Process for selectively recovering thallium from thallium-containing smoke dust

Through the cyclic alkali leaching-purification-cyclone electroplating process, the problems of complicated processes, serious pollution, and large amounts of wastewater in the extraction technology of thallium-containing smoke and dust are solved, and the efficient resource utilization and environmental protection improvement of thallium are achieved.

CN118745519APending Publication Date: 2024-10-08CENT SOUTH UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411000505.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing thallium-containing smoke extraction technology has problems such as complicated processes, serious pollution, large amounts of wastewater, and low product purity, which limits the resource utilization of thallium.

Method used

The cyclic alkali leaching-purification-cyclone electrowinning process is used to selectively extract thallium through alkaline solution, use calcium oxide and other defluoridating agents to remove fluoride ions, use ion exchange and membrane exchange to separate chloride ions, reduce wastewater production, and use cyclone to remove fluorine ions. Recovery of thallium metal by galvanic deposition.

Benefits of technology

It achieves efficient enrichment and resource utilization of thallium, reduces the amount of waste water and toxic gas generation, and improves product purity and environmental protection of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004961447770000011
    Figure HDA0004961447770000011
Patent Text Reader

Abstract

The invention discloses a method for selectively recovering thallium from thallium-containing smoke dust. The method comprises the following steps: firstly, leaching thallium-containing smoke dust in alkali liquor with a certain concentration; if the material contains fluorine, a certain amount of fluorine removal agent can be added in the leaching process to remove fluorine in the form of fluoride precipitation. After leaching is completed, thallium enters the solution in the form of thallium hydroxide, and soluble heavy metals such as lead, zinc and cadmium are hydrolyzed and precipitated. And removing chloride ions in the thallium-containing filtrate by means of precipitation, ion exchange, membrane exchange and the like. And the dechlorinated liquid is recycled as a leaching agent of smoke dust to realize enrichment of thallium in the solution. And after thallium in the solution is enriched to a certain degree, thallium ions in the solution are converted into metal thallium through rotational flow electrodeposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a process for selectively extracting thallium from thallium-containing smoke, and belongs to the field of nonferrous metal metallurgy. Background Art

[0002] Thallium is a typical toxic heavy metal element and one of the 13 metal pollutants recognized as priority control in the world. Its toxicity is greater than that of Cd, Pb, and Hg. The toxic effect of thallium on the human body is mainly neurotoxicity, which can cause functional damage to multiple organs such as the kidneys and liver. In the non-ferrous metal smelting industry, thallium often enters the smoke in the form of flue gas, which in turn imposes a heavy burden on smelting and the environment. In addition, in order to alleviate the shortage of raw materials, and in recent years, the environmental protection department has increasingly tightened restrictions on the long-term storage of thallium-containing smoke by enterprises, and the demand for thallium-containing secondary resources in the smelting industry has become increasingly large.

[0003] However, the thallium in the thallium-containing dust can cause serious harm to the smelting system and on-site personnel. Taking wet zinc smelting as an example, since its deposition potential is more positive than zinc, the presence of thallium will cause the "burning plate" phenomenon in the zinc electrolysis process, reducing the quality of the product and even causing the inability to produce continuously normally. In addition, thallium-containing materials will also dissolve into groundwater and soil under the action of water and oxygen, and invade the human body through the food chain, skin contact and other channels, causing thallium poisoning in the human body. Therefore, based on normal smelting and human health, the removal of thallium in thallium-containing dust becomes extremely important.

[0004] At present, hydrometallurgy is the mainstream process for extracting thallium from thallium-containing smoke, including leaching-replacement method, leaching-extraction method, leaching-chlorination precipitation method, leaching-sulfide precipitation method, leaching-crystallization method, etc. Among them, the leaching-sulfide precipitation method is the more mainstream process. This method uses an alkaline solution as a leaching agent to make thallium enter the solution in the form of thallium hydroxide, while elements such as lead, zinc, and cadmium are hydrolyzed into the filter residue, thereby realizing the separation of thallium from other metal ions. Afterwards, a certain amount of sodium sulfide is added to the alkaline leaching solution to further enrich thallium in the form of thallium sulfide. Finally, a thallium sulfate solution is obtained by adding sulfuric acid to the thallium sulfide slag, which is subsequently recovered by replacement. As mentioned above, the existing mainstream process flow is complicated, and highly toxic hydrogen sulfide gas is generated during the production process, causing serious pollution to the environment. In addition, in the above processes, thallium is produced as a "crude thallium" product with relatively low purity, which makes it difficult to realize the resource utilization of thallium.

