Composite hydrophobic material for inhibiting crystallization of tunnel drainage pipeline

By coating the tunnel drainage pipe with a composite hydrophobic material, the problem of crystallization blockage in the tunnel drainage pipe is solved, and the effective crystallization inhibition and anti-icing effect in an alkaline environment is achieved, extending the service life of the pipe.

CN118745319AActive Publication Date: 2024-10-08LANZHOU UNIVERSITY OF TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410719248.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-08
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

Tunnel drainage pipes are prone to crystallization blockage, which affects the drainage effect. This is mainly due to the weak alkalinity of the water and the conditions for full contact with easily crystallized ions.

Method used

A composite hydrophobic material is used, including a hydrophobic inner layer and a scale-inhibiting outer layer. The hydrophobic inner layer is composed of tetrahydrofuran, nano-silica, silane coupling agent, etc., and the scale-inhibiting outer layer is composed of EDTA, sulfamic acid, etc., through The inner wall of the pipe is coated to form an imitation umbrella structure to reduce the contact area and increase the surface contact angle, enhance the rolling properties of water droplets, and add low-temperature expansion particles and hydrophobic microspheres in low-temperature environments to enhance the anti-icing effect.

Benefits of technology

It effectively inhibits the formation of calcium carbonate crystals in an alkaline environment, improves hydrophobic properties and anti-icing effects, extends the service life of pipelines, and maintains excellent hydrophobic properties and anti-scaling effects during long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745319A_ABST
    Figure CN118745319A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of pipeline drainage, in particular to a composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipeline and a preparation method. The composite hydrophobic material comprises a hydrophobic inner layer and a scale inhibition outer layer attached to the outer surface of the hydrophobic inner layer, wherein the hydrophobic inner layer comprises tetrahydrofuran, a solvent volatilizer, an interfacial agent, nano silicon dioxide, a cross-linking agent and a curing agent; the scale inhibition outer layer comprises a scale inhibitor solution and a colloid material, and the scale inhibitor solution comprises EDTA, hydrolytic maleic anhydride and sulfamic acid. The preparation method comprises the following steps: S1, coating the hydrophobic inner layer material, S2, airing to obtain the hydrophobic inner layer, and S3, coating the surface of the hydrophobic inner layer with the scale inhibition outer layer material to obtain the composite material. The prepared composite material still has excellent hydrophobic performance after standing for 24 h and can be kept for a long time, the outer scale inhibition layer protects the inner hydrophobic layer and plays a scale inhibition role at the same time, and the functionality of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pipeline drainage, and in particular to a composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipeline. Background Art

[0002] According to the analysis of tunnel water samples, Ca 2+ Mg 2+ The average concentrations were only 16.46 mg / L and 8.67 mg / L, respectively. 3- The average concentration is as high as 208mg / L. Since the water flow rate in the drainage pipe is low, it creates conditions for the easy-to-crystallize ions to fully contact; and the water quality is weakly alkaline, which is also conducive to the formation of crystals. Therefore, under long-term use, the tunnel drainage pipe is prone to crystal blockage, thus affecting the drainage effect.

[0003] In order to solve the common tunnel crystallization blockage problem in tunnel construction and operation and maintenance, the present invention develops a new type of composite hydrophobic material for inhibiting the formation of crystals. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe.

[0005] A composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe, comprising a hydrophobic inner layer for coating on the inner wall of the pipe and a scale-inhibiting outer layer attached to the outer surface of the hydrophobic inner layer;

[0006] The hydrophobic inner layer comprises tetrahydrofuran: solvent volatile agent: surfactant: nano-silica: cross-linking agent: curing agent in a volume mass ratio of 4.5-5.5:6:0.05:1:1:0.02;

[0007] The anti-scaling outer layer comprises, in a mass volume ratio, an anti-scaling agent solution and a colloid material in a ratio of 1 to 1.5:5, wherein the anti-scaling agent solution comprises, in a mass ratio, EDTA: hydrolyzed maleic anhydride: aminosulfonic acid in a ratio of 4:3:0.5 to 0.6.

[0008] Furthermore, the surfactant is a silane coupling agent, and the solvent volatile agent is isopropyl alcohol.

[0009] Note: When the surfactant is a silane coupling agent, the composite material finally prepared still has excellent hydrophobic properties after standing for 24 hours, and can be maintained for a long time; when an appropriate amount of isopropanol is added, the droplet rolling speed when water flows through the composite material is optimal.

[0010] Furthermore, the cross-linking agent is RTV-2 silicone rubber, and the curing agent is DOP.

[0011] Description: After curing, RTV-2 silicone rubber can maintain elasticity in the temperature range of -60 to 200°C. It is suitable for high temperature environments and can provide a material option with stable performance, easy operation, and environmentally friendly.

[0012] Furthermore, the colloid material comprises polyvinyl alcohol: sodium alginate in a mass ratio of 1:0.1.

[0013] Description: When polyvinyl alcohol is mixed with sodium alginate, it has more stable compatibility and solubility, will not cause additional crystallization burden, and can give the antiscalant solution a certain mechanical strength.

[0014] Furthermore, the preparation method of the hydrophobic inner layer is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and then nano-silicon dioxide and a surfactant are sequentially added to the solution A and stirred for 4 to 6 minutes to obtain a solution B, and then RTV-2 crosslinking agent and a curing agent are sequentially added to the solution B and stirred for 9 to 11 minutes. After stirring, a hydrophobic inner layer material is obtained.

