Organic metal porphyrin polymer, preparation method thereof and application of organic metal porphyrin polymer in optical detector
By using organometallic porphyrin polymers as the photoactive layer material, the problems of high fabrication cost and insufficient performance of existing photodetectors have been solved, realizing an organic photodetector with low dark current, high specific detectivity and fast response, meeting the needs of the next generation of photodetectors.
Patent Information
- Application Number
- CN202410730443.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-06
AI Technical Summary
Existing inorganic semiconductor-based photodetectors suffer from problems such as high manufacturing costs, low spectral responsivity, poor compatibility with flexible substrates, and inability to be fabricated on a large scale. Organic semiconductor photodetectors, on the other hand, have disadvantages such as low detectivity and long response time, which cannot meet the needs of next-generation photodetectors.
Organic semiconductor photodetectors are prepared by using organometallic porphyrin polymers as photoactive layer materials and through specific synthesis methods. This includes preparing conductive cathodes, electron transport layers, organic photoactive layers, and transport layers on a substrate. The planar rigid structure of these polymers improves the planarity of the molecular backbone and the intermolecular interactions, thereby enhancing carrier mobility.
An organic photodetector with low dark current, high specific detectivity and fast response was achieved. The dark current density is 1.5×10-11A cm-2, the response current is 0.4A W-1 at 800nm and 0.35A W-1 at 850nm, the specific detectivity exceeds 1.84×1014 Jones, and the response time is as low as 0.5µs.
Smart Images

Figure CN118745241A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organic photoelectricity, and particularly relates to an organic metal porphyrin polymer and a preparation method thereof and application thereof in organic semiconductor electronic devices, particularly organic semiconductor photoelectric detectors. Background Art
[0002] Photodetectors play an indispensable role in real life and are widely used in various fields of civil and military applications, such as imaging, night vision, optical communications, infrared remote sensing, process control, real-time monitoring, safety and security, environmental monitoring, biomedicine, spectroscopy and many other aspects. Compared with thermal detectors, photodetectors have a higher detection rate. At present, photodetectors based on semi-inorganic conductors such as silicon, germanium and III-V compounds have been developed to a relatively mature level. However, photodetectors based on traditional inorganic semiconductor materials have a series of disadvantages such as high preparation cost, low spectral responsivity, poor compatibility with flexible substrates and inability to prepare on a large scale, which cannot meet people's demand for a new generation of photodetectors.
[0003] Organic semiconductors have the advantages of low preparation cost, simple preparation method, large-area preparation, good flexible substrate compatibility, easily adjustable absorption spectrum, high extinction coefficient, etc. Organic semiconductor-based light detection plays a key role in many emerging applications and is expected to overcome the shortcomings of inorganic semiconductor-based light detectors. However, the current organic semi-monomer light detectors have the disadvantages of low specific detection rate and long response time, which limits their development. Summary of the invention
[0004] In order to solve the shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a class of organic metal porphyrin polymers, which have strong spectral absorption characteristics and a wide spectral absorption range. At the same time, due to their large planar rigid structure, they can promote the planarity of the molecular main chain and the interaction between molecules, improve the carrier mobility of organic semiconductors, and then prepare an organic semiconductor photodetector with low dark current, high detection rate and fast response.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned organometallic porphyrin polymer.
[0006] Another object of the present invention is to provide application of the above-mentioned organometallic porphyrin polymer in an organic semiconductor photodetector.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] An organometallic porphyrin polymer, the general structural formula of which is shown below:
[0009]
[0010] In the polymer structure, multiple Rs may be the same or different, and each R independently represents one or more of an H atom, a Cl atom, an F atom, a straight-chain alkyl group with 1-60 carbon atoms, a branched alkyl group with 1-60 carbon atoms, an alkoxy group with 1-60 carbon atoms, and an alkanethio group with 1-60 carbon atoms; n is any natural number greater than 1; in the polymer structure, M represents one of metal elements such as Mn, Fe, Co, Ni, Cu, Zn, and Pd; in the polymer structure, multiple Xs may be the same or different, and each X independently represents one or more of elements such as N, O, S, and Se.
