Carbonization product production device and preparation method for recovering CO2 and smelting waste residues
By designing a carbonization product production device that recovers CO2 and smelting waste residue, and using wet carbonization process and ultrasonic, stirring, and temperature control technologies, the problems of high cost and poor stability in the carbonization process of metallurgical waste residue are solved, and efficient and low-cost carbonization is achieved. and improved stability, suitable for preparing low-carbon and environmentally friendly gelling materials.
Patent Information
- Application Number
- CN202410744721.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-11
AI Technical Summary
The existing technology in the carbonization process of metallurgical waste residue has high costs, complicated operations, and fails to effectively utilize CO2. It also fails to consider the impact of volume expansion on material stability when the metallurgical waste residue is hydrated.
A carbonization product production device is designed to recover CO2 and smelting waste residue. The metallurgical waste residue is mixed with water through a wet carbonization process. The carbonization reaction is carried out using ultrasonic, stirring and temperature control technology, and is regulated by an integrated CO2 filtration and heat exchange device. Under the reaction conditions, efficient carbonization products are generated, which are then mixed with cement to prepare green cementitious materials.
It achieves efficient carbonization of metallurgical waste residue, reduces production costs, improves the strength and stability of the material, solves the problem of volume expansion during hydration, and can directly utilize CO2 generated by industry, which has the characteristics of low carbon and environmental protection.
Smart Images

Figure HDA0004886062160000011 
Figure HDA0004886062160000012 
Figure HDA0004886062160000013
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of industrial waste resource utilization and carbon neutrality, and specifically relates to a method for efficiently recovering CO 2 A device for producing carbonized products of smelting waste slag and a method for preparing a new type of low-carbon material. Background Art
[0002] my country's metal smelting industry is well developed and ranks among the best in the world. When smelting metals, a large amount of industrial solid waste, smelting slag, is produced. The slag is rich in Ca and Mg mineral phases and may also contain a large amount of heavy metal elements. The accumulation of metallurgical slag not only occupies a large amount of land resources, but also pollutes the surrounding environment. Since cement consumes a lot of energy and emits CO in the production process, 2 It is regarded as a seriously polluting industry and urgently needs to be optimized and upgraded. Metallurgical waste slag contains a large amount of calcium silicate minerals and has the advantages of large reserves and low prices. Applying it in the field of auxiliary cementitious materials can not only solve the problem of industrial solid waste utilization, but also reduce environmental pollution and energy consumption caused by cement production. my country's main energy supply is coal combustion, which produces a large amount of CO 2 , leading to the intensification of the greenhouse effect, which has a significant impact on the environment. 2 Gas emissions, various energy-saving and emission reduction technologies are developing rapidly. From the perspective of building materials, CO 2 Capture, storage and utilization technologies can effectively 2 Sequestered in building materials, reducing CO emissions into the atmosphere 2 The principle is to use carbon dioxide to react with alkaline earth metals to generate stable carbonates, thereby achieving the effect of carbon fixation, which can consume a large amount of CO 2 , and can also optimize the performance of building materials.
[0003] Prior art CN115093138A discloses an additive and its application for magnesium slag-based cementitious materials suitable for silicon thermal magnesium smelting, wherein organic chitosan oligosaccharide is added to magnesium slag to promote the degradation of CaO, β-C 2 S and γ-C 2 S-Ca 2+ The method dissolves the magnesium slag and adds inorganic components such as sodium carbonate or sodium bicarbonate to generate calcium carbonate, thereby ensuring the carbonization reaction of the magnesium slag, improving the strength and dimensional stability of the magnesium slag cementitious material, and its application method ensures the activity of the admixture. Although this method improves the strength and dimensional stability of the magnesium slag cementitious material, the price of the chitosan oligosaccharide used is relatively expensive, which increases the cost of material manufacturing. At the same time, it needs to add sodium carbonate or sodium bicarbonate to ensure the carbonization reaction of the magnesium slag, which further increases the cost, and fails to use CO 2Carbonization is possible. CN113733303A discloses a magnesium slag product, a preparation method and application thereof, and proposes to adjust the cooling rate of the hot magnesium slag, and then regulate the thermal stress to control the pulverization rate of the magnesium slag to 50% to 70%, so that the prepared magnesium slag cementitious material is easier to compact; at the same time, by shortening the contact time between the magnesium slag and water, the hydration of the magnesium slag is inhibited, and the carbonated product of calcium silicate is reduced, so that the magnesium slag cementitious material becomes more dense and its strength is increased, up to 200MPa; however, the hot magnesium slag needs to be temperature-controlled and cooled, and the large amount of waste magnesium slag that has been produced cannot be utilized. If the magnesium slag is heated and cooled again, it is a great waste of energy; therefore, it can only take effect when the magnesium slag is produced, and the existing magnesium slag cannot be processed. CN111892363B discloses a magnesium slag cementitious material and a molding process method thereof, by doping baking soda (NaHCO 3 ) makes the calcium salt in the magnesium slag react with it to form calcium carbonate, thereby improving its compressive strength and reducing the porosity of the sample, making it more compact; however, baking soda needs to be added to the magnesium slag to achieve carbonization, and CO cannot be directly used. 2 There is still room for improvement. CN104478256B discloses a magnesium calcium carbonate cementitious material and its preparation method. The patent uses industrial alkaline waste residue, active magnesium oxide and cement as raw materials, and then uses CO 2 Carbonization is carried out; this method fails to solve the volume expansion change caused by the hydration of magnesium slag, which may have a certain impact on the stability performance of the specimen.
