Polyester waste cloth regenerated fiber and preparation method thereof
Through the combination technology of ethylene glycol, alcoholysis catalyst and antimony catalyst, combined with alcohol ethers and anionic dispersants, the viscosity and spinnability problems affected by impurities in polyester waste fabrics are solved, and the generation of high-quality regenerated fibers is achieved. and stability improvements.
Patent Information
- Application Number
- CN202410801253.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of waste polyester regeneration, and more specifically, to a polyester waste cloth regenerated fiber and a preparation method thereof. Background Art
[0002] With the increasing demand for textiles, a large amount of polyester waste fabrics has gradually increased. How to deal with these waste fabrics efficiently and environmentally friendly has gradually aroused people's thinking. Traditional treatment methods such as landfill and incineration are prone to cause environmental pollution and occupy land resources.
[0003] At present, the recycling methods of waste fabric textiles mainly include chemical method and physical method. At present, the physical method is mainly used to melt-spin waste fabric textiles using screws. However, due to the high impurity content in the waste fabrics, the viscosity and spinnability of polyester products are unstable, and even the quality of polyester is too low to be spun. Summary of the invention
[0004] In order to improve the quality of recycled fibers from polyester waste fabrics, the present application provides recycled fibers from polyester waste fabrics and a preparation method thereof.
[0005] In the first aspect, the present application provides a polyester waste cloth regenerated fiber, using the following technical solution: A polyester waste cloth regenerated fiber comprises the following raw materials in parts by weight: 40-50 parts of polyester waste cloth, 80-120 parts of ethylene glycol, 0.03-0.05 parts of alcoholysis catalyst, 0.01-0.03 parts of antimony catalyst, 0.005-0.008 parts of heat stabilizer, and 15-25 parts of dispersant; the dispersant is at least one of an anionic dispersant and an alcohol ether dispersant.
[0006] By adopting the above technical scheme, ethylene glycol, alcoholysis catalyst and antimony catalyst can be used to depolymerize the macromolecular chains in polyester waste cloth into polymerized monomers, which are then purified and then centrally polymerized to obtain regenerated fibers with higher stability. The waste cloth is alcoholyzed to remove oligomers and impurities using an alcoholysis catalyst, and the antimony catalyst is used to promote the polycondensation reaction of polyester fibers, so that the molecular weight and viscosity of the formed regenerated fibers are improved, thereby obtaining regenerated fibers with better quality and higher strength. Alcohol ether dispersants can promote more uniform dispersion of regenerated fibers, reduce entanglement between regenerated fibers, and improve the spinnability and quality of regenerated fibers. Alcohol ether dispersants and anionic dispersants can be adsorbed on the surface of regenerated fibers to form a protective film, enhance the negative charge on the fiber surface, promote repulsion between fibers, and reduce the agglomeration rate of regenerated fibers.
[0007] Preferably, the dispersant is a mixture of an anionic dispersant and an alcohol ether dispersant, and the mass ratio of the anionic dispersant to the alcohol ether dispersant is (1-1.5):1.
[0008] Preferably, the anionic dispersant is at least one of sodium dodecylbenzene sulfonate, sodium hexametaphosphate, and fatty alcohol ether phosphate, and the alcohol ether dispersant is at least one of polyoxyethylene alcohol, fatty alcohol polyoxyethylene ether, and alkylphenol polyoxyethylene ether.
[0009] By adopting the above technical solution, sodium dodecylbenzene sulfonate, sodium hexametaphosphate, and fatty alcohol ether phosphate salts can be adsorbed on the surface of the regenerated fiber as dispersants to form a protective film, prevent mutual attraction between fibers, reduce the phenomenon of regenerated fiber agglomeration, and promote the regenerated fiber to maintain a good dispersion state. Alcohol ether dispersants can maintain the stable dispersion state of the regenerated fiber, reduce flocculation, and can emulsify and remove the grease and wax on the surface of the regenerated fiber, improve the spinnability of the regenerated fiber, reduce the mechanical damage of the regenerated fiber, and improve the quality stability of the regenerated fiber.
[0010] Preferably, the alcoholysis catalyst is a metal salt catalyst or a metal oxide catalyst.
[0011] By adopting the above technical scheme, metal salt catalysts and metal oxide catalysts are used as alcoholysis catalysts, which can accelerate the alcoholysis reaction of polyester fibers, selectively break the ester bonds in polyester fibers, reduce the occurrence of side reactions, improve the conversion rate and spinnability of fibers, promote more polymers to be effectively decomposed, and reduce the impact of fiber impurities.