[0015] Note: The above hydrophobic inner layer material was applied to the surface of the square piece and allowed to stand for 24 hours. The contact angle was measured to be 130.63° and the rolling angle was 8.110°, indicating that the hydrophobic inner layer has excellent hydrophobic properties.

[0016] Furthermore, the preparation method of the anti-scaling outer layer is: firstly, the raw materials of the anti-scaling agent solution are mixed in proportion to obtain the anti-scaling agent solution, and then the colloidal material is put into the anti-scaling agent solution in proportion, and then dissolved and stirred in a water bath at 92 to 98°C for 0.4 to 0.6 hours, and the anti-scaling outer layer material is obtained after the dissolution and stirring are completed.

[0017] Note: Calcium carbonate crystals in the pipe are due to the Ca 2+ and HCO 3- By selecting a suitable scale inhibitor and adding a certain amount of glue material, it can be slow-released and react with Ca in water. 2+ and HCO 3- Reaction, slowly release the drug and reduce the amount of crystals formed.

[0018] Furthermore, the hydrophobic inner layer also includes low-temperature expansion particles and hydrophobic microspheres;

[0019] The preparation method of the hydrophobic inner layer is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and the solution A is divided into two parts;

[0020] Then, using ultrasound, the low temperature expansion particles are dispersed in one of the A solutions at a solid-liquid ratio of 1:1-2 for 8-10 minutes to obtain a C1 solution, and then using ultrasound, the hydrophobic microspheres are dispersed in another A solution at a solid-liquid ratio of 1:4-6 for 8-10 minutes to obtain a C2 solution;

[0021] Then, nano-silica and surfactant are sequentially added to the C1 solution and stirred for 4 to 6 minutes to obtain a D solution, a cross-linking agent and a curing agent are sequentially added to the D solution and stirred for 9 to 11 minutes, and the solution is semi-cured at 80 to 90° C. for 15 to 25 minutes to obtain a semi-cured material, and the semi-cured material is then immersed in the C2 solution and completely cured at 100 to 105° C. to obtain a B hydrophobic inner layer material;

[0022] The shell of the hydrophobic microsphere is made of silicone rubber, the inner core of the hydrophobic microsphere is filled with polydimethylsiloxane mucus, the diameter of the hydrophobic microsphere is 3-5 μm, and the thickness of the shell is 20-30% of the diameter; the low-temperature expansion particles include 2-3 parts of expanded perlite, 10-20 parts of sodium acrylate, 5-7 parts of sodium chloride and 0.4-0.5 parts of isopropyl cyanoacetate by weight, and the diameter of the low-temperature expansion particles is 40-50 μm.

[0023] Description: In a low temperature environment, the moisture in the water will condense to form ice, which can easily lead to crystallization or freezing of the pipe, thereby affecting the drainage effect. Therefore, the present application adds low-temperature expansion particles to the hydrophobic inner layer material, so that in a low temperature environment such as winter, the low-temperature expansion particles expand, thereby increasing the contact area between the hydrophobic inner layer material and the inner wall of the pipe, thereby improving the anti-icing effect. In addition, due to the addition of hydrophobic microspheres, the low-temperature expansion particles will squeeze the hydrophobic microspheres while expanding, so that the polydimethylsiloxane mucus inside them will be discharged, thereby further improving the hydrophobic effect, thereby further improving the effect of inhibiting crystallization.

[0024] Furthermore, the hydrophobic inner layer comprises a first hydrophobic inner layer material and a second hydrophobic inner layer material in a mass ratio of 1:0.5-1.5.

[0025] The preparation method of the first hydrophobic inner layer material is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and then nano-silicon dioxide and a surfactant are sequentially added to the solution A and stirred for 4 to 6 minutes to obtain a solution B, and then a cross-linking agent and a curing agent are sequentially added to the solution B and stirred for 9 to 11 minutes, and after stirring, the first hydrophobic inner layer material is obtained;

[0026] The preparation method of the second hydrophobic inner layer material is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and the solution A is divided into two parts;

[0027] Then, using ultrasound, the low temperature expansion particles are dispersed in one of the A solutions at a solid-liquid ratio of 1:1-2 for 8-10 minutes to obtain a C1 solution, and then using ultrasound, the hydrophobic microspheres are dispersed in another A solution at a solid-liquid ratio of 1:4-6 for 8-10 minutes to obtain a C2 solution;

[0028] Then, nano-silica and surfactant are added to the C1 solution in sequence and stirred for 4 to 6 minutes to obtain a D solution. A cross-linking agent and a curing agent are added to the D solution in sequence and stirred for 9 to 11 minutes. The solution is semi-cured at 80 to 90° C. for 15 to 25 minutes to obtain a semi-cured material. The semi-cured material is then immersed in a C2 solution and completely cured at 100 to 105° C. to obtain a second hydrophobic inner layer material.

[0029] Description: The first hydrophobic inner layer material and the second hydrophobic inner layer material have similar components, which helps to reduce the contact area and increase the surface contact angle, thereby enhancing the rolling properties of water droplets on the surface, making it easier for water droplets to roll off the pipe surface and achieving a better hydrophobic effect.

