Multifunctional tent cloth and preparation method thereof
By modifying the water-based polyurethane coating and adding antibacterial fillers, the problem of poor water resistance of multi-functional tent coatings in outdoor environments is solved, the water resistance, mechanical and thermal insulation properties of the tent fabric are improved, the durability of the function is extended and the antibacterial properties are enhanced performance.
Patent Information
- Application Number
- CN202410765641.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-08
AI Technical Summary
When a multi-functional tent is exposed to the outdoor environment for a long time, especially under rainy conditions, the water resistance of its coating is poor, resulting in functional damage and affecting its service life.
Using modified water-based polyurethane coating, by adjusting the mass ratio of polypropylene glycol and polytetrahydrofuran alcohol, combined with alcohol polyurethane chain extender and silicone modifier, a coating with excellent water resistance and mechanical properties is formed, and titanium dioxide and titanium dioxide are added to the surface. Silica to improve thermal insulation properties, while antimicrobial fillers are added to enhance antimicrobial properties.
Significantly improve the water resistance, mechanical and thermal insulation properties of the tent fabric, extend the durability of the function, and enhance the antibacterial performance, ensuring the versatility and service life of the tent in complex environments.
Smart Images

Figure BDA0004892370320000181 
Figure BDA0004892370320000191
Abstract
Description
Technical Field
[0001] The present application relates to the field of tents, and in particular to a multifunctional tent cloth and a preparation method thereof. Background Art
[0002] As a type of tent, multifunctional tents have more properties, such as rainproof, breathable, heat-insulating, ventilated, anti-aging and other properties required by tents in different scenarios. Therefore, multifunctional tents are widely used in outdoor camping, temporary residences, temporary warehouses and other occasions. At present, multifunctional tents have expanded their application areas in other aspects due to their excellent and rich performance, such as fire rescue, disaster relief and flood control, field construction, leisure tourism, etc. Due to the application scenarios of multifunctional tents, the objective environment that multifunctional tents need to face is more complex.
[0003] At present, the preparation of multifunctional tents usually adopts coating to form a coating with functions such as waterproofing and heat insulation. For environmental protection considerations, water-based polyurethane coatings are often used, and because of the need to have multiple functions, a variety of functional additives need to be added. However, water-based polyurethane coatings have poor water resistance, and multifunctional additives will also affect the water resistance of the coating. Multifunctional tents usually need to be in an outdoor environment for a long time. If they are in an environment where it rains for a long time, the water washability of the coating is poor. After being exposed to rain for a long time, the coating is easily damaged, which affects the function of the multifunctional tent and directly affects the service life of the tent. Summary of the invention
[0004] In order to enable the multifunctionality of a multifunctional tent cloth to be maintained longer in a complex environment, the present application provides a multifunctional tent cloth and a preparation method thereof.
[0005] In the first aspect, the present application provides a multifunctional tent fabric, which adopts the following technical solution:
[0006] A multifunctional tent cloth comprises a modified three-proof base cloth, a multifunctional coating coated on the three-proof base cloth and a heat-insulating coating coated on the multifunctional coating, wherein the multifunctional coating comprises the following raw materials in parts by weight: 80-100 parts of modified waterborne polyurethane, 1-3 parts of anti-ultraviolet absorber, 5-10 parts of antibacterial filler, 20-30 parts of flame retardant, 1-2 parts of defoamer, 1-2 parts of silane coupling agent, 2-3 parts of crosslinking agent and 1-2 parts of thickener.
[0007] Preferably, the ultraviolet absorber is one or more combinations of ultraviolet absorbers UV-326, UV-328, and UV-531.
[0008] Preferably, the modified waterborne polyurethane is prepared from the following raw materials in parts by weight: 25-75 parts of polypropylene glycol, 25-75 parts of polytetramethylene ether glycol, 4-11 parts of silicone modifier, 4.5-7 parts of chain extender, 0.5-1 parts of isophorone diisocyanate, and 1-3 parts of ethylenediamine, and the mass ratio of the polypropylene glycol to the polytetramethylene ether glycol is 1-3:1-3.