[0005] In summary, the current thallium extraction technology for thallium-containing soot has problems such as long process flow, large amount of wastewater, and low product added value, which has become a technical bottleneck restricting the secondary resource recycling of soot. Therefore, this field urgently needs to develop a new, environmentally friendly and efficient thallium resource extraction technology for thallium-containing soot. Summary of the invention

[0006] Aiming at the problems of long thallium extraction process, heavy pollution, large amount of wastewater and low added value of products in existing thallium-containing smoke, the present invention proposes to selectively extract thallium from thallium-containing smoke by using the method of circulating alkaline leaching-purification-cyclone electrolysis. First, the selective extraction of thallium in an alkaline system is realized by using the principle that thallium hydroxide dissolves in alkali and other metal ions are hydrolyzed. In addition, the opening of fluoride ions can be achieved by adding defluorinating agents such as calcium oxide during the alkaline leaching process. Afterwards, the residual chloride ions are separated from the thallium-containing leachate by means of adsorption, ion exchange, membrane exchange, etc., thereby avoiding the influence of chloride ions on the electrolysis process, and also avoiding the generation of slightly soluble thallium chloride. The thallium-containing leachate after dechlorination can continue to be used as a leaching agent to treat thallium-containing smoke. This process can not only achieve effective enrichment of thallium, but also greatly reduce the generation of thallium-containing wastewater. Finally, the circulating leachate is treated by cyclone electrodeposition to recover thallium in the form of metal.

[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0008] (1) Alkali dissolution and defluorination: Place the thallium-containing material in an alkaline solution and react for a certain period of time; for materials with a high fluorine content, a certain amount of defluorinating agent can be added during the reaction.

[0009] (2) Dechlorination of alkaline leaching solution: For materials with high soluble chlorine content, a suitable dechlorination method is required to remove all or part of the chloride ions in the alkaline leaching solution obtained in step (1).

[0010] (3) Circular leaching: The dechlorinated solution obtained in step (2) is used as a leaching agent to return to the leaching of thallium-containing dust, so that thallium is gradually enriched in the solution. The operation in step (2) needs to be repeated for each several cycles of the leaching solution, thereby avoiding the supersaturation precipitation of slightly soluble thallium chloride.

[0011] (4) Electrodeposition of thallium: The circulating leaching solution in step (3) is passed into a cyclonic electrolytic device, and a metal thallium plate is obtained after electrolysis for a period of time.

[0012] The alkaline solution in step (1) is one or more combinations of alkali metal hydroxide solutions.

[0013] Preferably, the alkaline solution in step (1) is a sodium hydroxide solution

[0014] The leaching pH endpoint range in step (1) is 4 to 14, and the specific judgment standard is the pH corresponding to the complete hydrolysis of impurity ions other than Tl.

[0015] The leaching temperature in step (1) is 25-100°C. Considering that the solubility of thallium chloride increases with temperature, the leaching temperature is preferably 50-100°C.

[0016] The leaching time in step (1) is 30 to 240 minutes, more preferably 60 to 120 minutes.

[0017] The defluorinating agent in step (1) is a substance that can form a precipitate with fluoride ions, such as calcium oxide; the amount added is 1.1 to 2 times the theoretical amount of defluorinating agent.

[0018] The dechlorination method in step (2) includes but is not limited to ultra-high lime aluminum method, ion exchange method and membrane separation method.

[0019] The number of cycles in step (3) depends on the saturated solubility of thallium hydroxide and the dechlorination effect in step (2), that is, during the cyclic leaching process, it should be ensured that TlOH will not be saturated and precipitated, and at the same time, TlCl will not be oversaturated and precipitated due to excessive chlorine.