[0030] The method for preparing the composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe as described above comprises the following steps:

[0031] S1. First, apply a layer of hydrophobic inner layer material with a thickness of ≤0.03cm on the inner wall of the pipeline;

[0032] S2, waiting for the hydrophobic inner layer material to dry to obtain a hydrophobic inner layer;

[0033] S3. Coat a scale-inhibiting outer layer material with a thickness of 0.15 to 0.25 cm on the outer surface of the hydrophobic inner layer, and obtain a composite material after drying.

[0034] The method for preparing the composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe as described above comprises the following steps:

[0035] S1. First, a layer of the second hydrophobic inner layer material with a thickness of ≤0.03 cm is coated on the inner wall of the pipeline. The coating method is to use any point corresponding to the center of the pipeline as the center point, and then scatter multiple paths outward from the center point to coat, and the end point of the path returns to the center point. After coating, use a light dryer to dry and cure at 75-85°C for 5-10 minutes;

[0036] S2. After the second hydrophobic inner layer material is dried, a layer of the first hydrophobic inner layer material with a thickness of ≤0.03 cm is applied to the blank area between the inner wall of the pipe and the second hydrophobic inner layer material, and dried in a hot air drying oven at 65-75° C. for 20-30 minutes to obtain a hydrophobic inner layer;

[0037] S3. Apply a layer of anti-scaling outer layer material with a thickness of 0.15 to 0.25 cm to obtain a composite material.

[0038] Description: The second hydrophobic inner layer material is formed into multiple paths, namely the ribs, and the first hydrophobic inner layer material forms a base, namely the umbrella surface, thereby obtaining an umbrella-like structure. This structure helps to reduce the contact area and increase the surface contact angle, thereby enhancing the rolling properties of water droplets on the surface, making it easier for water droplets to roll off the pipe surface, achieving a better hydrophobic effect. The first hydrophobic inner layer material and the second hydrophobic inner layer material have similar components, and the two are tightly combined under the action of hot air drying to form a stable umbrella-like structure; and then the scale-inhibiting outer layer is coated on the surface of the hydrophobic inner layer of the umbrella-like structure. Because the surface of the ribs is not flat, the bonding surface between the hydrophobic inner layer and the scale-inhibiting outer layer can be regarded as wavy rather than straight, thereby further enhancing the bonding strength of the composite material.

[0039] Compared with the existing hydrophobic materials, the beneficial effects of the present invention are:

[0040] (1) In the present application, when tetrahydrofuran and isopropanol are mixed, the droplet rolling speed is optimal during drainage. When the surfactant is a silane coupling agent, it still has excellent hydrophobic properties after standing for 24 hours and can be maintained for a long time. When nano-silicon dioxide is used as a thickening enhancer, the material on the surface of the hydrophobic material is evenly dispersed, the material has no adhesion phenomenon and no obvious concave-convex texture, which is more conducive to the droplet rolling without staying on the contact surface. After curing, the RTV-2 silicone rubber can maintain elasticity in the temperature range of -60 to 200°C, and the prepared hydrophobic inner layer has excellent hydrophobic properties.

[0041] (2) In order to inhibit the formation of calcium carbonate type crystals in an alkaline environment, the present application selects EDTA, aminosulfonic acid, and hydrolyzed maleic anhydride as scale inhibitors, and selects polyvinyl alcohol and sodium alginate as colloidal materials. The scale inhibitor solvent is mixed with the colloidal material, which has more stable compatibility and solubility, will not cause additional crystallization burden, and can give the scale inhibitor solution a certain mechanical strength, protect the hydrophobic inner layer while playing a scale inhibitor role, thereby improving the functionality of the material.

[0042] (3) The present application adds low-temperature expansion particles to the hydrophobic inner layer material, so that in low-temperature environments such as winter, the low-temperature expansion particles expand, thereby increasing the contact area between the hydrophobic inner layer material and the inner wall of the pipe, thereby improving the anti-icing effect. In addition, due to the addition of hydrophobic microspheres, the low-temperature expansion particles will squeeze the hydrophobic microspheres while expanding to discharge the polydimethylsiloxane mucus inside, thereby further improving the hydrophobic effect, thereby further improving the crystallization inhibition effect; and the hydrophobic inner layer material B to which the low-temperature expansion particles are added and the hydrophobic inner layer material A to which the expansion particles are not added are combined into an umbrella structure. This structure helps to reduce the contact area and increase the surface contact angle, thereby enhancing the rolling properties of water droplets on the surface, making it easier for water droplets to roll off the pipe surface, achieving a better hydrophobic effect. The low-temperature expansion particles will expand in a low-temperature environment, which helps to prevent the formation and adhesion of ice crystals, thereby reducing the damage to the drainage pipe caused by freezing and extending its service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a result diagram of experimental example and control example 1 of the composite hydrophobic material of the present invention;

[0044] Figure 2 This is a diagram showing the anti-crystallization results of Experimental Example 1 of the composite hydrophobic material of the present invention;

[0045] Figure 3 This is a scale inhibition result diagram of Experimental Example 1 of the composite hydrophobic material of the present invention;

[0046] Figure 4 This is a diagram showing the anti-crystallization results of Experimental Example 2 of the composite hydrophobic material of the present invention. DETAILED DESCRIPTION

[0047] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.