[0012] Preferably, the metal salt catalyst is one of sodium acetate, sodium carbonate and zinc acetate.
[0013] Preferably, the antimony-based catalyst is one of antimony acetate, antimony glycol, and antimony trioxide.
[0014] By adopting the above technical solution, antimony acetate, antimony glycol, and antimony trioxide as antimony catalysts can promote the rupture of ester bonds on polyester molecular chains, converting macromolecular polyester into reusable small molecular monomers, which is beneficial to the production of regenerated fibers and improves the spinnability of regenerated fibers. At the same time, antimony acetate, antimony glycol, and antimony trioxide can selectively act on the ester bonds of polyester molecular chains, reduce the generation of side reactions, improve reaction efficiency, and promote the production of regenerated fibers.
[0015] Preferably, the heat stabilizer is one of triethyl phosphonoacetate, phosphoric acid, and triethyl phosphate.
[0016] By adopting the above technical solution, triethyl phosphonoacetate, phosphoric acid, and triethyl phosphate as heat stabilizers can absorb free radicals generated in high-temperature reactions, reduce thermal degradation of polyester fibers during melting and high-temperature processing, improve the stability of the molecular structure of polyester fibers, and thus promote the generation of regenerated fibers. At the same time, the heat stabilizer has high oxidation resistance, reduces the reaction of polyester fibers with oxygen at high temperatures, improves the fluidity of molten polyester, and enhances the spinnability of regenerated fibers.
[0017] In a second aspect, the present application provides a method for preparing recycled fibers from polyester waste fabrics, using the following technical solution: A method for preparing recycled fibers from polyester waste fabrics comprises the following specific steps: The polyester waste fabric is washed and dried in advance, crushed after plasma treatment, melted after crushing to obtain a melt mixture, and then the melt mixture is filtered and mixed with a dispersant, ethylene glycol, and an alcoholysis catalyst, and heated to react to obtain a pre-alcoholysis mixture, and then the pre-alcoholysis mixture is mixed with an antimony catalyst, heated to react, and spun to obtain regenerated fibers.
[0018] By adopting the above technical scheme, the polyester waste fabric can be fully activated by plasma treatment in advance, and the activated small molecular impurities can be separated by subsequent filtration, thereby improving the purity of the polyester fiber, thereby improving the efficiency of subsequent reactions, promoting the generation of regenerated fibers, and improving the viscosity and spinnability of the regenerated fibers.
[0019] Preferably, the heating temperature is 200-275°C.
[0020] In summary, this application has the following beneficial effects: 1. Since the present invention uses ethylene glycol, alcoholysis catalyst and antimony catalyst to break the ester bond of polyester fiber, remove oligomers and impurities, increase the molecular weight and viscosity of the regenerated fiber, and enhance the spinnability of the regenerated fiber, the compounding of anionic dispersant and alcohol ether dispersant can reduce the entanglement between regenerated fibers, improve the fluidity of the regenerated fiber melt, reduce the fiber agglomeration rate, and improve the spinnability of the fiber.
[0021] 2. In the present application, metal salt catalysts and metal oxide catalysts are preferably used as alcoholysis catalysts to accelerate the alcoholysis reaction of polyester fibers, reduce the occurrence of side reactions, and promote the generation of regenerated fibers. DETAILED DESCRIPTION
[0022] The present application is further described in detail below with reference to the embodiments. Example
[0023] Example 1 This embodiment provides a polyester waste cloth regenerated fiber, including the following raw materials in parts by weight: 45 kg polyester waste cloth, 100 kg ethylene glycol, 0.04 kg alcoholysis catalyst, 0.02 kg antimony catalyst, 0.007 kg heat stabilizer, and 20 kg dispersant, wherein the alcoholysis catalyst is sodium acetate, the antimony catalyst is antimony acetate, the heat stabilizer is triethyl phosphonoacetate, and the dispersant is sodium dodecylbenzene sulfonate anion dispersant.
