Composite fluxing agent for reducing melting point of coal ash as well as preparation method and application of composite fluxing agent
By using a composite flux made from industrial solid waste red mud and steel slag, the problem of high ash melting point coal ash and limited resource utilization of industrial solid waste is solved, and the effective reduction of coal ash melting point and coal gasification efficiency are achieved promote.
Patent Information
- Application Number
- CN202410779152.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-08
AI Technical Summary
High-ash melting point coal resources are abundant, but the flow temperature of its ash is high and cannot meet the requirements of entrained-bed gasifiers. Furthermore, the utilization of industrial solid waste resources is limited, and existing fluxes are costly and ineffective.
A composite flux made from industrial solid waste red mud and steel slag is crushed, screened and mixed in a ratio of 7:3 to 1:9, and then added to coal to reduce the melting point of coal ash for entrained bed coal gasification. middle.
It significantly reduces the melting point of Shanxi high-ash melting point coal ash, meets the requirements of entrained bed gasifiers, realizes resource utilization of industrial solid waste, reduces flux usage costs, and improves coal gasification efficiency.
Smart Images

Figure CN118745362A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flux, and in particular relates to a composite flux for reducing the melting point of coal ash, and a preparation method and application thereof. Background Art
[0002] Coal gasification technology is an important part of the modern coal chemical system. The development of efficient and clean coal gasification technology is of great significance to the promotion of my country's national energy development strategy. Entrained-bed gasification technology uses a relatively high reaction temperature (>1300℃) and pressure (~8MPa). Under these conditions, the conversion rate and reaction rate of organic matter in coal are almost the same. At this time, the evolution behavior of inorganic matter (ash, minerals, slag) in coal at high temperature, especially the liquid slag discharge process of slag, is the key factor affecting the long-term stable operation of the entrained-bed gasifier. Entrained-bed gasification technology has strict requirements on the ash melting point of raw coal. For water-coal slurry gasifiers using refractory bricks (such as Texaco gasifiers, OMB, etc.), the ash flow temperature (FT) is usually required to be between 1300 and 1400℃; for dry powder gasifiers using water-cooled walls (such as Shell gasifiers, aerospace furnaces, etc.), the gasification operating temperature must be 100 to 150℃ higher than the ash FT. At the same time, in order to prevent the corrosion of the refractory lining by the high-temperature slag and the ash accumulation problem in the syngas outlet cooler, the flow temperature of the fly ash cannot be too low.
[0003] my country is rich in high ash melting point coal resources (FT>1400℃), of which high ash melting point coal accounts for about 40% of the total coal resources in Shanxi. The main minerals in the coal ash are kaolin and mullite rich in acidic components such as silicon dioxide and aluminum oxide. Due to the high flow temperature of the coal ash of high ash melting point coal, it cannot meet the requirements of liquid slag discharge of entrained flow gasification and cannot be directly used for entrained flow gasification. Adding flux and coal blending are the main ways to regulate the melting characteristics of coal ash, but the coal blending method has the disadvantages of high transportation cost and difficult control. Therefore, adding flux is the best choice for regulating the melting characteristics of coal ash. However, the total silicon and aluminum of the coal ash of high ash melting point coal in Shanxi is greater than 80%, and the silicon-aluminum ratio is less than 2. The commonly used flux limestone in industry cannot reduce the flow temperature of Shanxi high ash melting point coal ash to below the requirements of the raw material coal ash melting point for entrained flow gasification. However, when the calcium oxide content in the coal ash is too high, part of the calcium oxide will exist in a free state, which will increase the melting point of the coal ash. In addition, the high amount of flux added leads to a decrease in coal gasification efficiency. When a single-component flux cannot effectively improve the melting characteristics of coal ash, a two-component composite flux is a better choice, which can not only reduce the excessive addition of a single-component flux, but also improve the fluxing efficiency by utilizing the synergistic fluxing effect between the two components. The results of previous studies have shown that calcium-iron composite flux has a significant synergistic effect on reducing the melting point of coal ash, which can reduce the amount of flux added and improve the overall efficiency of coal gasification.