[0048] Embodiment 1: A composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe, comprising a hydrophobic inner layer for coating on the inner wall of the pipe and a scale-inhibiting outer layer attached to the outer surface of the hydrophobic inner layer;

[0049] The hydrophobic inner layer comprises tetrahydrofuran: solvent volatile agent: surfactant: nano-silicon dioxide: cross-linking agent: curing agent in a volume mass ratio of 5:6:0.05:1:1:0.02; the surfactant is a silane coupling agent, the solvent volatile agent is isopropanol; the cross-linking agent is RTV-2 silicone rubber, and the curing agent is DOP;

[0050] The preparation method of the hydrophobic inner layer is as follows: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, nano-silicon dioxide and a surfactant are then sequentially added to the solution A and stirred for 5 minutes to obtain a solution B, and then an RTV-2 crosslinking agent and a curing agent are sequentially added to the solution B and stirred for 10 minutes, and after stirring, a hydrophobic inner layer material is obtained;

[0051] The anti-scaling outer layer comprises, by mass volume ratio, an anti-scaling agent solution and a colloid material in a ratio of 1.25:5, wherein the anti-scaling agent solution comprises, by mass ratio, EDTA: hydrolyzed maleic anhydride: aminosulfonic acid in a ratio of 4:3:0.55; the colloid material comprises, by mass ratio, polyvinyl alcohol: sodium alginate in a ratio of 1:0.1;

[0052] The preparation method of the anti-scaling outer layer is as follows: firstly, the raw materials of the anti-scaling agent solution are mixed in proportion to obtain the anti-scaling agent solution, and then the colloid material is put into the anti-scaling agent solution in proportion, and then dissolved and stirred in a water bath at 95° C. for 0.5 h, and the anti-scaling outer layer material is obtained after the dissolution and stirring are completed.

[0053] Embodiment 2: A method for preparing a composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe comprises the following steps:

[0054] S1, firstly coating a layer of the hydrophobic inner layer material with a thickness of 0.03 cm prepared in Example 1 on the inner wall of the pipeline;

[0055] S2, drying the mixed hydrophobic inner layer material to obtain a hydrophobic inner layer;

[0056] S3. Then, a layer of anti-scaling outer layer material with a thickness of 0.20 cm is coated on the outer surface of the hydrophobic inner layer, and the composite material is obtained after drying.

[0057] Example 3: This example is different from Example 1 in that the hydrophobic inner layer comprises tetrahydrofuran: solvent volatile agent: surfactant: nano-silica: cross-linking agent: curing agent in a volume mass ratio of 4.5:6:0.05:1:1:0.02.

[0058] Example 4: This example is different from Example 1 in that the hydrophobic inner layer comprises tetrahydrofuran: solvent volatile agent: surfactant: nano-silica: cross-linking agent: curing agent in a volume mass ratio of 5.5:6:0.05:1:1:0.02.

[0059] Example 5: This example is different from Example 1 in that the antiscaling outer layer comprises, by mass volume ratio, an antiscaling agent solution and a colloid material in a ratio of 1:5.

[0060] Example 6: This example is different from Example 1 in that the antiscaling outer layer comprises, by mass volume ratio, an antiscaling agent solution and a colloid material in a ratio of 1.5:5.

[0061] Example 7: This example is different from Example 1 in that the scale inhibitor solution includes EDTA: hydrolyzed maleic anhydride: aminosulfonic acid in a mass ratio of 4:3:0.5.

[0062] Example 8: This example is different from Example 1 in that the scale inhibitor solution includes EDTA: hydrolyzed maleic anhydride: aminosulfonic acid in a mass ratio of 4:3:0.6.

[0063] Example 9: The difference between this example and Example 1 is that the preparation method of the hydrophobic inner layer is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and then nano-silica and a surfactant are sequentially added to the solution A and stirred for 4 minutes to obtain a solution B, and then RTV-2 cross-linking agent and a curing agent are sequentially added to the solution B and stirred for 9 minutes.

[0064] Example 10: This example is different from Example 1 in that the method for preparing the hydrophobic inner layer is as follows: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and then nano-silica and a surfactant are sequentially added to the solution A and stirred for 6 minutes to obtain a solution B, and then RTV-2 cross-linking agent and a curing agent are sequentially added to the solution B and stirred for 11 minutes.

[0065] Example 11: This example is different from Example 1 in that the colloidal material is put into the antiscalant solution in proportion, and then dissolved and stirred in a water bath at 92°C for 0.4h.

[0066] Example 12: This example is different from Example 1 in that the colloidal material is put into the antiscalant solution in proportion, and then dissolved and stirred in a water bath at 98°C for 0.6h.