[0009] By adopting the above technical scheme, polytetrahydrofuran ether diol is a polyether polyol with a primary hydroxyl terminal group, and there are more COC in its molecular chain, so it has better flexibility, and there is no -CH3 in its molecular side chain, the coplanarity of the molecular chain is better, the intermolecular force is larger, and there is no easily hydrolyzed ester group, so the waterborne polyurethane coating can have excellent water resistance and mechanical properties. The chain extender can adjust the hard segment ratio in the polyurethane molecular structure, thereby regulating the intramolecular force of the polyurethane. The greater the intramolecular force, the higher the mechanical properties of the polyurethane coating, and the water resistance can be improved to a certain extent, but the excessive intramolecular force will also affect the flexibility of the molecular chain, and reduce its mechanical properties, hydrophobicity, and water resistance.
[0010] In addition, because the intermolecular force of polytetrahydrofuran ether diol is large, the increase in the amount of addition can increase the fracture stress and elongation at break of the coating to varying degrees, but when the amount of addition is too much, the crystal grains of the soft segment of the polyurethane coating may continue to grow, and the large crystal grains cause the polyurethane film to become brittle, so the elongation at break and the fracture stress of the film decrease. The present application proposes a mass ratio of polypropylene glycol and polytetrahydrofuran ether diol, and the water-based polyurethane coating has good mechanical properties; and because the molecular structure of polytetrahydrofuran ether diol does not have a -CH3 side chain, the molecular structure has good regularity, so that the density of the polyurethane coating is improved, and the appropriate mass ratio of polypropylene glycol and polytetrahydrofuran ether diol can make it difficult for water molecules to enter the interior of the coating, so that the hydrophobicity and mechanical properties of the coating can achieve better performance accordingly.
[0011] Preferably, the organosilicon modifier comprises hydroxy silicone oil and double-terminal hydroxypropyl silicone oil, and the mass ratio of the hydroxy silicone oil to the double-terminal hydroxypropyl silicone oil is 1-4:3-7.
[0012] By adopting the above technical scheme, hydroxyl silicone oil and double-terminal hydroxypropyl silicone oil are respectively subjected to silicone block copolymerization modification of polytetramethylene ether glycol, so that the thermal stability and mechanical properties of the polyurethane coating can be improved, and by compounding hydroxyl silicone oil and double-terminal hydroxypropyl silicone oil, the introduction of a single hydroxyl silicone oil is likely to affect the water resistance of the polyurethane coating, while the compounding of hydroxyl silicone oil and double-terminal hydroxypropyl silicone oil, the double-terminal hydroxypropyl silicone oil can reduce the influence of hydroxyl silicone oil on water resistance.
[0013] Preferably, the chain extender is an alcohol polyurethane chain extender;
[0014] Preferably, the alcohol polyurethane chain extender includes one or more combinations of bisphenol A dihydroxyethyl ether, bisphenol A dihydroxypropyl ether, dimethylolbutyric acid, 1,4-butanediol, diethylene glycol, ethylene glycol, 1,6-hexanediol, and 1,4-dimethylolcyclohexane;
[0015] More preferably, the polyurethane chain extender includes bisphenol A dihydroxyethyl ether and 1,4-butanediol.
[0016] Preferably, the mass ratio of bisphenol A dihydroxyethyl ether to 1,4-butanediol is 4-6:0.5-1.