[0011] The present invention also provides a method for preparing the above-mentioned organometallic porphyrin polymer, which comprises the following steps:
[0012] Under the protection of nitrogen or inert gas, 5,15-di-ethynyl metal porphyrin compound and compound A are added to a solvent, and a reflux reaction is carried out in the presence of a catalyst. After the reaction is completed, the reaction is quenched, and then the metal porphyrin polymer is obtained by purification.
[0013] The reaction scheme of the preparation method of the organometallic porphyrin polymer is as follows:
[0014]
[0015] The solvent includes, but is not limited to, one or two of toluene, tetrahydrofuran (THF), triethylamine (Et3N), chloroform (CHCl3), xylene, chlorobenzene (CB), and dichlorobenzene (DCB).
[0016] The catalyst is tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) and cuprous iodide (CuI).
[0017] The reflux reaction time is 10 to 24 hours.
[0018] The quenching reaction refers to adding a hydrochloric acid / methanol mixture to quench the reaction.
[0019] The purification refers to filtering the obtained reaction solution, and removing impurities, ions and small molecular oligomers of the polymer by one or more of Soxhlet extraction, recrystallization and dialysis. Preferably, the obtained reaction solution is filtered, and then the obtained solid is ground into powder and loaded into a filter paper bucket for Soxhlet extraction, and then acetone, petroleum ether and chloroform are used in sequence, and the chloroform extraction solution is collected, concentrated, recrystallized and / or dialyzed 3-5 times to obtain a molecular weight greater than 10 3 Organometallic porphyrin polymers from Da.
[0020] The present invention also provides an application of a metal porphyrin-based polymer in preparing an organic semiconductor photodetector, comprising the following steps:
[0021] (1) preparing a conductive cathode on a substrate;
[0022] (2) preparing an electron transport layer on the conductive cathode;
[0023] (3) preparing an organic photoactive layer thin film on the electron transport layer;
[0024] (4) A MoO3 transport layer and a Ag anode are sequentially deposited on the organic photoactive layer.
[0025] The organic photoactive layer film described in step (3) is composed of the above-mentioned metalloporphyrin-based polymer and receptor material.
[0026] Furthermore, the substrate in step (1) is at least one of glass, polyvinyl alcohol (PVA), polyester (PET), polyimide (PI), polyethylene naphthalate (PEN), and polydimethylsiloxane (PDMS) film, and its thickness is 0.5 to 1.5 mm.
[0027] Furthermore, the conductive cathode in step (1) is at least one of indium tin oxide ITO and fluorine tin oxide FTO, and its thickness is 100 to 300 nm.
[0028] Furthermore, the electron transport layer in step (2) is ZnO with a thickness of 30 to 50 nm.
[0029] Furthermore, the organic photoactive layer in step (3) is prepared by mixing the metal porphyrin polymer donor and the non-fullerene acceptor in a mass ratio of 1:(1-1.5) (preferably 1:1, 1:1.2, 1:1.5), dissolving them in an organic solvent, and preparing a thin film by spin coating, and annealing to remove the organic solvent to obtain the photoactive layer. The organic solvent is one of chloroform, chlorobenzene, toluene, o-xylene, and p-xylene.
[0030] During the dissolution process of step (3), a suitable solvent additive may be added to improve the solubility of the material so as to obtain a better film morphology, wherein the solvent additive is at least one of 1,8-diiodooctane (DIO), 1,8-dibromooctane (DIO), pyrrole, and pyridine;
[0031] The non-fullerene acceptor is selected from one of the following structures:
[0032]
[0033] In the non-fullerene acceptor structure, R may be the same or different, and R independently represents one or more of an H atom, a straight-chain alkyl group with 1-60 carbon atoms, a branched-chain alkyl group with 1-60 carbon atoms, and an alkoxy group with 1-60 carbon atoms.