[0067] Example 13: This example is different from Example 1 in that the hydrophobic inner layer further comprises low-temperature expansion particles and hydrophobic microspheres; the preparation method of the hydrophobic inner layer is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and the solution A is equally divided into 2 parts;

[0068] Then, the low-temperature expansion particles were dispersed in one of the A solutions at a solid-liquid ratio of 1:1.5 for 9 minutes by ultrasonic wave to obtain a C1 solution, and then the hydrophobic microspheres were dispersed in another A solution at a solid-liquid ratio of 1:5 for 9 minutes by ultrasonic wave to obtain a C2 solution; the ultrasonic wave power was 50KHz;

[0069] Then, nano-silica and surfactant were added to the C1 solution in sequence and stirred for 5 minutes to obtain a D solution, a cross-linking agent and a curing agent were added to the D solution in sequence and stirred for 10 minutes, and the solution was semi-cured at 85° C. for 20 minutes to obtain a semi-cured material, and the semi-cured material was immersed in the C2 solution and completely cured at 103° C. to obtain a hydrophobic inner layer material;

[0070] The shell of the hydrophobic microsphere is made of silicone rubber, the inner core of the hydrophobic microsphere is filled with polydimethylsiloxane mucus, the diameter of the hydrophobic microsphere is 4 μm, and the thickness of the shell is 25% of the diameter; the low-temperature expansion particles include 2.5 parts of expanded perlite, 15 parts of sodium acrylate, 6 parts of sodium chloride and 0.45 parts of isopropyl cyanoacetate by weight, and the diameter of the low-temperature expansion particles is 45 μm.

[0071] Example 14: This example is different from Example 13 in that the low-temperature expansion particles are dispersed in solution A at a solid-liquid ratio of 1:1 for 8 minutes using ultrasound to obtain solution C1.

[0072] Example 15: This example differs from Example 13 in that the low-temperature expansion particles are dispersed in solution A at a solid-liquid ratio of 1:2 for 10 minutes using ultrasound to obtain solution C1.

[0073] Example 16: This example is different from Example 13 in that the hydrophobic microspheres are dispersed in solution A at a solid-liquid ratio of 1:4 for 8 minutes using ultrasound to obtain solution C2.

[0074] Example 17: This example is different from Example 13 in that the hydrophobic microspheres are dispersed in solution A at a solid-liquid ratio of 1:6 for 10 minutes using ultrasound to obtain solution C2.

[0075] Example 18: This example is different from Example 13 in that the semi-cured material is obtained by semi-curing at 80°C for 15 minutes, and then the semi-cured material is immersed in C2 solution and completely cured at 100°C to obtain a hydrophobic inner layer material.

[0076] Example 19: This example is different from Example 13 in that the semi-cured material is obtained by semi-curing at 90°C for 25 minutes, and then the semi-cured material is immersed in C2 solution and completely cured at 105°C to obtain a hydrophobic inner layer material.

[0077] Example 20: This example is different from Example 13 in that the diameter of the hydrophobic microspheres is 3 μm and the thickness of the shell is 30% of the diameter.

[0078] Example 21: This example is different from Example 13 in that the diameter of the hydrophobic microspheres is 5 μm and the thickness of the shell is 20% of the diameter.

[0079] Example 22: This example is different from Example 13 in that the low-temperature expanding particles include 2 parts of expanded perlite, 20 parts of sodium acrylate, 7 parts of sodium chloride and 0.5 parts of isopropyl cyanoacetate by weight, and the diameter of the low-temperature expanding particles is 40 μm.

[0080] Example 23: This example is different from Example 13 in that the low-temperature expanding particles include 3 parts of expanded perlite, 10 parts of sodium acrylate, 5 parts of sodium chloride and 0.4 parts of isopropyl cyanoacetate by weight, and the diameter of the low-temperature expanding particles is 50 μm.

[0081] Example 24: This example is different from Example 13 in that the hydrophobic inner layer comprises a first hydrophobic inner layer material and a second hydrophobic inner layer material in a mass ratio of 1:1, wherein the first hydrophobic inner layer material is prepared in the manner of Example 1, and the second hydrophobic inner layer material is prepared in the manner of Example 13.

[0082] Example 25: This example is different from Example 24 in that the hydrophobic inner layer includes a first hydrophobic inner layer material and a second hydrophobic inner layer material in a mass ratio of 1:0.5.

[0083] Example 26: This example is different from Example 24 in that the hydrophobic inner layer includes a first hydrophobic inner layer material and a second hydrophobic inner layer material in a mass ratio of 1:1.5.

[0084] Example 27: This example is different from Example 2 in that the thickness of the scale-inhibiting outer layer material is 0.15 cm.

[0085] Example 28: This example is different from Example 2 in that the thickness of the scale-inhibiting outer layer material is 0.25 cm.

[0086] Example 29: This example is different from Example 2 in that a method for preparing a composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe comprises the following steps:

[0087] S1. First, a layer of the second hydrophobic inner layer material with a thickness of 0.03 cm is coated on the inner wall of the pipeline. The coating method is to use any point corresponding to the center of the pipeline as the center point, and then scatter multiple paths outward from the center point to coat, and the end point of the path returns to the center point. After coating, use a light dryer to dry and cure at 80°C for 8 minutes;

[0088] S2. After the second hydrophobic inner layer material is dried, a layer of the first hydrophobic inner layer material with a thickness of 0.03 cm is applied to the blank area between the inner wall of the pipe and the second hydrophobic inner layer material, and dried in a hot air drying oven at 70° C. for 25 minutes to obtain a hydrophobic inner layer;

[0089] S3. Then apply a scale-inhibiting outer layer with a thickness of 0.20 cm to obtain a composite material.

[0090] Example 30: This example is different from Example 29 in that, in step S1, a light dryer is used for drying and curing at 75°C for 5 minutes.

[0091] Example 31: This example is different from Example 29 in that, in step S1, a light dryer is used for drying and curing at 85°C for 10 minutes.