[0004] Industrial solid waste as a whole faces problems such as huge output and unbalanced regional development, low industrialization conversion rate, supporting policies and relevant standards to be improved, and high investment pressure for comprehensive utilization projects. Industrial solid wastes such as phosphogypsum, steel slag, and red mud are rich in calcium and iron, and are high-quality raw materials for the preparation of calcium-iron composite fluxes. By using calcium-rich and iron-rich industrial solid wastes to prepare composite fluxes for coal gasification, not only can the resource utilization of industrial solid wastes be realized, but also the high cost of fluxes in entrained-bed gasification can be reduced. Summary of the invention
[0005] The main purpose of the present invention is to provide a composite flux for reducing the melting point of coal ash, and its preparation method and application, so as to realize the use of industrial solid waste to reduce the melting point of coal ash, and solve the current problems of high melting point of high ash ash and limited resource utilization of industrial solid waste.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] A composite flux for reducing the melting point of coal ash. The composite flux is composited from industrial solid waste red mud and steel slag.
[0008] Furthermore, the mass ratio of the industrial solid waste red mud and steel slag is 7:3 to 1:9.
[0009] A method for preparing a composite flux for reducing the melting point of coal ash as described above comprises the following steps: crushing and sieving industrial solid waste red mud and steel slag powder respectively to make the particles smaller than 75 μm, and then mixing them evenly in a mass ratio of 7:3 to 1:9 to obtain a composite flux for reducing the melting point of coal ash.
[0010] An application of the composite flux for reducing the melting point of coal ash as described above is used for reducing the melting point of coal ash in entrained flow coal gasification.
[0011] Furthermore, the method comprises the following steps: taking coal as a base, adding 2-8wt% into high ash melting point coal, mixing evenly and using the mixture as raw coal for the fluidized bed gasifier.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] (1) The composite flux is prepared by combining industrial solid waste red mud and steel slag. By adding 2-8wt% (coal-based) of the composite flux, the melting point of Shanxi high-ash melting point coal ash can be significantly reduced, so that it meets the requirements of entrained bed gasification for the melting point of coal ash, solving the technical problem that high-ash melting point coal cannot be used for entrained bed gasification. At the same time, industrial solid waste red mud and steel slag are rich in calcium oxide and iron oxide, which not only utilizes the synergistic effect of calcium and iron on reducing the melting point of coal ash, but also has low cost of use, which can reduce the cost of using flux in coal gasification and improve the overall benefits of coal gasification.
[0014] (2) The composite flux of the present invention is made by uniformly mixing industrial solid waste red mud and steel slag in a certain proportion, and has the characteristics of easy raw material availability, flexible proportioning, simple preparation and convenient use. At the same time, the synergistic effect of calcium oxide and iron oxide in industrial solid waste to reduce the melting point of coal ash is effectively utilized, realizing the resource utilization of industrial solid waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The effect of the composite flux prepared according to Example 3 on the ash melting point of high ash melting point coal from Lu'an, Shanxi. DETAILED DESCRIPTION
[0016] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0017] Example 1
[0018] Industrial solid waste red mud and steel slag powder were crushed and sieved separately to make the particles smaller than 75μm, and then fully mixed in a mass ratio of 1:9 to make a composite flux; the composite flux with a mass fraction of 2%, 4%, 6% and 8% (based on coal, the number of flux added to 100 parts of coal) was added to the high ash melting point coal from Lu'an, Shanxi, and mixed evenly. According to the Chinese national standard "GB / T219-2008 Determination of Fusibility of Coal Ash", the melting point of the high ash melting point coal ash from Lu'an, Shanxi after adding the composite flux was determined. The test results are shown in Table 4.
[0019] Example 2
[0020] Industrial solid waste red mud and steel slag powder were crushed and sieved separately to make the particles smaller than 75μm, and then fully mixed in a mass ratio of 3:7 to make a composite flux; the composite flux with a mass fraction of 2%, 4%, 6% and 8% (based on coal, the number of flux added to 100 parts of coal) was added to the high ash melting point coal from Lu'an, Shanxi, and mixed evenly. According to the Chinese national standard "GB / T219-2008 Determination of Fusibility of Coal Ash", the melting point of the high ash melting point coal ash from Lu'an, Shanxi after adding the composite flux was determined. The test results are shown in Table 5.
[0021] Example 3
[0022] Industrial solid waste red mud and steel slag powder were crushed and sieved separately to make the particles smaller than 75μm, and then fully mixed in a mass ratio of 5:5 to make a composite flux; the composite flux with a mass fraction of 2%, 4%, 6% and 8% (based on coal, the number of flux added to 100 parts of coal) was added to the high ash melting point coal from Lu'an, Shanxi, and mixed evenly. According to the Chinese national standard "GB / T219-2008 Determination of Fusibility of Coal Ash", the melting point of the high ash melting point coal ash from Lu'an, Shanxi after adding the composite flux was determined. The test results are shown in Table 6.