[0034] The thickness of the MoO3 transport layer in step (4) is 5 to 50 nm; the thickness of the Ag anode is 80 to 180 nm.
[0035] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0036] (1) The organic photodetector of the present invention has a low dark current. At an operating voltage of -0.1 V, a 1.5×10 -11 Acm -2 The dark current density is 0.4 AW at 800 nm. -1 , the response current at 850nm is 0.35AW -1 , the device achieved more than 1.84×10 14 Jones's specific detection rate and response time are as low as 0.5us. The invention constructs an organic photodetection device with low dark current, high specific detection rate and fast response.
[0037] (2) Compared with similar detectors, the organic photodetector of the present invention has a higher detection rate and a shorter response time, and has great application prospects in future research and engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 1 is a device structure of an organic photodetector in an embodiment.
[0039] Figure 2 is the H of polymer P1 1 -NMR spectrum.
[0040] Figure 3 This is an atomic force microscope photograph of the blend film of P1 polymer donor material and L8-BO acceptor material.
[0041] Figure 4 This is a diagram showing the dark current test results of the organic photodetector of the present invention.
[0042] Figure 5 This is a graph showing the EQE test results of the organic photodetector of the present invention.
[0043] Figure 6 This is a graph showing the specific detectivity test results of the organic photodetector of the present invention.
[0044] Figure 7This is a graph showing the responsivity test results of the organic photodetector of the present invention.
[0045] Figure 8 This is a graph showing the response time test results of the organic photodetector of the present invention.
[0046] Fig. 9 is the -3dB cutoff frequency of the organic photodetector of the present invention. DETAILED DESCRIPTION
[0047] The present invention is further described in detail below in conjunction with examples and drawings, but the embodiments of the present invention are not limited thereto.
[0048] Unless otherwise specified, the reagents used in the examples can be purchased from the market.
[0049] Example 1
[0050] Preparation of Metalloporphyrin-Based Polymers
[0051] (1) Preparation of 5-(2-ethylhexylthio)thiophene-2-carboxaldehyde
[0052]
[0053] First, under nitrogen protection, 1g thiophene (0.5g, 6.0mmol) was placed in a 250ml two-necked bottle, and 60ml of THF was added to dissolve it. It was transferred to a -78℃ cryostat, stirred for 15min, and then n-BuLi (1.6M concin hex, 3.8mL) was slowly added dropwise and stirred for 30min, and then transferred to an ice bath, 0.2g of sulfur powder was added and stirred, and after the reaction liquid turned from turbid to transparent, 6.0mmol 1-bromo-2-ethylhexane was added and continued to stir for 2h. Then it was washed with water, extracted with n-hexane, the organic solution was collected and concentrated, and the crude product was separated by column chromatography, and the eluent was n-hexane, and 1.24g of colorless transparent oily liquid was obtained, with a yield of 90%.
[0054] Then, under nitrogen protection, the obtained 2-(2-ethylhexylthio)thiophene (1.2 g, 4.4 mmol) was transferred into a 100 mL two-necked bottle, and the solution was evacuated and filled with nitrogen three times; then, N,N-dimethylformamide (DMF) (4.3 mL, 1 equiv.) and 1,2-dichloroethane (25 mL, 0.15 M conc) were added, and the mixture was stirred evenly; then, POCl3 (4.1 mL, 1 equiv.) was slowly added dropwise under ice bath conditions, and stirred in a nitrogen atmosphere for 1 h; then, the reaction mixture was moved to an oil bath, heated to 60°C and stirred overnight, and the reaction was tracked using a thin layer chromatography plate; then, after the reaction was complete, the mixture restored to room temperature was poured into ice water and stirred, neutralized with a NaHCO3 aqueous solution, extracted with n-hexane, dried with anhydrous MgSO4, the solvent was removed, and freeze-dried to obtain a yellow solid, which was directly subjected to the next step of reaction without further purification.