[0092] Example 32: This example differs from Example 29 in that, in step S2, hot air drying is performed in a hot air drying oven at 65°C for 20 minutes.

[0093] Example 33: This example is different from Example 29 in that, in step S2, hot air drying is performed in a hot air drying oven at 75°C for 30 minutes.

[0094] Experimental Example: The description of this experimental example is based on the scheme described in Example 1 or 2, and is intended to illustrate the practical application effect of the present invention.

[0095] Experimental Design 1: To explore the performance of the hydrophobic inner layer and the scale-inhibiting outer layer in Example 1, a HDPE pipe with a wall thickness of 2 cm and a length of 15 cm was selected, and 1 / 4 of the pipe cross section was cut (to facilitate observation of the crystallization effect inside the pipe), and 3 / 4 was left for simulation experiments and encapsulated on both sides with silicone rubber (HG / T3947-2007 single-package room temperature curing silicone rubber) and tape, and a 30-day immersion simulation was carried out at room temperature. The results are as follows:

[0096] 1. Investigate the influence of the component ratio of the hydrophobic inner layer and the anti-scaling outer layer and the preparation parameters on the single-layer performance.

[0097] Table 1 Anti-crystallization rate of the hydrophobic inner layer in Examples 1, 3-4, 9-10 and Comparative Example 1

[0098] Group Example 1 Example 3 Example 4 Example 9 Example 10 Comparative Example 1 Anti-crystallization rate% 89.08 87.69 88.54 88.01 88.92 43.21

[0099] Table 2 Scale inhibition rate of the scale inhibition outer layer in Examples 1, 5-8, 11-12 and Comparative Example 1

[0100]

[0101] The difference between Control Example 1 and Example 1 is that no material is coated inside the pipe;

[0102] Through the 30-day immersion simulation experiment, it is known that Figure 1 The original pipe of (Comparative Example 1) has obvious crystallization inside. Figure 2(The hydrophobic inner layer of Example 1) can effectively inhibit the formation of crystals on the surface of the pipe and exert stable hydrophobic properties, but there is a phenomenon of slight shedding of the hydrophobic interface; Figure 3 (Scale-inhibiting outer layer of Example 1) Part of the scale-inhibiting outer layer still remains on the inner surface of the pipe, indicating that the scale-inhibiting outer layer has a slow-release property;

[0103] And by comparing Examples 1, 3 to 12, it can be seen that if the proportion of tetrahydrofuran is too small or too large, the stirring parameters during the preparation of the hydrophobic inner layer material A are too small or too large, the proportion of the scale inhibitor solution is too small or too large, and the parameters of the dissolution of the colloidal material are too small, the anti-crystallization and scale inhibition effects on the pipe will be reduced. The scale inhibition rate of Example 12 with higher temperature and longer stirring time is the same as that of Example 1. From an economic point of view, the parameter effect of Example 1 is relatively better.

[0104] 2. Investigate the effect of the preparation method and components of the hydrophobic inner layer on the anti-crystallization rate at low temperatures.

[0105] Table 3 Low temperature (-10°C) anti-crystallization rate of the hydrophobic inner layer in Examples 13 to 23 and Comparative Examples 2 to 3

[0106]

[0107] The difference between Control Example 2 and Example 13 is that there are no hydrophobic microspheres;

[0108] The difference between Control Example 3 and Example 13 is that there is no isopropyl cyanoacetate in the low-temperature expansion particles;

[0109] From the results in Table 3, it can be seen that although the low-temperature anti-crystallization rate of Control Example 2 lacking hydrophobic microspheres and Control Example 3 lacking isopropyl cyanoacetate is improved compared with Example 1, the improvement is much smaller than that of Examples 13 to 23. Therefore, both hydrophobic microspheres and isopropyl cyanoacetate play a certain role in preventing the material from crystallizing at low temperatures;

[0110] By comparing Examples 13 to 23, it can be seen that too small or too large a proportion of low-temperature expanding particles, too small or too large a proportion of hydrophobic microspheres, too small or too large a degree of solidification, too small or too large a size of the hydrophobic microspheres, and too small or too large a proportion of expanded perlite in the low-temperature expanding particles will reduce the improvement in the low-temperature anti-crystallization rate. By comparing Examples 13 and 24 to 26, it can be seen that the combination of the two can further improve the effect of the hydrophobic inner layer, and too small or too large a proportion of the second hydrophobic inner layer material will reduce the improvement in the effect. Therefore, in comprehensive comparison, the parameter effect of Example 26 is relatively better.

[0111] Experimental Design 2: The composite hydrophobic material was applied to the surface of the PE square sheet according to the method of Example 2, and red ink was dotted on the surface of the PE square sheet with the inner layer applied to reflect the effect of the scale-inhibiting outer layer through color change. After drying in an oven, the scale-inhibiting outer layer was applied, and after drying, it was fixed in a simulated pipeline environment and immersed for 30 days at room temperature. The results are as follows:

[0112] 3. Investigate the influence of preparation steps and parameters of composite materials on the anti-crystallization rate of composite materials.