[0020] The current density of the cyclone electrowinning process in step (4) is 100 to 500 A / m 2 , more preferably 200 to 400 A / m 2 .

[0021] Beneficial Effects

[0022] The present invention innovatively proposes to selectively extract thallium from thallium-containing dust by using a circulating alkaline leaching-purification-cyclone electrowinning route. Different from traditional extraction methods, the present invention has a short process flow, small amount of wastewater, low reagent consumption, high product added value, and does not produce toxic gases such as hydrogen sulfide. In addition, the present invention is not only suitable for treating thallium-containing dust in non-ferrous metal smelting processes, but can also be used to extract thallium from other multi-metal complex thallium-containing materials.

[0023] Taking thallium-containing zinc oxide dust as an example, the process principle of the present invention is described in detail as follows:

[0024] (1) Selective leaching of thallium

[0025] The selective leaching of thallium is based on the principle that thallium, thallium oxide and thallium sulfide react with alkali to enter the solution, and other metal elements react with alkali to form precipitation to achieve the selective dissolution of thallium. The specific reaction is as follows:

[0026] Tl+H 2 O=TlOH+H +

[0027] T1 2 O+H 2 O=2T1OH

[0028] T1 2 S+2NaOH=2T1OH+Na 2 S

[0029] In addition, soluble heavy metal ions such as zinc and cadmium will hydrolyze and precipitate under alkaline conditions.

[0030] CdSO 4 +2NaOH=Cd(OH) 2 ↓+Na 2 SO 4

[0031] ZnSO 4 +2NaOH=Zn(OH) 2 ↓+Na 2 SO 4

[0032] (2) Removal of fluoride and chloride ions

[0033] 2F - +Ca 2+ (s)=CaF 2 (s)↓(Taking calcium salt defluorination as an example)

[0034] 2Ca(OH) 2 +AlO 2 - +Cl - +2H 2 O=Ca 2 Al(OH) 6 Cl↓+2OH - (Take ultra-high lime aluminum method as an example)

[0035] (3) Cyclone Electrowinning Thallium Extraction

[0036] Cathode: Tl + +e=Tl

[0037] Anode: 4OH - -4e=H 2 O+O 2 BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 : Process flow chart of the present invention. DETAILED DESCRIPTION

[0039] The essential contents of the present invention are described below with examples, but the protection scope of the present invention is not limited thereto.

[0040] Example 1 (Fluorine-containing chlorine smoke)

[0041] The main components of zinc oxide smoke are Pb 21.3ωt.%, Zn 28.9ωt.%, Cd 7.23ωt.%, Tl1.44ωt.%, F 0.62ωt.%, and Cl 4.24ωt.%. Weigh 100g and 1g of smoke and calcium oxide respectively, control the end point pH to 9.5, and obtain the leachate after the liquid-solid ratio is 5 (mL): 1 (g), the leaching temperature is 80°C, and the leaching time is 2h. After that, a certain amount of sodium aluminate and calcium oxide are added to the alkaline leaching solution to react at 35°C for 50min. During the reaction, the molar ratio of calcium, aluminum, and chlorine is controlled to be 5:3:1. Then, the dechlorinated liquid is returned to leach the thallium-containing smoke, and dechlorination is performed after each leaching is completed. Finally, the metallic thallium in the solution is recovered by cyclonic electrolysis. At a solution flow rate of 300L / h and a current density of 300A / m 2 Metallic thallium was obtained by electrodeposition at 50°C for 90 minutes.

[0042] According to chemical testing and calculation, the average leaching rate of thallium during alkaline leaching and defluorination is 90.12%, the leaching rates of other metal elements are less than 0.1%, the leaching rate of fluorine is 1.2%, and the leaching rate of chlorine is 90.2%. After the alkaline leaching solution is dechlorinated by ultra-high lime aluminum method, the chlorine removal rate is 80%, and the chlorine content in the solution after dechlorination is 1.68g / L. After three cycles of purification and leaching, the concentration of thallium in the solution is 7.62g / L. After cyclone electrowinning, the concentration of thallium in the solution is reduced to 0.12g / L, and the thallium deposition rate and the purity of metal thallium are 98.21% and 94.69% respectively.