[0023] Example 4
[0024] Industrial solid waste red mud and steel slag powder were crushed and sieved separately to make the particles smaller than 75μm, and then fully mixed in a mass ratio of 7:3 to make a composite flux; the composite flux with a mass fraction of 2%, 4%, 6% and 8% (based on coal, the number of flux added to 100 parts of coal) was added to the high ash melting point coal from Lu'an, Shanxi, and mixed evenly. According to the Chinese national standard "GB / T219-2008 Determination of Fusibility of Coal Ash", the melting point of the high ash melting point coal ash from Lu'an, Shanxi after adding the composite flux was determined. The test results are shown in Table 7.
[0025] During use of the present invention, the amount of the composite flux added can be appropriately adjusted according to the requirements of the entrained bed gasification on the melting point of the coal ash.
[0026] The ash chemical composition of the Shanxi Lu'an high ash fusion point coal used in the present invention is shown in Table 1 and the ash fusion point is shown in Table 2, and the chemical composition of the red mud and steel slag is shown in Table 3.
[0027] Table 1 Chemical composition data of high ash melting point coal ash from Lu'an, Shanxi (wt%)
[0028] Coal Type <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[TiO2]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> <![CDATA[SO3]]> <![CDATA[P2O5]]> Lu'an 51.70 33.31 3.67 4.25 0.89 1.36 1.11 0.89 0.73 0.40
[0029] Table 2 Ash melting point data of high ash melting point coal from Lu'an, Shanxi (℃)
[0030] Coal Type DT ST HT FT Lu'an 1458 1500 >1500 >1500
[0031] (Note: DT: deformation temperature; ST: softening temperature; HT: hemisphere temperature; FT: flow temperature)
[0032] Table 3 Chemical composition data of red mud and steel slag powder (wt%)
[0033]
[0034] Table 4 Effect of composite flux (prepared according to Example 1) on the ash melting point of high ash melting point coal from Lu'an, Shanxi
[0035] Addition amount DT ST HT FT 2% 1311 1337 1347 1382 4% 1275 1289 1300 1338 6% 1245 1277 1290 1331 8% 1244 1269 1283 1332
[0036] Table 5 Effect of composite flux (prepared according to Example 2) on the ash melting point of high ash melting point coal in Lu'an, Shanxi
[0037]
[0038]
[0039] Table 6 Effect of composite flux (prepared according to Example 3) on the ash melting point of high ash melting point coal in Lu'an, Shanxi
[0040] Addition amount DT ST HT FT 2% 1328 1350 1372 1417 4% 1290 1301 1309 1338 6% 1248 1263 1271 1305 8% 1232 1250 1261 1307
[0041] Table 7 Effect of composite flux (prepared according to Example 4) on the ash melting point of high ash melting point coal from Lu'an, Shanxi
[0042] Addition amount DT ST HT FT 2% 1342 1376 1394 1443 4% 1300 1306 1316 1352 6% 1237 1255 1267 1317 8% 1227 1242 1252 1293
[0043] The above description is only for better explaining the embodiments of the present invention, and is not intended to limit the present invention. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.
Claims
1. A composite flux for reducing the melting point of coal ash, characterized in that: The composite flux is composited from industrial solid waste red mud and steel slag.
2. The composite flux for reducing the melting point of coal ash according to claim 1, characterized in that: The mass ratio of the industrial solid waste red mud to steel slag is 7:3 to 1:
9.
3. A method for preparing a composite flux for reducing the melting point of coal ash, characterized in that: The method comprises the following steps: crushing and sieving industrial solid waste red mud and steel slag powder respectively to make the particles smaller than 75 μm, and then mixing them evenly in a mass ratio of 7:3 to 1:9 to obtain a composite flux for reducing the melting point of coal ash.
4. An application of a composite flux for reducing the melting point of coal ash, characterized in that: The composite flux as claimed in any one of claims 1 or 2 is used in entrained-flow coal gasification to reduce the melting point of coal ash.
5. The use of the composite flux for reducing the melting point of coal ash according to claim 4, characterized in that: The following steps are involved: Taking coal as the base, 2-8wt% is added into high ash melting point coal, and after being evenly mixed, it is used as the raw coal of the entrained flow gasifier.