[0004] Most of the above existing technologies add additives to achieve the carbonation process of metallurgical waste slag, but the cost is high and the operation is difficult. The impact of the unique characteristics of each type of solid waste on the test piece during hydration is not considered, and the carbonization conditions are also relatively harsh. These problems need to be solved urgently. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention aims to provide a method for recovering CO 2 The invention discloses a production device and a preparation method for the carbonization product of smelting waste slag. The designed device is used to first modify the metallurgical waste slag by a wet carbonization process, and then filter and dry it, and screen it to a suitable particle size, and finally mix it with cement to prepare a green cementitious material. The prepared metallurgical waste slag cementitious material has the characteristics of high strength, good stability, good carbon fixation performance, low production cost, and low carbon and environmental protection.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0007] A CO recovery 2The carbonization product production device of the smelting waste slag includes a box, a dissolving vessel, a filter screen, a suction bottle, an electronic pump, a steam generator, a temperature control display, an ultrasonic generator, an ultrasonic transducer, a rotor, a speed controller, a pH monitor, a CO 2 Disperser, CO 2 The invention relates to an integrated filtering and heat exchange device; a filter screen is provided at the bottom of the dissolving vessel, and two one-way exhaust valves are provided under the filter screen; the bottom of the dissolving vessel is sealed and connected to a suction filtration bottle through a funnel, a funnel valve is provided on the funnel, and the suction filtration bottle is connected to an electronic pump outside the box; the steam generator is connected to the box body, and the temperature is regulated by controlling the pressure; the temperature control display is arranged below the dissolving vessel; the ultrasonic generator and the ultrasonic transducer are connected by a wire and installed next to the dissolving vessel; the rotor is located in the dissolving vessel, and the speed controller is arranged below the dissolving vessel; the pH monitor is used to monitor the pH value change of the solution in the dissolving vessel; the CO 2 Integrated filtration and heat exchange device including CO 2 Filters and heat exchange fans, CO 2 The filter device is equipped with a one-way exhaust valve to 2 Pipeline connected to CO 2 Diffuser, CO 2 The disperser is located in the dissolving vessel, and the heat exchange fan can regulate the reaction environment temperature according to the heat released by the internal carbonization reaction and the external heat.
[0008] The present invention also includes the following technical features:
[0009] Specifically, the dissolving vessel is cylindrical, and its highest water level is at 1 / 2 of the height of the dissolving vessel. 2 Pipeline and CO 2 The disperser was 1-2 cm from the top of the dissolution vessel.
[0010] Specifically, the filter has an aperture of 50 μm, the filter is close to the bottom of the dissolution vessel, and the one-way exhaust valve under the filter is installed 1 cm below the filter and at 1 / 4 and 3 / 4 of the filter diameter.
[0011] Specifically, the rotor is arranged above the filter screen and is located at 1 / 4 and 3 / 4 of the diameter of the filter screen.