[0024] The method for preparing recycled fibers from waste polyester fabrics comprises the following specific steps: The polyester waste fabric is washed and dried in advance, and the working gas is argon at normal pressure, and the discharge frequency of the dielectric barrier discharge is 100 MHz. The polyester waste fabric is subjected to plasma treatment and then crushed, and heated to 260°C to melt to obtain a melt mixture; then the melt mixture is filtered with a filtration accuracy of 30 μm, and then mixed with a dispersant, ethylene glycol, and an alcoholysis catalyst, heated to 250°C and reacted for 2 hours to obtain a pre-alcoholysis mixture, and then the pre-alcoholysis mixture is mixed with an antimony-based catalyst, reacted at 275°C for 1 hour, and then spun, and the drafting multiple is controlled to be 3.0 to obtain polyester waste fabric recycled fiber.
[0025] Example 2 The difference between Example 2 and Example 1 is that the amount of polyester waste cloth used in the polyester waste cloth regenerated fiber raw material is 40 kg, the amount of ethylene glycol used is 80 kg, the amount of alcoholysis catalyst used is 0.03 kg, the amount of antimony catalyst used is 0.01 kg, the amount of heat stabilizer used is 0.005 kg, and the amount of dispersant used is 15 kg.
[0026] Example 3 The difference between Example 3 and Example 1 is that the amount of polyester waste cloth used in the polyester waste cloth regenerated fiber raw material is 50 kg, the amount of ethylene glycol used is 120 kg, the amount of alcoholysis catalyst used is 0.05 kg, the amount of antimony catalyst used is 0.03 kg, the amount of heat stabilizer used is 0.008 kg, and the amount of dispersant used is 25 kg.
[0027] Example 4 The difference between Example 4 and Example 1 is that the alcoholysis catalyst in the polyester waste cloth regenerated fiber raw material is potassium oxide.
[0028] Example 5 The difference between Example 5 and Example 1 is that the alcoholysis catalyst in the polyester waste cloth regenerated fiber raw material is zinc acetate.
[0029] Example 6 The difference between Example 6 and Example 1 is that the antimony catalyst in the polyester waste cloth regenerated fiber raw material is ethylene glycol antimony.
[0030] Example 7 The difference between Example 7 and Example 1 is that the heat stabilizer in the polyester waste cloth regenerated fiber raw material is triethyl phosphate.
[0031] Example 8 The difference between Example 8 and Example 1 is that the dispersant in the polyester waste cloth regenerated fiber raw material is polyoxyethylene alcohol, and the molecular weight of the polyoxyethylene alcohol is 170,000.
[0032] Example 9 The difference between Example 9 and Example 1 is that the dispersant in the polyester waste cloth regenerated fiber raw material is a mixture of anionic dispersants and alcohol ether dispersants, and the mass ratio of the anionic dispersant to the alcohol ether dispersant is 1.2: 1. The anionic dispersant is sodium hexametaphosphate, and the alcohol ether dispersant is alkylphenol polyoxyethylene ether OP-10.
[0033] Example 10 The difference between Example 10 and Example 9 is that the mass ratio of the anionic dispersant to the alcohol ether dispersant in the polyester waste cloth regenerated fiber raw material is 1:1.
[0034] Embodiment 11 The difference between Example 11 and Example 9 is that the mass ratio of the mixture of the anionic dispersant and the alcohol ether dispersant in the polyester waste cloth regenerated fiber raw material is 1.5:1.
[0035] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that no dispersant is used in the polyester waste cloth regenerated fiber raw material.
[0036] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that no heat stabilizer and dispersant are used in the polyester waste cloth recycled fiber raw material.
[0037] Performance testing The following performance tests were performed on the polyester waste cloth recycled fibers provided by Examples 1-11 and Comparative Examples 1-2 of the present application, and the specific test results are shown in Table 1.
[0038] Detection Methods 1. Viscosity test The regenerated fiber prepared in the present application was dissolved in a 1,1,2,2-tetrachloroethane-phenol mixed solution, where the mass ratio of phenol to 1,1,2,2-tetrachloroethane was 1:1. The solution was tested using an Ubbelohde viscometer at 25°C, and the intrinsic viscosity was calculated using the Solomon-Ciuta equation.
[0039] 2. Mechanical properties The tensile strength and elongation at break of the regenerated fiber prepared in the present application were tested with reference to the standard of GB / T14337-2008 "Test method for tensile properties of chemical staple fibers".
[0040] Table 1: Performance test data table The test results show that the polyester waste cloth regenerated fiber prepared in the present application has strong viscosity and strength and good spinnability. The present application can improve the spinnability of polyester fiber through the synergistic effect of various components, promote the regenerated fiber to have good tensile strength and elongation at break, and improve the quality of the regenerated fiber.