[0055] (2) Preparation of Compound 1
[0056] First, dipyrromethene (DPM) (0.645 g, 4.4 mmol) and 5-(2-ethylhexylthio)thiophene-2-carboxaldehyde (1.87 g, 4.4 mmol) were placed in a 2 L reaction bottle, and 1.5 L of DCM was added to dissolve them, and nitrogen was bubbled for 30 mins; then, trifluoroacetic acid (TFA) (33.5 μL, 0.43 mmol) was added, and stirred overnight at room temperature under a nitrogen atmosphere with shielding; then, 2,3-dichloro-5,6-dicyanobenzoquinone (DDQ) (1.51 g, 6.61 mmol) was added all at once and the reaction mixture was stirred for 1 to 2 h; then, triethylamine (NEt3) (5 mL) was added to quench the reaction; finally, the solvent was evaporated, and the crude product was purified by silica gel chromatography to obtain 2.2 g of a purple solid product with a yield of about 65.5%.
[0057] (3) Preparation of Compound 2
[0058] First, compound 1 (1.53 g, 2.0 mmol), NBS (0.75 g, 4.2 mmol) and pyridine (0.1 mL) were added to DCM (200 mL) and stirred at 0°C for 30 mins. TLCs were used to track the progress of the reaction. After the reaction was complete, 5 mL of acetone was added and the solvent was removed in vacuo. Finally, the crude product was purified by silica gel chromatography to obtain 1.75 g of a purple solid product with a yield of approximately 95.1%.
[0059] (4) Preparation of Compound 3
[0060] Compound 2 (1.38 g, 1.5 mmol) was dissolved in CHCl3 (200 mL); then, zinc acetate (1.0 g, 4.5 mmol) dissolved in methanol (20 mL) was added, and the reaction was refluxed for 4 h, and the solution changed from purple-red to green. After the reaction was completed by TLC tracking, the crude product was purified by silica gel chromatography; about 1.37 g of a solid product with a purple metallic luster was obtained, and the yield was about 90%.
[0061] (5) Preparation of Compound 4
[0062] First, the product compound 3 (1.37 g, 1.35 mmol) in the previous step was placed in a 100 mL two-necked reaction bottle, and CuI (11.7 mg, 0.1 eq), Pd(PPh3)4 (21.52 mg, 0.05 eq) and a stirrer were added; then, a rubber stopper was connected to one end of the reaction bottle, and a condenser and a double-row tube were connected to the other end, and the reaction bottle was evacuated and filled with nitrogen (operation three times); then, 15 mL of THF and 15 mL of NEt3 were added to the reaction bottle in sequence, and stirred evenly. Next, 0.3 mL of trimethylsilyl acetylene (TMSA) was slowly added dropwise to the reaction bottle under ice bath conditions using a syringe, the temperature in the reaction container was slowly raised to 65°C (reacted overnight), and the reaction was tracked in real time by MOLIT-TOF. After the raw materials reacted completely, the reaction was stopped and the system was allowed to return to room temperature; then, the reaction solution was poured into 50 mL of water, extracted with DCM (30 mL×3), the lower organic phase was collected, dried over anhydrous magnesium sulfate, filtered, and the solvent was spin-dried; finally, the crude product was passed through a column to obtain 945 mg of the product with a yield of approximately 70%.
[0063] (6) Preparation of Compound 5 (5,15-bis-ethynyl-10,20-bis(5-ethylhexylthiophene[3,2-b]thiophene-2-yl)zinc porphyrin)
[0064] First, compound 4 (0.923 g, 0.88 mmol) was placed in a reaction flask, and 30 mL of THF was added to dissolve it. Then, Bu4NF (1 M / THF, 7.5 mL) was slowly added dropwise to the reaction flask under nitrogen protection, and the mixture was stirred at room temperature for 1.5 h. Next, the solution was poured into 50 mL of water, extracted with DCM, and dried by spin drying. Finally, the crude product was separated by column to obtain 477 mg of a yellow viscous liquid with a yield of about 60%.