[0012] A method for preparing low-carbon materials by wet carbonization, based on the recovery of CO 2 A device for producing carbonized products of smelting waste slag; comprising the following steps:
[0013] Step 1: Recover CO 2 The carbonization reaction is carried out with the carbonization product production device of smelting waste slag, and the process is carried out in four steps: dissolution, carbonization, filtration and drying:
[0014] First, put the metallurgical waste slag into the dissolving vessel, then add water, set the temperature and stirring speed, and turn on the ultrasonic generator, ultrasonic transducer, steam generator, and speed controller at the same time, stir to disperse the Ca and Mg mineral phases in the metallurgical waste slag in the solution, and wait until the metallurgical waste slag is dispersed in the water;
[0015] Industrial tail gas is passed through CO 2 The integrated filtration and heat exchange device recovers the heat of the exhaust gas, and at the same time regulates the heat release of the internal carbonization reaction, removes toxic gases and purifies CO 2 , and then the filtered CO is blown through the fan 2 Continuously introduce CO into the dissolving vessel from the pipeline 2 Ca and Mg mineral phases are combined with CO 2 Carbon mineralization reaction occurs to generate various carbonization products; the temperature environment of the processing technology is regulated by the heat exchange fan to meet the needs of forming carbonized materials with different crystal forms. After the carbonization reaction is completed, the pH value change of the solution is monitored by the pH monitor to reflect the progress of the carbonization reaction;
[0016] After the carbonization reaction is completed, the rotor, speed controller and steam generator are turned off, and the funnel valve at the bottom of the dissolving vessel and the electronic pump are opened for suction filtration to separate the carbonization product generated by the reaction from the water and leave it on the filter screen;
[0017] Close the funnel valve and the electronic pump at the bottom of the dissolving vessel, and introduce dry hot air to dry the carbonized metallurgical waste slag;
[0018] Step 2, screening the prepared carbonized metallurgical waste slag to an average particle size;
[0019] Step three, using the carbonized metallurgical waste slag obtained in step two to replace cement in equal amount to prepare cementitious material.
[0020] Specifically, in the carbonization process of step 1, CO 2 The diffuser makes CO 2 Disperse evenly in the solution to maintain the overall reaction uniformity of wet carbonization.
[0021] Specifically, in the carbonization process of step 1, an ultrasonic generator and an ultrasonic transducer are used to convert the CaCO generated by the reaction into 3 The silica gel material is vibrated away from the surface of the metallurgical waste slag to reduce the influence of the coating on the carbonization reaction process, thereby continuously producing carbonized material.
[0022] Specifically, the pore size of the filter used for screening the carbonized metallurgical waste slag in step 2 is 50 μm.
[0023] Specifically, the content of the cement substitute in step three is 1%-20%.
[0024] Specifically, in the step three, a cement slurry is prepared using a slurry mixer: water is first added, and then the mixed raw materials are added, with a water-cement ratio of 0.2-0.6; low-speed stirring is first performed for 30 seconds, and then switched to high-speed stirring for 90 seconds; and the slurry is cured and formed under standard curing conditions, with a temperature of 20° C. and a humidity of 95%.
[0025] Compared with the prior art, the present invention has the following technical effects:
[0026] The present invention integrates carbon dioxide recovery, dissolution and dispersion, carbonization, filtration and drying, greatly reducing the cumbersome steps in the actual process, making the wet carbonization of metallurgical waste slag simpler, and the process is simple, the operability is strong, the size and specifications of the equipment can be adjusted according to actual needs, and the adaptability is strong; CO in industrial tail gas can also be used 2 As raw materials for reaction, the cost is greatly reduced.
[0027] The present invention can control the dissolution, dispersion and carbonization conditions during wet carbonization of metallurgical waste slag, and can be carried out under relatively suitable conditions without being affected by the external environment. 2 The disperser and ultrasonic device can ensure the uniformity of the carbonization degree of the metallurgical waste slag and make the produced calcium carbonate and silica gel products fall off from the surface of the metallurgical waste slag through ultrasonic action, reduce the influence on the subsequent carbonization, and obtain a higher carbonization degree.
[0028] The present invention accelerates the carbonization reaction of metallurgical waste slag through the triple effects of ultrasound, stirring and temperature control, and can adjust the real-time parameters of the carbonization reaction to adapt to the CO2 content of various metallurgical solid wastes. 2 The mineralization reaction proceeds and effectively improves the carbonization degree of metallurgical waste slag.
[0029] The present invention can easily achieve the crystal form regulation of the carbonized product by adding the corresponding crystal form regulator to the solution, thereby achieving the production of a more functionalized calcium carbonate product without negatively affecting other systems. This allows the system to directly connect to the production of functionalized calcium carbonate products, greatly improving the application value of the carbonized product.