[0113] Table 4 Anti-crystallization rate of the composite materials in Examples 2, 27-33 and Comparative Examples 4-8

[0114]

[0115] The difference between Control Example 4 and Example 29 is that the first hydrophobic inner layer material is applied in both Steps S1 and S2;

[0116] The difference between Control Example 5 and Example 29 is that the coating methods of the second hydrophobic inner layer material and the first hydrophobic inner layer material are opposite;

[0117] The difference between Control Example 6 and Example 29 is that the second hydrophobic inner layer material is applied in both Steps S1 and S2;

[0118] The difference between Control Example 7 and Example 2 is that the second hydrophobic inner layer material is coated in step S1;

[0119] The difference between Control Example 8 and Example 2 is that in step S1, a mixed hydrophobic inner layer material obtained by mixing the first hydrophobic inner layer material and the second hydrophobic inner layer material in a mass ratio of 1:1 is coated;

[0120] Through the 30-day immersion simulation experiment, it is known that Figure 4 (Example 2) From left to right, the simulation conditions at the 10th day, the 20th day and the 30th day are shown. The degree of color development of the red ink reflects the efficacy of the outer layer, indicating that the scale-inhibiting outer layer can stably exert a sustained-release period of at least 30 days to prevent the formation of crystals. After the experiment, the scale-inhibiting outer layer on the surface of the PE square sheet was removed and cleaned, and it was observed that the hydrophobic inner layer did not fall off slightly and showed good hydrophobic performance.

[0121] Compared with the single-layer performance explored in Experimental Design 1, the anti-crystallization rate of the double-layer composite material is obviously improved. The scale inhibition rate is maintained between 94.76 and 95.03 because the improvement is small and Examples 27 to 33 are improvements to the hydrophobic inner layer structure. The fluctuation range is small and it is not necessary to compare them one by one.

[0122] From the results in Table 4, it can be seen that since the second hydrophobic inner layer material and the first hydrophobic inner layer material of Example 1 used in Control Example 4 are the same, that is, the improvement of Example 13 is not performed, and the performance of the second hydrophobic inner layer material in Control Example 5 is better than that of the first hydrophobic inner layer material, and the rib part is the key part supporting the entire hydrophobic inner layer, the effect of the second hydrophobic inner layer material as an umbrella rib is better than that of the first hydrophobic inner layer material, and Control Example 6 only uses the second hydrophobic inner layer material, and although the performance is worse than Control Example 4, it is not as good as the combination of the two. Therefore, Control Examples 4 to 6 significantly reduce the improvement of the anti-crystallization rate compared with Examples 27 to 30;

[0123] Since the second hydrophobic inner layer material is an improvement on the first hydrophobic inner layer material, the material properties of Control Examples 6 and 7 are improved compared with those of Example 2, but the effect presented by the coating method of Example 29 is weaker;

[0124] By comparing Examples 27 to 33, it can be seen that when the thickness of the scale-inhibiting outer layer is too small, the parameters of the drying and curing and the hot air drying are too low, the improvement of the anti-crystallization rate will be reduced. When the scale-inhibiting outer layer is larger, the protection strength of the hydrophobic inner layer is higher, so the anti-crystallization rate is higher than that of Example 1. When the drying and curing and hot air drying parameters are higher, the anti-crystallization rate is higher than that of Example 29, but the improvement is smaller. Therefore, from an economic point of view, the steps and parameter effects of Example 29 are relatively better.

[0125] In summary, experimental designs 1 and 2 prove that the material has excellent hydrophobicity and scale inhibition properties, and the scale inhibition outer layer can prevent the hydrophobic inner layer from slightly falling off. In long-distance water transportation, the composite hydrophobic material can exert its scale inhibition performance for at least 30 days, and the hydrophobic inner layer can exert its hydrophobic performance for a long time in the absence of external scratches.

Claims

1. A composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes, characterized in that: It includes a hydrophobic inner layer applied to the inner wall of the pipe and a scale-inhibiting outer layer attached to the outer surface of the hydrophobic inner layer; The hydrophobic inner layer comprises tetrahydrofuran: solvent volatile agent: surfactant: nano-silica: cross-linking agent: curing agent in a mass ratio of 4.5-5.5:6:0.05:1:1:0.02; The anti-scaling outer layer comprises, by mass ratio, an anti-scaling agent solution and a colloid material in a ratio of 1 to 1.5:5, wherein the anti-scaling agent solution comprises, by mass ratio, EDTA: hydrolyzed maleic anhydride: aminosulfonic acid in a ratio of 4:3:0.5 to 0.

6.

2. A composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes according to claim 1, characterized in that: The surfactant is a silane coupling agent, and the solvent volatile agent is isopropyl alcohol.

3. A composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes as claimed in claim 2, characterized in that: The crosslinking agent is RTV-2 silicone rubber, and the curing agent is DOP.

4. The composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes according to claim 1, characterized in that: The colloid material comprises polyvinyl alcohol and sodium alginate in a mass ratio of 1:0.

1.

5. The composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes according to claim 1, characterized in that: The preparation method of the hydrophobic inner layer material is as follows: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, nano silicon dioxide and a surfactant are then added to the solution A in sequence and stirred for 4 to 6 minutes to obtain a solution B, a crosslinking agent and a curing agent are then added to the solution B in sequence and stirred for 9 to 11 minutes, and after stirring, the hydrophobic inner layer material is obtained.