[0065] (7) Preparation of Metalloporphyrin-Based Polymer (P1)
[0066] Weigh the pre-synthesized compound 5 and compound 1,3-bis[(5-bromo-4-(2-ethylhexyl)thiophene-2-yl]-5,7-bis(2-ethylhexyl)benzo[1,2-C:4,5-C']dithiophene-4,8-dione (BBDT), weigh equal molar amounts of compound 5 and BBDT respectively and add them into a test tube under argon protection, add a small magnetic rotor, add catalytic amounts of Pd(PPh3)4 and CuI, and add equal volumes of THF and Et3N through a syringe, evacuate under liquid nitrogen protection, return to room temperature, and then fill with argon. Repeat the operation more than three times to ensure that the air in the reaction tube is completely replaced by argon. Seal the reaction tube after returning to room temperature, then transfer it to an oil bath and stir. After the reactants are dissolved, slowly heat it to reflux, observe the reaction progress (about 18 hours), and after the reactants are basically consumed, add hydrochloric acid / methanol to quench the reaction. Filter the resulting reaction solution, then grind the resulting solid into powder and put it into a filter paper bucket for Soxhlet extraction, and use acetone, petroleum ether, and chloroform in turn. Collect the chloroform extraction solution, concentrate it, and dialyze it 3-5 times to obtain a molecular weight of 1.5×10 4 The metalloporphyrin-based polymer of Da was dried in a vacuum oven.
[0067] The chemical reaction equation for synthesizing metalloporphyrin-based polymers is shown below:
[0068]
[0069] Example 2
[0070] Preparation of organic semiconductor photodetectors
[0071] (1) Solution preparation: The metal porphyrin-based polymer donor material and the non-fullerene acceptor material are mixed in a mass ratio of 1:1.2, dissolved in chloroform to a total mixed concentration of 16 mg / ml, heated and stirred at 50°C for 2 h, and finally a uniform solution without precipitation is obtained for use. The molecular structure of the non-fullerene (L8-BO) acceptor material is shown below:
[0072]
[0073] (2) Cleaning of ITO glass substrate: The ITO glass substrate was ultrasonically cleaned in acetone, ethanol, isopropanol, deionized water and isopropanol in an ultrasonic bath for 10 minutes in sequence to remove dust, glass debris and grease that may be attached to the surface. The cleaned ITO glass was transferred to a room temperature blast oven, heated to 70°C, and dried for more than two hours. The dried ITO glass substrate was placed in a clean glass petri dish with the ITO side facing up, and the surface was treated with a plasma oxygen plasma cleaner for 2 minutes.
[0074] (3) Preparation of ZnO film of cathode transport layer: 2g zinc acetate, 550μl ethanolamine, 20ml ethylene glycol methyl ether and 5μl 37% PEIE aqueous solution were heated and stirred at 60℃ for 9 hours to obtain a preliminary solution of zinc oxide. Let it stand for 20-30mins to return to room temperature. Use a syringe to take out an appropriate amount of solution and filter it with a 0.45μm polytetrafluoroethylene filter. Drop the prepared solution on the ITO substrate after plasma treatment, and deposit it on the ITO surface by a sizing machine at 3000rpm to obtain a ZnO film layer with a thickness of about 45nm.
[0075] (4) The ITO substrate after spin coating of ZnO was placed on a hot plate and annealed at 150° C. for 15 mins, then transferred to a nitrogen glove box and spin coated with an organic active layer after cooling.
[0076] (5) Spin coating of photoactive layer: The solution was prepared as described in (1) above. The preparation process of the photoactive layer was carried out in a nitrogen-protected glove box: a 200 nm thick bulk heterojunction layer was spin coated on the ZnO layer using chloroform solution in a ratio of donor:acceptor = 1:1.2 (wt:wt), and then thermally annealed at 100°C for 10 mins.