[0030] The present invention reflects the overall progress of the carbonization reaction by detecting the pH value change in the solution. Magnesium slag itself is alkaline, and the pH value rises to about 12 when dispersed in water. 2 As the mineralization reaction proceeds, the pH value of the solution decreases first and then remains constant. When the pH value of the solution drops below 7, the reaction is considered to be complete (100%).
[0031] The present invention utilizes greenhouse gas CO 2 Used as raw materials, it can consume CO generated in industrial production 2Gas, solidified inside cement products, can be directly connected to industrially produced CO 2 Gas pipelines, prepared into new low-carbon materials, are of great significance in the field of energy conservation and emission reduction.
[0032] Metallurgical waste slag may expand in volume when hydrated, which may cause poor stability of cement products. Carbonizing it first can perfectly solve this defect and enhance its mechanical properties and increase its compressive strength. The present invention fully embodies this point by using carbonized metallurgical waste slag in the preparation of cementitious materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the structure of the device of the present invention.
[0034] Figure 2 It is a process flow chart of the present invention.
[0035] Figure 3 The pH value change curve and fitting diagram during carbonization.
[0036] Figure 4 This is a comparison chart of the compressive strength of cementitious materials.
[0037] The meaning of each number in the figure is:
[0038] 1. One-way exhaust valve, 2. Dissolution vessel, 3. CO 2 Disperser, 4. Rotor, 5. Filter, 6. Box, 7. Steam generator, 8. Ultrasonic transducer, 9. Funnel valve, 10. Temperature control display, 11. Speed controller, 12. Ultrasonic generator, 13. Filter bottle, 14. Electronic pump, 15. pH monitor, 16. CO 2 Integrated filtering and heat exchange device. DETAILED DESCRIPTION
[0039] The present invention provides a method for recovering CO 2 The invention relates to a production device and preparation method for carbonization products of metallurgical waste slag, wherein the metallurgical waste slag is first modified by a wet carbonization process, then filtered and dried, and sieved to a suitable particle size, and finally mixed with cement to prepare a green gelling material; the prepared metallurgical waste slag gelling material has the characteristics of high strength, good stability, good carbon fixation performance, low production cost, low carbon and environmental protection. Specifically, the high-temperature kiln gas generated after the metallurgical waste slag is produced is used, and the waste heat is used to control the process environment by using a heat exchanger; the tail gas components after the calcination of the metallurgical waste slag are filtered, and the CO 2 The gas is recycled and then fed into a wet carbonization device. The smelting slag left over from the smelting process is loaded into the designed intelligent wet carbonization device and dissolved in a solution at a specific water-to-solid ratio. The solution is stirred at the same time so that the Ca and Mg mineral phases in the metallurgical waste slag are dispersed in the solution. The recycled CO is continuously fed into the solution.2 , so that Ca and Mg mineral phases are 2 Carbon mineralization reaction occurs to generate various carbonization products; using CO 2 The diffuser makes CO 2 The CaCO generated by the reaction is dispersed more evenly in water to maintain the overall uniformity of the wet carbonization reaction; the ultrasonic and vibration devices are used to 3 The materials such as silica gel are vibrated away from the surface of the metallurgical waste slag to reduce the influence of the coating on the carbonization reaction process, thereby continuously producing carbonized materials; a pH monitor is used to monitor the reaction process and the amount of reaction products in real time, and the temperature environment of the processing technology is adjusted by a heat exchange fan to meet the needs of the formation of carbonized materials with different crystal forms. The prepared material is filtered, dried, screened and other steps to make the particles evenly dispersed to form a suitable particle size. The prepared wet carbonized metallurgical waste slag product is used to replace cement in an equal amount to prepare a cementitious material. The device of the present invention integrates carbon dioxide recovery, dissolution, carbonization, filtration and drying, can perform wet carbonization modification on metallurgical waste slag, and can achieve the production of functionalized calcium carbonate by adding different crystal form regulators; this device can directly utilize CO generated by industry 2 As a carbonization source, it can be applied to a variety of industrial scenarios; the device has extremely high adaptability, and the scale of the device can be adjusted according to the scale of the industrial site and equipment. The method for making the new low-carbon cementitious material of the present invention, all the experimental raw materials come from the reducing waste slag produced when smelting metals, and the Ca and Mg mineral phases in the metallurgical waste slag are converted into carbonization products by a wet carbonization process, and the new cementitious material is prepared by replacing cement in equal amounts. The method has a simple preparation process, low cost, and high efficiency, allowing the metallurgical waste slag industry to enter a circular and sustainable benign industrial development path. The concrete prepared using the low-carbon cementitious material prepared in this way as a raw material can not only enhance its overall compressive strength and improve mechanical properties, but also enhance the carbon fixation performance of ordinary concrete, which can make a huge contribution to the grand goal of achieving carbon neutrality in concrete.