[0043] Example 2

[0044] The main components of zinc oxide smoke are Pb 23.4ωt.%, Zn 30.1ωt.%, Cd 5.63ωt.%, Tl0.62ωt.%, F 0.54ωt.%, and Cl 3.11ωt.%. Weigh 100g and 0.9g of smoke and calcium oxide respectively, control the end point pH to 9.5, and obtain the leachate after the liquid-solid ratio is 5 (mL): 1 (g), the leaching temperature is 80°C, and the leaching time is 2h. After that, a certain amount of sodium aluminate and calcium oxide are added to the alkaline leaching solution to react at 35°C for 50min. During the reaction, the molar ratio of calcium, aluminum, and chlorine is controlled to be 5:3:1. Then, the dechlorinated liquid is continued to leach thallium-containing smoke, and dechlorination is performed after each leaching is completed. Finally, the metallic thallium in the solution is recovered by cyclone electrolysis. At a solution flow rate of 300L / h and a current density of 300A / m 2 Metallic thallium was obtained by electrodeposition at 50°C for 90 minutes.

[0045] According to chemical testing and calculation, the average leaching rate of thallium during alkaline leaching and defluorination is 91.25%, the leaching rates of other metal elements are less than 0.1%, the leaching rate of fluorine is 1.12%, and the leaching rate of chlorine is 91.3%. After the alkaline leaching solution is dechlorinated by ultra-high lime aluminum method, the chlorine removal rate is 81.24%, and the chlorine content in the solution after dechlorination is 1.24g / L. After five cycles of purification and leaching, the concentration of thallium in the solution is 5.54g / L. After cyclone electrowinning, the concentration of thallium in the solution is reduced to 0.09g / L, and the thallium deposition rate and the purity of metal thallium are 97.98% and 95.21% respectively.

[0046] Example 3 (containing no fluorine or chlorine)

[0047] The main components of the waste catalyst are Ti 37.2ωt.%, V 2.1ωt.%, Mo 3.21ωt.%, Tl 5.62ωt.%, F 0.21ωt.%, and Cl 0.13ωt.%. Weigh 100g of the catalyst, control the end point pH to 9.5, and obtain the leachate at a liquid-solid ratio of 5 (mL): 1 (g), a leaching temperature of 80°C, and a leaching time of 2h. The waste catalyst is repeatedly treated with the above leachate as a leaching agent. After three cycles of leaching, the metal thallium in the solution is recovered by cyclonic electrolysis. At a solution flow rate of 300L / h and a current density of 300A / m 2 Metallic thallium was obtained by electrodeposition at 50°C for 120 min.

[0048] According to chemical testing and calculation, the average leaching rate of thallium in alkaline leaching is 92.35%, and the leaching rates of other metal elements are less than 0.1%. After three cycles of purification and leaching, the concentration of thallium in the solution is 30.23g / L. After cyclone electrowinning, the concentration of thallium in the solution is reduced to 0.087g / L, and the deposition rate of thallium and the purity of metal thallium are 98.78% and 96.21% respectively.

[0049] Example 4 (controlling pH 7.5, incomplete Cd precipitation)

[0050] The main components of zinc oxide smoke are Pb 21.3ωt.%, Zn 28.9ωt.%, Cd 7.23ωt.%, Tl1.44ωt.%, F 0.62ωt.%, and Cl 4.24ωt.%. Weigh 100g and 1g of smoke and calcium oxide respectively, control the end point pH7.5, and obtain the leachate after the liquid-solid ratio is 5 (mL): 1 (g), the leaching temperature is 80°C, and the leaching time is 2h. After that, a certain amount of sodium aluminate and calcium oxide are added to the alkaline leaching solution to react at 35°C for 50min. During the reaction, the molar ratio of calcium, aluminum, and chlorine is controlled to be 5:3:1. Then, the dechlorinated liquid is continued to leach thallium-containing smoke, and dechlorination is performed after each leaching is completed. Finally, the metallic thallium in the solution is recovered by cyclonic electrolysis. At a solution flow rate of 300L / h and a current density of 300A / m 2 Metallic thallium was obtained by electrodeposition at 50°C for 90 minutes.