[0017] By adopting the above technical scheme, the alcohol polyurethane chain extender can increase the hard segment ratio in the polyurethane molecular structure, increase the intramolecular force of the polyurethane, improve the mechanical properties of the polyurethane coating, and improve the water resistance to a certain extent. Among them, bisphenol A dihydroxyethyl ether and bisphenol A dihydroxypropyl ether are aromatic diols, dimethylolbutyric acid, 1,4-butanediol, diethylene glycol, ethylene glycol, 1,6-hexanediol, and 1,4-dimethylolcyclohexane are aliphatic diols, and the molecular weight of aromatic diols is generally larger than that of aliphatic diols, and the cyclic structure has rigidity. The polyurethane prepared by using aromatic diols as chain extenders has good properties such as heat resistance, and among them, 1,4-butanediol, diethylene glycol, ethylene glycol, 1,6-hexanediol, and 1,4-dimethylol are small molecular diols, which are used in small amounts when used as polyurethane chain extenders, and have high requirements for the amount of addition. When compounded with large molecular aromatic diols, the dosage needs to be accurately controlled.
[0018] Preferably, the thermal insulation coating comprises 25-35 parts of polyurethane solution, 2.5-4.5 parts of titanium dioxide, 1.5-1.8 parts of silicon dioxide, and 0.5-1 part of JFC penetrant.
[0019] Preferably, the mass ratio of the polyurethane solution, titanium dioxide and silicon dioxide is 1:0.09-0.15:0.04-0.06.
[0020] By adopting the above technical solution, there are many pores in the silica aerogel, which makes the thermal conductivity very low and has excellent thermal insulation performance. Titanium dioxide reflects or absorbs ultraviolet rays and infrared rays to block convective heat and conductive heat in the environment. When titanium dioxide and silicon dioxide are added at the same time, the polyurethane thermal insulation coating formed can form a dense coating on the surface of the base fabric, reducing the heat transfer to the inside of the fabric. The barrier and reflective thermal insulation work at the same time, which can better improve the thermal insulation performance of the base fabric, and due to the density of the thermal insulation coating, the water resistance and mechanical properties of the base fabric can also be improved accordingly.
[0021] Preferably, the antibacterial filler is graphene oxide powder and illite, and the mass ratio of the graphene oxide powder to illite is 1:0.4-0.6.
[0022] By adopting the above technical scheme, the modified waterborne polyurethane multifunctional coating has good adhesion and waterproof properties, and is very suitable for the surface coating of tent fabrics. In addition, the waterborne polyurethane has amino groups, which can be chemically bonded with the carboxyl groups on the graphene oxide in the antibacterial filler, thereby improving the connection strength between the coating matrix and the filler, thereby improving the antibacterial properties of the coating and the life of the antibacterial properties; and the illite can absorb odors, so that the tent can reduce odors after use, and can also absorb bacteria and viruses, thereby improving the antibacterial and antibacterial effects of the coating.
[0023] In a second aspect, the present application provides a method for preparing a multifunctional tent fabric, using the following technical solution:
[0024] A method for preparing a multifunctional tent cloth comprises the following steps:
[0025] Step 1: Take a polyester base fabric, and perform a three-proof finishing on the polyester base fabric with a three-proof finishing liquid to obtain a three-proof base fabric;
[0026] Step 2: subjecting the three-proof base fabric to plasma modification treatment to obtain a modified three-proof base fabric;
[0027] Step 3: Wash the modified three-proof base fabric in ethanol and deionized water for 10-20 minutes respectively, then dry it at 80-100℃, and then apply multifunctional coating on the outside of the modified three-proof base fabric with a coating weight of 60-70g / m 2, After coating, dry at 110-160℃ for 5-7min to form a multifunctional coating on the outside of the three-proof base fabric;
[0028] Step 4: Apply heat-insulating coating on the multifunctional coating surface of the three-proof base fabric, and then dry it at 140-160℃ for 40-80s to form a heat-insulating coating on the surface of the surface-modified base fabric. The dry weight of the coating is controlled at 60-65g / m 2 , to make multifunctional tent cloth.
[0029] Preferably, the step of three-proof finishing in step 1 comprises: applying the three-proof finishing liquid on the polyester base fabric at a temperature of 10-30°C and a coating amount of 50-75g / m 2 The liquid-carrying rate is 35%-45%, and the impregnated base fabric is obtained; the impregnated base fabric is dried at 70-90°C for 1-2 minutes, and then baked at 140-150°C for 1-3 minutes to obtain the three-proof base fabric.
