particle size of the tungsten oxide prepared by the nano-tungsten oxide preparation methods provided in Example 3 and Comparative Examples 1-8 are shown in Table 1 below.
[0079] Table 1 Purity and particle size of nano tungsten oxide provided by Example 3 and Comparative Examples 1-8
[0080]
[0081] It can be seen from Table 1 that within the theoretical range, the particle size of tungsten oxide increases with the increase of reagent content, hydrogen peroxide affects the particle size, and propylene glycol does not affect the particle size. It mainly improves the morphology and particle dispersion. If the temperature of the autoclave is too low, the particle size of tungsten oxide will increase. The concentration of hydrogen peroxide has the greatest influence on the particle size. Too high or too low concentration will lead to uneven particle size distribution. As long as the time and temperature do not deviate too high, the roasting temperature has little effect on the particle size.
[0082] For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived from them are still within the scope of protection of the claims of the invention.
Claims
1. A method for preparing nano tungsten oxide, characterized in that: The following steps are involved: Step 1, mixing and dissolving ammonium tungstate and ammonium chloride, adding hydrogen peroxide to react, and obtaining a tungstate precursor solution; Step 2, adding propylene glycol to the tungstate precursor solution, keeping warm and stirring to obtain a sol; Step 3, subjecting the sol to a hydrothermal reaction, cooling, solid-liquid separation, and drying to obtain a tungsten oxide precursor; Step 4: calcining the tungsten oxide precursor and cooling it to obtain the nano tungsten oxide.
2. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 1, the molar ratio of ammonium tungstate to ammonium chloride is 1:1 to 1:1.
5.
3. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 1, the concentration of hydrogen peroxide is 30wt% to 40wt%, and the molar ratio of the added amount of hydrogen peroxide to ammonium tungstate is 1:1 to 1:1.
5.
4. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 1, the reaction temperature is 75°C to 85°C, and the reaction time is 3.5h to 4.5h.
5. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 2, the added amount of propylene glycol is 40wt% to 70wt% of the ammonium tungstate.
6. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 2, the insulation temperature is 75° C. to 85° C., and the insulation time is 3 h to 4 h.
7. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 3, the hydrothermal reaction temperature is 150° C. to 250° C., and the reaction time is 10 h to 12 h.
8. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 4, the heating rate is 4.5°C / min to 5.5°C / min, the calcination temperature is 500°C to 800°C, and the calcination time is 1h to 3h.
9. The method for preparing nano tungsten oxide according to claim 1, characterized in that: In step 4, the cooling rate is 9.5°C / min to 10.5°C / min.
10. A nano-tungsten oxide, characterized in that: The nano tungsten oxide is prepared by the preparation method of the nano tungsten oxide according to any one of claims 1 to 9, wherein the particle size of the nano tungsten oxide is 100nm to 300nm.
Citation Information
Cited By
Perovskite solar cell taking alcohol-soluble tungsten oxide as electron transport layer, alcohol-soluble tungsten oxide and preparation method thereof
CN119677292A