[0040] like Figure 1 As shown, the present invention recovers CO 2 The carbonized product production device of the smelting waste slag comprises a box 6, a dissolving vessel 2, a filter screen 5, a suction bottle 13, an electronic pump 14, a steam generator 7, a temperature control display 10, an ultrasonic generator 12, an ultrasonic transducer 8, a rotor 4, a speed controller 11, a pH monitor 15, a CO 2 Disperser 3, CO 2Integrated filtering and heat exchange device 16; filter screen 5 is provided at the bottom of dissolving vessel 2, and two one-way exhaust valves 1 are provided under filter screen 5; the bottom of dissolving vessel 2 is sealed and connected to suction bottle 13 through funnel, and funnel valve 9 is provided on the funnel, and suction bottle 13 is connected to electronic pump 14 outside housing 6; steam generator 7 is connected to housing 6, and temperature is regulated by controlling pressure; temperature control display 10 is provided under dissolving vessel 2; ultrasonic generator 12 and ultrasonic transducer 8 are connected by wires and installed beside dissolving vessel 2; ultrasonic transducer 8 is installed at the bottom of the upper half of housing 6, and converts ultrasonic wave into vibration to promote dissolution; ultrasonic generator 12 is installed on control panel, and is responsible for generating ultrasonic wave. Rotor 4 is located in dissolving vessel 2, and speed controller 11 is located under dissolving vessel 2; pH monitor 15 is used to monitor pH value change of solution in dissolving vessel 2; CO 2 Integrated filtration and heat exchange device including CO 2 Filters and heat exchange fans, CO 2 The filter device is equipped with a one-way exhaust valve 1. 2 Pipeline connected to CO 2 Disperser 3, CO 2 The disperser 3 is located in the dissolving vessel 2; CO 2 The filter absorbs other gases through the chemical absorbent inside the device to purify CO 2 The heat exchange fan can adjust the reaction environment temperature according to the heat released by the internal carbonization reaction and the external heat. 2 The integrated filtering and heat exchange device 16 recovers the waste heat of the tail gas and uses it to heat the device environment system again, and absorbs other gases through the chemical absorbent inside the device to purify CO 2 purpose.
[0041] Specifically, the dissolving vessel 2 is cylindrical, and its highest water level is at 1 / 2 of the height of the dissolving vessel 2. 2 Pipeline and CO 2 The disperser 3 is 1-2 cm away from the top of the dissolving vessel. The pore size of the filter screen 5 is 50 μm, and the filter screen 5 is close to the bottom of the dissolving vessel 2. The one-way exhaust valve 1 under the filter screen 5 is installed 1 cm below the filter screen 5 and at 1 / 4 and 3 / 4 of the diameter of the filter screen 5. The rotor 4 is arranged above the filter screen 5 and is located at 1 / 4 and 3 / 4 of the diameter of the filter screen 5.
[0042] This equipment can prepare high-value carbonized products by wet carbonization of metallurgical waste slag, and has a very wide application prospect. For example, it can be directly used to prepare low-carbon cementitious materials, and its performance is better than that of cementitious materials directly prepared from metallurgical waste slag.