[0077] (6) Scraping and evaporation of electrodes: The edge of the device coated with the active layer is cut off, leaving only a small strip of ITO. The side that is not spin-coated with ZnO and the organic functional layer is placed face up in the mask basket of the evaporation chamber, and vacuum is drawn until the pressure in the evaporation chamber is less than 1×10 -4 After Pa, MoO3 / Ag electrodes were deposited in sequence by thermal evaporation. The thickness of MoO3 was 20nm and the thickness of Ag was 100nm. The effective area of the device was 0.0516cm 2 .
[0078] (7) Device encapsulation: Apply an appropriate amount of epoxy resin on the top of the device, cover it with a glass sheet and encapsulate the device between two layers of glass to isolate it from water and oxygen, leaving the electrode pins exposed for testing, and finally cure it with a UV curing device for 2 minutes.
[0079] Figure 1 The device structure of the organic photodetector is composed of substrate material / ITO / ZnO / photoactive layer / MoO3 / Ag. The electron transport layer is ZnO, the thickness of MoO3 is 20nm, and the active layer is a blended film of metal porphyrin-based polymer donor material and non-fullerene acceptor material, and the thickness of the active layer is 200nm.
[0080] Figure 2 H of P1 polymer 1 -NMR spectrum, the results show that the molecular structure of the material is the target molecule.
[0081] Figure 3This is an atomic force microscope photograph of the blend film of the P1 polymer donor material and the L8-BO acceptor material. The root mean square roughness (RMS) of the surface morphology is 2.0 nm, indicating that the blend film has a relatively smooth surface.
[0082] Figure 4 The dark current test result of the bulk heterojunction organic photodetector of the present invention with the active layer of P1 polymer donor material and non-L8-BO acceptor material is shown in the figure. At an operating voltage of -2.0V, the photodetector device achieved a dark current of less than 10 -9 Acm -2 The dark current density.
[0083] Figure 5 This is a graph showing the EQE test results of the organic photodetector of the present invention. The external quantum efficiency in the range of 350nm-850nm exceeds 50%, indicating that the active layer material has a very wide spectral response range.
[0084] Figure 6 This is a graph showing the test results of the specific detection rate of the organic photodetector of the present invention under different spectra.
[0085] Figure 7 This is a graph showing the responsivity test results of the organic photodetector of the present invention under different spectra.
[0086] Figure 8 This is a graph showing the response time test results of the organic photodetector of the present invention, wherein the on and off response times are 0.5us and 2.0us respectively.
[0087] Fig. 9 is the -3dB cutoff frequency of the organic photodetector of the present invention.
[0088] At an operating voltage of -0.1 V, the photodetector device achieved a 10 -11 A cm -2 For incident light with a wavelength of 850nm, the device has a specific detection rate of 10 14 Jones, the spectral responsivity is 0.35A / W, and the cutoff response frequency of the photodetector is about 1.2MHz.
[0089] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the present invention should fall within the scope of the present invention.
Claims
1. An organometallic porphyrin polymer, characterized in that Its general structure is shown below: The R are the same or different, and each R independently represents one or more of an H atom, a Cl atom, an F atom, a straight-chain alkyl group with 1 to 60 carbon atoms, a branched-chain alkyl group with 1 to 60 carbon atoms, an alkoxy group with 1 to 60 carbon atoms, and an alkanethio group with 1 to 60 carbon atoms; Said n is any natural number greater than 1; The M represents one of Mn, Fe, Co, Ni, Cu, Zn, and Pd; The X's are the same or different, and each X is independently one or more of N, O, S, and Se.
2. The organometallic porphyrin polymer according to claim 1, characterized in that Its structure is as follows: The n is any natural number greater than 1.