6. The composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes according to claim 1, characterized in that: The preparation method of the anti-scaling outer layer is as follows: firstly, the raw materials of the anti-scaling agent solution are mixed in proportion to obtain the anti-scaling agent solution, and then the colloid material is put into the anti-scaling agent solution in proportion, and then dissolved and stirred in a water bath at 92 to 98° C. for 0.4 to 0.6 hours, and after the dissolution and stirring are completed, the anti-scaling outer layer material is obtained.

7. The composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes according to claim 1, characterized in that: The hydrophobic inner layer also includes low temperature expansion particles and hydrophobic microspheres; The preparation method of the hydrophobic inner layer is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and the solution A is equally divided into two parts; Then, using ultrasound, the low temperature expansion particles are dispersed in one of the A solutions at a solid-liquid ratio of 1:1-2 for 8-10 minutes to obtain a C1 solution, and then using ultrasound, the hydrophobic microspheres are dispersed in another A solution at a solid-liquid ratio of 1:4-6 for 8-10 minutes to obtain a C2 solution; Then, nano-silica and surfactant are sequentially added to the C1 solution and stirred for 4 to 6 minutes to obtain a D solution, a cross-linking agent and a curing agent are sequentially added to the D solution and stirred for 9 to 11 minutes, and the solution is semi-cured at 80 to 90° C. for 15 to 25 minutes to obtain a semi-cured material, and the semi-cured material is then immersed in the C2 solution and completely cured at 100 to 105° C. to obtain a hydrophobic inner layer material; The shell of the hydrophobic microsphere is made of silicone rubber, the inner core of the hydrophobic microsphere is filled with polydimethylsiloxane mucus, the diameter of the hydrophobic microsphere is 3-5 μm, and the thickness of the shell is 20-30% of the diameter; the low-temperature expansion particles include 2-3 parts of expanded perlite, 10-20 parts of sodium acrylate, 5-7 parts of sodium chloride and 0.4-0.5 parts of isopropyl cyanoacetate by weight, and the diameter of the low-temperature expansion particles is 40-50 μm.

8. The composite hydrophobic material for inhibiting crystallization of tunnel drainage pipes according to claim 7, characterized in that: The hydrophobic inner layer comprises a first hydrophobic inner layer material and a second hydrophobic inner layer material in a mass ratio of 1:0.5-1.

5. The preparation method of the first hydrophobic inner layer material is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and then nano-silicon dioxide and a surfactant are sequentially added to the solution A and stirred for 4 to 6 minutes to obtain a solution B, and then a cross-linking agent and a curing agent are sequentially added to the solution B and stirred for 9 to 11 minutes, and after stirring, the first hydrophobic inner layer material is obtained; The preparation method of the second hydrophobic inner layer material is: at room temperature, tetrahydrofuran and a solvent volatile agent are first mixed to obtain a solution A, and the solution A is divided into two parts; Then, using ultrasound, the low temperature expansion particles are dispersed in one of the A solutions at a solid-liquid ratio of 1:1-2 for 8-10 minutes to obtain a C1 solution, and then using ultrasound, the hydrophobic microspheres are dispersed in another A solution at a solid-liquid ratio of 1:4-6 for 8-10 minutes to obtain a C2 solution; Then, nano-silica and surfactant are added to the C1 solution in sequence and stirred for 4 to 6 minutes to obtain a D solution. A cross-linking agent and a curing agent are added to the D solution in sequence and stirred for 9 to 11 minutes. The solution is semi-cured at 80 to 90° C. for 15 to 25 minutes to obtain a semi-cured material. The semi-cured material is then immersed in a C2 solution and completely cured at 100 to 105° C. to obtain a second hydrophobic inner layer material.

9. The method for preparing a composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe according to claim 5, characterized in that: The following steps are involved: S1. First, apply a layer of hydrophobic inner layer material with a thickness of ≤0.03cm on the inner wall of the pipeline; S2, waiting for the hydrophobic inner layer material to dry to obtain a hydrophobic inner layer; S3. Coat a scale-inhibiting outer layer material with a thickness of 0.15 to 0.25 cm on the outer surface of the hydrophobic inner layer, and obtain a composite material after drying.

10. The method for preparing a composite hydrophobic material for inhibiting crystallization of a tunnel drainage pipe according to claim 8, characterized in that: The following steps are involved: S1. First, a layer of the second hydrophobic inner layer material with a thickness of ≤0.03 cm is coated on the inner wall of the pipeline. The coating method is to use any point corresponding to the center of the pipeline as the center point, and then scatter multiple paths outward from the center point to coat, and the end point of the path returns to the center point. After coating, use a light dryer to dry and cure at 75-85°C for 5-10 minutes; S2. After the second hydrophobic inner layer material is dried, a layer of the first hydrophobic inner layer material with a thickness of ≤0.03 cm is applied to the blank area between the inner wall of the pipe and the second hydrophobic inner layer material, and dried in a hot air drying oven at 65-75° C. for 20-30 minutes to obtain a hydrophobic inner layer; S3. Apply a layer of anti-scaling outer layer material with a thickness of 0.15 to 0.25 cm to obtain a composite material.

Citation Information

Patent Citations

  • Scale inhibition base material, preparation method, scale inhibition film, scale inhibition ball and scale inhibition sheet

    CN113135619A

  • Scale inhibition coating as well as preparation method, construction method and application thereof

    CN117965095A