[0043] like Figure 2 As shown, the wet carbonization low-carbon material preparation method of the present invention is based on the recovery of CO 2A device for producing carbonized products of smelting waste slag; comprising the following steps:
[0044] Step 1: Recover CO 2 The carbonization reaction is carried out with the carbonization product production device of smelting waste slag, and the process is carried out in four steps: dissolution, carbonization, filtration and drying:
[0045] 1.1 First put the metallurgical waste slag into the dissolving vessel, then add a certain amount of water (mass ratio 1:5-1:10), set the temperature and stirring speed, turn on the ultrasonic generator, ultrasonic transducer, steam generator, speed controller at the same time, stir to disperse the Ca and Mg mineral phases in the metallurgical waste slag in the solution, and continue for a period of time until the metallurgical waste slag is dispersed in the water;
[0046] 1.2 To carbonize metallurgical waste slag, first pass the industrial tail gas through CO 2 The integrated filtration and heat exchange device recovers the heat of the exhaust gas, and at the same time regulates the heat release of the internal carbonization reaction, removes toxic gases and purifies CO 2 , CO 2 A chemical absorbent that can absorb other harmful gases in the exhaust gas is placed in the filter device, and then the filtered CO 2 Continuously pass CO into the dissolution vessel from the pipeline 2 Gas concentration 20%-30%), continuously introducing recycled CO 2 Ca and Mg mineral phases are combined with CO 2 Carbon mineralization reaction occurs to generate various carbonization products; the temperature environment of the processing technology is regulated by the heat exchange fan to meet the needs of the formation of carbonized materials with different crystal forms, and the carbonization reaction is maintained for a long time. The pH value change of the solution is monitored by the pH monitor to reflect the progress of the carbonization reaction; the overall progress of the carbonization reaction is reflected by detecting the pH value change in the solution; magnesium slag itself is alkaline, and the pH value rises to about 12 when dispersed in water; with the CO 2 As the mineralization reaction proceeds, the pH value of the solution decreases first and then remains constant. When the pH value of the solution drops below 7, the reaction is considered to be complete (100%). Figure 3 The actual measured carbonization process (pH value change) changes over time. The carbonization process can be calculated by the following formula:
[0047]
[0048] 1.3 After the carbonization reaction is completed, turn off the rotor, speed controller and steam generator, open the funnel valve at the bottom of the dissolving vessel and the electronic pump for filtration, separate the carbonization product generated by the reaction from the water, and leave it on the filter.
[0049] 1.4 Close the funnel valve and electronic pump at the bottom of the dissolving vessel, turn on the fan to let in dry hot air to dry the carbonized metallurgical waste slag, and the drying temperature is 105℃.
[0050] Step 2, screening the prepared carbonized metallurgical waste slag to an average particle size;
[0051] Step three, using the carbonized metallurgical waste slag obtained in step two to replace cement in equal amount to prepare cementitious material.
[0052] Specifically, in the carbonization process of step 1, CO 2 The diffuser makes CO 2 Disperse evenly in the solution to maintain the overall uniformity of the wet carbonization reaction. In the carbonization process of step 1, an ultrasonic generator and an ultrasonic transducer are used to disperse the CaCO generated by the reaction. 3 The materials such as silica gel are vibrated away from the surface of metallurgical waste slag to reduce the influence of coating on the carbonization reaction process, thereby continuously producing carbonized materials.
[0053] Specifically, the filter mesh used for screening the carbonized metallurgical waste slag in step 2 has an aperture of 50 μm.
[0054] Specifically, the content of cement replacement in step 3 is 1%-20%. When the optimal dosage is 5%, the mechanical properties increase from 46.3MPa to 47.5MPa; when the maximum dosage is 20%, the mechanical properties can still reach 32.7MPa to meet the application requirements, and the cost is reduced by about 15%. In step 3, a cement slurry is prepared using a slurry mixer: first add water, then add the mixed raw materials, with a water-cement ratio of 0.2-0.6; first stir at a low speed for 30s, then switch to high-speed stirring for 90s; cure and shape under standard curing conditions, with a temperature of 20°C and a humidity of 95%.
[0055] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0056] Embodiment 1:
[0057] This embodiment provides a method for preparing a low-carbon material by wet carbonization, comprising the following steps:
[0058] Use of recycled CO 2 The modified metallurgical waste slag processed by the carbonization product production device of the smelting waste slag can replace cement in equal amounts, with a replacement content of 5%; the designed water-cement ratio is 0.4.
[0059] Use a slurry mixer to prepare cement slurry. The mixing system is: first add water, then add the mixed raw materials, first stir at a low speed for 30 seconds, and then switch to high speed for 90 seconds.
[0060] Curing and molding under standard curing conditions: temperature is 20℃ and humidity is 95%.
[0061] Experiments show that the prepared cementitious material has a 1d compressive strength of 15.1MPa, a 3d compressive strength of 27.9MPa, a 7d compressive strength of 44.3MPa, and a 28d compressive strength of 47.5MPa.