[0030] By adopting the above technical scheme, plasma treatment is performed on the polyester base fabric after the three-proof treatment, and amino groups can be grafted on the polyester surface. The amino groups can react with the functional groups in the functional coating subsequently sprayed on the surface of the base fabric to form chemical bonds, and the amino groups can also react with the carboxyl groups of graphene oxide to form amide bonds, so that the two are chemically bonded, making the graphene oxide in the coating more firmly connected.
[0031] The three-proof finishing liquid in the above steps is homemade, and the three-proof finishing liquid includes the following raw materials in parts by weight: 200-220 parts of deionized water and 40-60 parts of three-proof raw materials, and the three-proof raw materials include the following raw materials in parts by weight: 0.5-1 parts of emulsifier, 10-15 parts of lauryl methacrylate, 2-5 parts of methyl methacrylate, 25-30 parts of dodecafluoroheptyl methacrylate, 2-5 parts of silane coupling agent, 0.5-1 parts of initiator, 0.4-0.6 parts of foaming agent, and 0.5-0.7 parts of foam stabilizer.
[0032] In the three-proof finishing liquid, the emulsion prepared by dodecafluoroheptyl methacrylate has a low surface energy and can form a latex film on the surface of the polyester base fabric. It has good water and oil resistance, but its bonding ability with the polyester base fabric is weak. After adding methyl methacrylate, the emulsion forms a network structure, which can effectively improve the bonding ability with the polyester base fabric and improve the wear resistance of the polyester base fabric. Lauryl methacrylate can improve the softness and film-forming property of the latex film. The compound use of lauryl methacrylate and methyl methacrylate can not only improve the thermal stability of the polyester base fabric, but also form a hydrophobic layer on the surface of the polyester base fabric, improve the performance of the polyester fabric, and reduce the amount of three-proof finishing liquid. The foaming agent can make the emulsion form foam. When the temperature rises, the foam will become unstable, and the foam stabilizer can make the foam more stable and extend the life of the foam.
[0033] In summary, this application has the following beneficial effects:
[0034] 1. The present application adopts polytetramethylene glycol and polypropylene glycol to regulate the soft and hard segments of the polyurethane molecular chain, thereby adjusting the mechanical properties, hydrostatic pressure resistance, water washability and other properties of the polyurethane, and cooperates with the selection of alcohol polyurethane chain extenders to make the polyurethane coating have excellent water resistance and mechanical properties.
[0035] 2. The present application prepares a thermal insulation coating by compounding silica and titanium dioxide to reflect or absorb ultraviolet rays and infrared rays to block convective heat and conductive heat in the environment. By adding titanium dioxide and silica at the same time, the polyurethane thermal insulation coating formed can form a dense coating on the surface of the base fabric, reducing the transfer of heat to the inside of the fabric. The barrier and reflective thermal insulation work at the same time, which can better improve the thermal insulation performance of the base fabric. Moreover, due to the density of the thermal insulation coating, the water resistance and mechanical properties of the base fabric can also be improved accordingly.
[0036] 3. This application uses water-based polyurethane as the coating matrix, and improves the antibacterial properties of the coating by adding graphene oxide and illite. The base fabric is treated with plasma and dispersion to allow polyester to have certain multifunctionality and to improve the connection strength between the base fabric and the coating, making the multifunctionality of the tent fabric more durable. DETAILED DESCRIPTION
[0037] Preparation Example
[0038] Preparation Example 1
[0039] The preparation of the three-proof finishing liquid includes the following steps:
[0040] The three-proof base fabric is obtained by finishing the base fabric with a three-proof finishing liquid, and the three-proof finishing liquid includes the following raw materials: deionized water, emulsifier, lauryl methacrylate, methyl methacrylate, dodecafluoroheptyl methacrylate, silane coupling agent, initiator, foaming agent, and foam stabilizer.