3. A method for preparing an organometallic porphyrin polymer according to claim 1 or 2, characterized in that The following steps are involved: Under the protection of nitrogen or inert gas, 5,15-di-ethynyl metal porphyrin compound and compound A are added to a solvent, and a reflux reaction is carried out in the presence of a catalyst. After the reaction is completed, the reaction is quenched, and then the metal porphyrin polymer is obtained by purification; The reaction scheme of the preparation method of the organometallic porphyrin polymer is as follows: The definitions of R, X, M and n in the reaction scheme are the same as those in claim 1 or 2.
4. The method for preparing an organometallic porphyrin polymer according to claim 3, characterized in that: The solvent is one or two of toluene, tetrahydrofuran, triethylamine, chloroform, xylene, chlorobenzene and dichlorobenzene; The catalyst is tetrakis(triphenylphosphine)palladium and cuprous iodide; The reflux reaction time is 10 to 24 hours; The purification refers to filtering the obtained reaction solution, removing polymer impurities, ions and small molecule oligomers by one or more of Soxhlet extraction, recrystallization and dialysis to obtain a polymer with a molecular weight greater than 10 3 Organometallic porphyrin polymers from Da.
5. Use of the organometallic porphyrin polymer according to claim 1 or 2 in the preparation of an organic semiconductor photodetector.
6. An organic semiconductor photodetector, characterized in that Prepared by the following method: (1) preparing a conductive cathode on a substrate; (2) preparing an electron transport layer on the conductive cathode; (3) preparing an organic photoactive layer thin film on the electron transport layer; (4) depositing a MoO3 transport layer and a Ag anode on the organic photoactive layer in sequence; The organic photoactive layer film described in step (3) is composed of the metal porphyrin-based polymer described in claim 1 or 2 and a receptor material.
7. The organic semiconductor photodetector according to claim 6, characterized in that: The substrate in step (1) is at least one of glass, polyvinyl alcohol, polyester, polyimide, polyethylene naphthalate, and polydimethylsiloxane film, and has a thickness of 0.5 to 1.5 mm; The conductive cathode in step (1) is at least one of indium tin oxide (ITO) and fluorine tin oxide (FTO), and has a thickness of 100 to 300 nm; The electron transport layer in step (2) is ZnO with a thickness of 30 to 50 nm; The thickness of the MoO3 transport layer in step (4) is 5 to 50 nm; the thickness of the Ag anode is 80 to 180 nm.
8. The organic semiconductor photodetector according to claim 6, characterized in that: The organic photoactive layer in step (3) is prepared by mixing a metal porphyrin polymer donor and a non-fullerene acceptor according to claim 1 or 2 in a mass ratio of 1: (1-1.5), dissolving them in an organic solvent, preparing a thin film by spin coating, and annealing to remove the organic solvent to obtain the photoactive layer.
9. The organic semiconductor photodetector according to claim 6, characterized in that: The non-fullerene acceptor is selected from one of the following structures: In the non-fullerene acceptor structure, R is the same or different, and each R relatively independently represents one or more of an H atom, a straight-chain alkyl group with 1-60 carbon atoms, a branched-chain alkyl group with 1-60 carbon atoms, and an alkoxy group with 1-60 carbon atoms.
10. The organic semiconductor photodetector according to claim 6, characterized in that: The organic solvent is one of chloroform, chlorobenzene, toluene, o-xylene and p-xylene; During the dissolution process of step (3), a suitable solvent additive is also added to improve the solubility of the material, and the solvent additive is at least one of 1,8-diiodooctane, 1,8-dibromooctane, pyrrole, and pyridine.
Citation Information
Patent Citations
Metalloporphyrin-quinoxaline organic semiconductor material and preparation method and application thereof
CN102443141A
Osmium-containing conjugated polymer as well as preparation method and application thereof
CN112745485A
High-specific-detection-rate optical detection device and preparation method thereof
CN114784189A
Porphyrin compound and its manufacturing method, organic semiconductor film and its manufacturing method, and semiconductor device and its manufacturing method
JP2006182710A