[0062] Embodiment 2:
[0063] This embodiment provides a method for preparing a low-carbon material by wet carbonization, comprising the following steps:
[0064] Use of recycled CO 2 The modified metallurgical waste slag processed by the carbonization product production device of the smelting waste slag can replace cement in equal amounts, with a replacement content of 10%; the designed water-cement ratio is 0.4.
[0065] Use a slurry mixer to prepare cement slurry. The mixing system is: first add water, then add the mixed raw materials, first stir at a low speed for 30 seconds, and then switch to high speed for 90 seconds.
[0066] Curing and molding under standard curing conditions: temperature is 20℃ and humidity is 95%.
[0067] Experiments show that the 1d compressive strength of the prepared cementitious material is 13.5MPa, the 3d compressive strength is 26.5MPa, the 7d compressive strength is 36.7MPa, and the 28d compressive strength is 46.9MPa.
[0068] Embodiment 3:
[0069] This embodiment provides a method for preparing a low-carbon material by wet carbonization, comprising the following steps:
[0070] Use of recycled CO 2 The modified metallurgical waste slag processed by the carbonization product production device of the smelting waste slag can replace cement in equal amounts, with a replacement content of 20%; the designed water-cement ratio is 0.4.
[0071] Use a slurry mixer to prepare cement slurry. The mixing system is: first add water, then add the mixed raw materials, first stir at a low speed for 30 seconds, and then switch to high speed for 90 seconds.
[0072] Curing and molding under standard curing conditions: temperature is 20℃ and humidity is 95%.
[0073] Experiments show that the prepared cementitious material has a 1d compressive strength of 9.36MPa, a 3d compressive strength of 20.1MPa, a 7d compressive strength of 29.5MPa, and a 28d compressive strength of 36.7MPa.
[0074] The experiment shows that the compressive strength of the cementitious material prepared in the embodiment is significantly improved. Compared with the sample directly using metallurgical waste slag as the cementitious material, it not only increases the carbon fixation performance, but also has a higher compressive strength than pure cement and the cementitious material directly prepared using metallurgical waste slag. The specific data are as follows: Figure 4 As shown, it can be seen that: when metallurgical waste slag is directly added to prepare cementitious materials, its strength is lower than that of pure cement, and the performance of metallurgical waste slag itself will affect the performance of cementitious materials; after the cementitious materials are prepared with modified metallurgical waste slag, it can be obviously seen that the 3d strength of the prepared composite cementitious materials is the same as that of pure cement, and then the compressive strength of the sample with a modified metallurgical waste slag dosage of 5% has exceeded that of pure cement, proving that the addition of modified metallurgical waste slag can effectively improve the compressive strength of the specimen.
Claims
1. A method for recovering CO 2 and a device for producing carbonized products from smelting waste slag, It is characterized in that Including box, dissolving vessel, filter, suction bottle, electronic pump, steam generator, temperature control display, ultrasonic generator, ultrasonic transducer, rotor, speed controller, pH monitor, CO 2 Disperser, CO 2 The invention relates to an integrated filtering and heat exchange device; a filter screen is provided at the bottom of the dissolving vessel, and two one-way exhaust valves are provided under the filter screen; the bottom of the dissolving vessel is sealed and connected to a suction filtration bottle through a funnel, a funnel valve is provided on the funnel, and the suction filtration bottle is connected to an electronic pump outside the box; the steam generator is connected to the box body, and the temperature is regulated by controlling the pressure; the temperature control display is provided under the dissolving vessel; the ultrasonic generator and the ultrasonic transducer are connected by a wire and installed next to the dissolving vessel; the rotor is located in the dissolving vessel, and the speed controller is provided under the dissolving vessel; the pH monitor is used to monitor the pH value change of the solution in the dissolving vessel; the CO 2 Integrated filtration and heat exchange device including CO 2 Filters and heat exchange fans, CO 2 The filter device is equipped with a one-way exhaust valve to 2 Pipeline connected to CO 2 Diffuser, CO 2 The disperser is located in the dissolving vessel, and the heat exchange fan can regulate the reaction environment temperature according to the heat released by the internal carbonization reaction and the external heat.
2. The CO recovery method according to claim 1 2 and a device for producing carbonized products from smelting waste slag, It is characterized in that The dissolving vessel is cylindrical, and its highest water level is at 1 / 2 of the height of the dissolving vessel. 2 Pipeline and CO 2 The disperser was 1-2 cm from the top of the dissolution vessel.