[0041] Emulsifier selected: DNS-86 emulsifier; silane coupling agent selected: coupling agent SCA-V71E; initiator selected: initiator AIBI; foaming agent selected: sodium dodecyl sulfate; foam stabilizer selected: sodium hydroxyethyl cellulose.
[0042] Step 1: Add 20 kg of deionized water and 0.1 kg of DNS-86 emulsifier into a stirred reactor and mix and stir for 15 min at a speed of 600 r / min to obtain an emulsifier aqueous solution;
[0043] Step 2: Add 1.5 kg of lauryl methacrylate, 0.5 kg of methyl methacrylate, 3 kg of dodecafluoroheptyl methacrylate, 0.5 kg of coupling agent SCA-V71E, and 0.1 kg of initiator AIBI to the emulsifier aqueous solution, stir and mix at a speed of 700 r / min, a time of 35 min, and a temperature of 55° C., and then emulsify by high-speed shearing emulsifier at 4000 r / min to obtain a pre-emulsion;
[0044] Step 3: adding deionized water to the pre-emulsion to adjust the concentration of the pre-emulsion to 40 g / L;
[0045] Step 4: Add 0.06 kg of sodium dodecyl sulfate and 0.05 kg of sodium hydroxyethyl cellulose to the pre-emulsion in step 3, and perform foaming treatment through a foaming machine to obtain a three-proof finishing liquid.
[0046] Preparation Example 2
[0047] In the preparation of multifunctional coatings, the anti-ultraviolet absorber is selected as UV absorber UV-328, the flame retardant is selected as bromine antimony flame retardant (C7), the defoamer is selected as polyurethane system defoamer YS-T118 / T131, the silane coupling agent is selected as silane coupling agent KH-792, the cross-linking agent is selected as melamine cross-linking agent, and the thickener is selected as water-based polyacrylate thickener G1;
[0048] The following steps are involved:
[0049] Step 1: Prepare modified waterborne polyurethane, add 25kg of polypropylene glycol, 25kg of polytetramethylene glycol, 2.5kg of hydroxy silicone oil and 5kg of double-terminal hydroxypropyl silicone oil into a reactor, then add 4kg of bisphenol A dihydroxyethyl ether, heat to 80°C, control the initial R value of the system at 1.5, slowly drip 0.75kg of isophorone diisocyanate through a constant pressure separatory funnel, add 0.5kg of 1,4-butanediol after dripping, and add a catalyst dibutyltin dilaurate at the same time, react at 80°C for 2h, stop heating and reduce the temperature to 40°C, add 50kg of deionized water for high-speed emulsification and dispersion for 30min; add 0.2kg of ethylenediamine under ice bath conditions and then extend the chain for 2h; finally, remove the residual acetone by vacuum rotary evaporation to obtain a modified waterborne polyurethane with a solid content of about 35%;
[0050] Step 2: Weigh 9.5 kg of waterborne polyurethane, 0.2 kg of UV absorber UV-328, 2.5 kg of bromine antimony flame retardant (C7), 1 kg of antibacterial filler (including 0.72 kg of graphene oxide powder and 0.28 kg of illite), 0.15 kg of polyurethane system defoamer YS-T118 / T131, 0.2 kg of waterborne polyacrylate thickener G1, 0.15 kg of silane coupling agent KH-792, 0.2 kg of melamine cross-linking agent; firstly, the water-based polyurethane and the antibacterial filler were mixed and stirred for 15 minutes at a speed of 150 r / min, and then ultraviolet absorber UV-328, polyurethane system defoamer YS-T118 / T131, silane coupling agent KH-792, and melamine cross-linking agent were added, and the stirring was continued at a speed of 150 r / min. The viscosity of the system was adjusted to 12000 mPa·s by adding water-based polyacrylate thickener G1 to prepare a multifunctional coating.