[0051] According to chemical testing and calculation, the average leaching rate of thallium during alkaline leaching and defluorination is 89.01%, the leaching rates of lead and zinc are less than 0.1%, the leaching rate of cadmium is 20.12%, the leaching rate of fluorine is 0.5%, and the leaching rate of chlorine is 85.24%. After the alkaline leaching solution is dechlorinated by ultra-high lime aluminum method, the chlorine removal rate is 80%, and the chlorine content in the solution after dechlorination is 0.88g / L. After three cycles of purification and leaching, the concentration of thallium in the solution is 7.55g / L. After cyclone electrowinning, the concentration of thallium in the solution is reduced to 0.085g / L, and the deposition rate of thallium and the purity of metal thallium are 98.21% and 46.21% respectively.

[0052] Comparative Example 1 (without using cyclonic electrowinning)

[0053] The other conditions of Comparative Example 1 are the same as those of Example 1, except that the electrodeposition process does not use cyclone electrowinning, but uses a conventional electrolytic cell. The results show that the alkaline leaching, defluorination and dechlorination process indicators are very similar to those of Example 1. However, after cyclone electrowinning, the concentration of thallium in the solution is reduced to 5.65 g / L, and the deposition rate of thallium and the purity of metallic thallium are 25.31% and 93.89%, respectively.

Claims

1. A process for selectively recovering thallium from thallium-containing dust, characterized in that: The thallium-containing dust is placed in an alkaline solution of a certain concentration to leach the thallium into the solution in the form of thallium hydroxide, and other soluble metals are hydrolyzed and precipitated. If the raw material contains fluorine, a certain amount of defluorinating agent can be added during the alkaline leaching process. In addition, chloride ions in the solution can be removed by precipitation, ion exchange, membrane exchange and other means, thereby avoiding the precipitation of slightly soluble thallium chloride. The dechlorinated solution can be used as a leaching agent to circulate and leach smoke to achieve the enrichment of thallium in the solution. After the thallium in the solution is enriched to a certain extent, the thallium ions in the solution are converted into metallic thallium by electrodeposition.

2. A process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The alkaline solution is one or more combinations of alkali metal hydroxides. Preferably, the alkaline solution in step (1) is a sodium hydroxide solution.

3. A process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The leaching pH endpoint range is 4 to 14. Preferably, the endpoint is a pH corresponding to complete hydrolysis of impurity ions other than thallium.

4. A process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The leaching temperature is 25-100°C. Considering that the solubility of thallium chloride increases with temperature, the leaching temperature is preferably 50-100°C.

5. The process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The leaching time is 30 to 240 minutes, more preferably 60 to 120 minutes.

6. The process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The defluoridation agent is a substance that can form a precipitate with fluoride ions, such as calcium oxide; the amount of the defluoridation agent added is 1.1 to 2 times the theoretical amount of defluoridation.

7. The process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The dechlorination method refers to a method that can separate chloride ions in the alkaline leaching solution from the thallium-containing solution system without causing the thallium ions in the solution to precipitate. It includes but is not limited to ultra-high lime aluminum method, ion exchange method and membrane separation method.

8. The process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The number of cyclic leaching is the maximum number of times to ensure that TlOH will not saturate and precipitate, and that TlCl will not be supersaturated and precipitate due to excessive chlorine ion.

9. The process for selectively recovering thallium from thallium-containing dust according to claim 1, characterized in that: The method of extracting thallium by electrodeposition is cyclonic electrowinning. Preferably, the current density of the cyclone electrowinning process is 100-500 A / m 2 , more preferably 200 to 400 A / m 2 .

Citation Information

Cited By

  • Method for selectively recovering thallium from zinc-cadmium slag

    CN119530571A

  • Organic salt leaching separation method of thallium-chlorine-containing solid waste

    CN120861572A

  • Method for strengthening alkaline leaching separation of thallium in thallium-chlorine-containing solid waste

    CN120924819A