3. The CO recovery method according to claim 1 2 and a device for producing carbonized products from smelting waste slag, It is characterized in that The filter has an aperture of 50 μm, the filter is close to the bottom of the dissolving vessel, and the one-way exhaust valve under the filter is installed 1 cm below the filter and at 1 / 4 and 3 / 4 of the filter diameter.
4. The CO recovery method according to claim 1 2 and a device for producing carbonized products from smelting waste slag, It is characterized in that The rotor is arranged above the filter screen and is located at 1 / 4 and 3 / 4 of the filter screen diameter.
5. A method for preparing low-carbon materials by wet carbonization, It is characterized in that The method is based on the recovery of CO according to claim 1 2 A device for producing carbonized products of smelting waste slag; comprising the following steps: Step 1: Recover CO 2 The carbonization reaction is carried out with the carbonization product production device of smelting waste slag, and the process is carried out in four steps: dissolution, carbonization, filtration and drying: First, put the metallurgical waste slag into the dissolving vessel, then add water, set the temperature and stirring speed, and turn on the ultrasonic generator, ultrasonic transducer, steam generator, and speed controller at the same time, stir to disperse the Ca and Mg mineral phases in the metallurgical waste slag in the solution, and wait until the metallurgical waste slag is dispersed in the water; Industrial exhaust gas is passed through CO 2 The integrated filtration and heat exchange device recovers the heat of the exhaust gas, and at the same time regulates the heat release of the internal carbonization reaction, removes toxic gases and purifies CO 2 , and then the filtered CO 2 Continuously introduce CO into the dissolving vessel from the pipeline 2 Ca and Mg mineral phases are combined with CO 2 Carbon mineralization reaction occurs to generate various carbonization products; the temperature environment of the processing technology is regulated by the heat exchange fan to meet the needs of forming carbonized materials with different crystal forms. After the carbonization reaction is completed, the pH value change of the solution is monitored by a pH monitor to reflect the progress of the carbonization reaction; After the carbonization reaction is completed, the rotor, speed controller and steam generator are turned off, and the funnel valve at the bottom of the dissolving vessel and the electronic pump are opened for suction filtration to separate the carbonization product generated by the reaction from the water and leave it on the filter screen; Close the funnel valve and the electronic pump at the bottom of the dissolving vessel, and introduce dry hot air to dry the carbonized metallurgical waste slag; Step 2, screening the prepared carbonized metallurgical waste slag to an average particle size; Step three, using the carbonized metallurgical waste slag obtained in step two to replace cement in equal amount to prepare cementitious material.
6. The method for preparing low-carbon material by wet carbonization according to claim 5, It is characterized in that In the carbonization process of step 1, CO 2 The diffuser makes CO 2 Disperse evenly in the solution to maintain the overall reaction uniformity of wet carbonization.
7. The method for preparing low-carbon materials by wet carbonization according to claim 5, It is characterized in that In the carbonization process of step 1, an ultrasonic generator and an ultrasonic transducer are used to convert the CaCO generated by the reaction into 3 The silica gel material is vibrated away from the surface of the metallurgical waste slag to reduce the influence of the coating on the carbonization reaction process, thereby continuously producing carbonized material.
8. The method for preparing low-carbon materials by wet carbonization according to claim 5, It is characterized in that The filter used for screening carbonized metallurgical waste slag in step 2 has an aperture of 50 μm.
9. The method for preparing low-carbon materials by wet carbonization according to claim 5, It is characterized in that The content of the cement substitute in step 3 is 1%-20%.
10. The method for preparing low-carbon materials by wet carbonization according to claim 9, It is characterized in that In the step 3, a cement slurry is prepared using a slurry mixer: water is first added, and then the mixed raw materials are added, with a water-cement ratio of 0.2-0.6; low-speed stirring is first performed for 30 seconds, and then high-speed stirring is performed for 90 seconds; and the slurry is cured and formed under standard curing conditions, with a temperature of 20° C. and a humidity of 95%.
Citation Information
Patent Citations
Method for carbonizing and activating waste concrete recycled micro powder by wet process and application of regenerated micro-powder
CN112125541A
Activation of natural pozzolan and use thereof
CN113490651A
Gas-solid reactor for preparing calcium carbonate by using carbon dioxide
CN115970624A
Carbon sequestration type composite cementing material as well as preparation method and application thereof
CN117069395A
Cited By
Low-carbon preparation method of coal mine underground filling material
CN120289124A
Preparation method of steel slag-based high-density composite composition for balance iron filling