[0041] By comparing Examples 4-5 with Example 1, it can be seen that different types of alcoholysis catalysts are used in the polyester waste cloth regenerated fiber raw materials. From the performance test results, it can be seen that the alcoholysis catalysts used in Examples 1 and 5 have better effects. This may be because metal salt catalysts have higher solubility, improve the efficiency of alcoholysis reaction, and promote the generation of regenerated fibers.
[0042] By comparing Examples 8-9 with Example 1, it can be seen that Examples 8-9 use different dispersants, and from the performance test results, it can be seen that the comprehensive performance of Example 9 is significantly improved. It is further explained that the use of a mixture of anionic dispersants and alcohol ether dispersants as dispersants can simultaneously utilize the adsorption film-forming effect of anionic dispersants and the good dispersing and emulsifying effect of alcohol ether dispersants, which can promote the polyester fiber to have better dispersibility, reduce the fiber agglomeration rate, and improve the strength and quality of the regenerated fiber.
[0043] By comparing Comparative Examples 1-2 with Example 1, it can be seen that Comparative Example 1 does not use a dispersant, and Comparative Example 2 does not use a heat stabilizer and a dispersant. From the performance test results, it can be seen that the comprehensive performance of the regenerated fiber will decrease. It is further explained that adding an appropriate amount of heat stabilizer to the regenerated fiber raw material can improve the thermal stability of polyester fiber during high-temperature processing, reduce high-temperature thermal degradation of polyester fiber, and thus promote the generation of regenerated fiber and improve the quality of regenerated fiber. At the same time, the use of a dispersant can improve the fluidity of the polyester fiber melt, enhance the spinnability of the fiber, and reduce the fiber agglomeration rate.
[0044] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A recycled fiber from waste polyester fabric, characterized in that: The invention comprises the following raw materials in parts by weight: 40-50 parts of polyester waste fabric, 80-120 parts of ethylene glycol, 0.03-0.05 parts of alcoholysis catalyst, 0.01-0.03 parts of antimony catalyst, 0.005-0.008 parts of heat stabilizer and 15-25 parts of dispersant; the dispersant is at least one of an anionic dispersant and an alcohol ether dispersant.
2. The polyester waste cloth regenerated fiber according to claim 1, characterized in that: The dispersant is a mixture of an anionic dispersant and an alcohol ether dispersant, and the mass ratio of the anionic dispersant to the alcohol ether dispersant is (1-1.5):
1.
3. The polyester waste cloth regenerated fiber according to claim 2, characterized in that: The anionic dispersant is at least one of sodium dodecylbenzene sulfonate, sodium hexametaphosphate, and fatty alcohol ether phosphate salts; the alcohol ether dispersant is at least one of polyoxyethylene alcohol, fatty alcohol polyoxyethylene ether, and alkylphenol polyoxyethylene ether.
4. The polyester waste cloth regenerated fiber according to claim 1, characterized in that: The alcoholysis catalyst is one of a metal salt catalyst and a metal oxide catalyst.
5. The polyester waste cloth regenerated fiber according to claim 4, characterized in that: The metal salt catalyst is one of sodium acetate, sodium carbonate and zinc acetate.
6. The polyester waste cloth regenerated fiber according to claim 1, characterized in that: The antimony catalyst is one of antimony acetate, antimony glycol, and antimony trioxide.
7. The polyester waste cloth regenerated fiber according to claim 1, characterized in that: The heat stabilizer is one of triethyl phosphonoacetate, phosphoric acid, and triethyl phosphate.
8. A method for preparing recycled fibers from polyester waste fabrics as claimed in any one of claims 1 to 7, characterized in that: The specific steps include: The polyester waste fabric is washed and dried in advance, crushed after plasma treatment, melted after crushing to obtain a melt mixture, and then the melt mixture is filtered and mixed with a dispersant, ethylene glycol, and an alcoholysis catalyst, and heated to react to obtain a pre-alcoholysis mixture, and then the pre-alcoholysis mixture is mixed with an antimony catalyst, heated to react, and spun to obtain regenerated fibers.
9. The method for preparing recycled fibers from polyester waste fabrics according to claim 8, characterized in that: The heating temperature is 200-275°C.
Citation Information
Patent Citations
Whitened regenerated terylene staple fiber
CN102936758A
Process for spinning regenerated fibers through complete alcoholysis of waste polyester textiles
CN113584641A
Recycled polyester staple fiber using waste polyester and method thereof
KR1020110116457A
Method for producing terylene fiber using polyester waste
WO2012027935A1