[0051] Preparation Example 3
[0052] The difference between Preparation Example 3 and Preparation Example 2 is that 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether glycol in step 1 are replaced by 2.5 kg of polypropylene glycol and 7.5 kg of polytetramethylene ether glycol.
[0053] Preparation Example 4
[0054] The difference between Preparation Example 4 and Preparation Example 2 is that 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether glycol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene ether glycol.
[0055] Preparation Example 5
[0056] The difference between Preparation Example 5 and Preparation Example 2 is that 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether glycol in step 1 are replaced by 7.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether glycol.
[0057] Preparation Example 6
[0058] The difference between Preparation Example 6 and Preparation Example 2 is that 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether glycol in step 1 are replaced by 5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether glycol.
[0059] Preparation Example 7
[0060] The difference between Preparation Example 7 and Preparation Example 2 is that: 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene glycol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene glycol; 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.4 kg of dihydroxymethylbutyric acid.
[0061] Preparation Example 8
[0062] The difference between Preparation Example 8 and Preparation Example 2 is that: 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene glycol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene glycol; 0.75 kg of 1,4-butanediol is replaced by 0.75 kg of ethylene glycol.
[0063] Preparation Example 9
[0064] The difference between Preparation Example 9 and Preparation Example 2 is that: 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene glycol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene glycol; 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.6 kg of bisphenol A dihydroxyethyl ether.
[0065] Preparation Example 10
[0066] The difference between Preparation Example 10 and Preparation Example 2 is that: 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene glycol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene glycol; 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.5 kg of bisphenol A dihydroxyethyl ether.
[0067] Preparation Example 11
[0068] The difference between Preparation Example 11 and Preparation Example 2 is that: the 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether diol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene ether diol; 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.5 kg of bisphenol A dihydroxyethyl ether, and 0.5 kg of 1,4-butanediol is replaced by 1 kg of 1,4-butanediol.
[0069] Preparation Example 12
[0070] The difference between Preparation Example 12 and Preparation Example 2 is that: 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether diol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene ether diol; 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.5 kg of bisphenol A dihydroxyethyl ether, and 0.5 kg of 1,4-butanediol is replaced by 0.75 kg of 1,4-butanediol.
[0071] Preparation Example 13
[0072] The difference between Preparation Example 13 and Preparation Example 2 is that: 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether diol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene ether diol; 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.5 kg of bisphenol A dihydroxyethyl ether; 1 kg of antibacterial filler (including 0.72 kg of graphene oxide powder and 0.28 kg of illite) in step 2 is replaced by 1 kg of antibacterial filler (including 0.625 kg of graphene oxide powder and 0.375 kg of illite).
[0073] Preparation Example 14
[0074] The difference between Preparation Example 14 and Preparation Example 2 is that: 2.5 kg of polypropylene glycol and 2.5 kg of polytetramethylene ether diol in step 1 are replaced by 2.5 kg of polypropylene glycol and 5 kg of polytetramethylene ether diol; 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.5 kg of bisphenol A dihydroxyethyl ether; 1 kg of antibacterial filler (including 0.72 kg of graphene oxide powder and 0.28 kg of illite) in step 2 is replaced by 1 kg of antibacterial filler (including 0.67 kg of graphene oxide powder and 0.33 kg of illite).
[0075] Preparation Example 15
[0076] The preparation of the thermal insulation coating includes the following steps: the silicon dioxide is selected as silicon dioxide aerogel; the titanium dioxide is selected as rutile titanium dioxide; 0.27 kg of rutile titanium dioxide and 0.12 kg of silicon dioxide aerogel are added to 3 kg of polyurethane solution, and then 0.1 kg of JFC penetrant is added dropwise, and stirred for 30 minutes to make it evenly dispersed, so as to prepare the thermal insulation coating.
[0077] Preparation Example 16
[0078] The difference between Preparation Example 16 and Preparation Example 15 is that 0.27 kg of rutile titanium dioxide is replaced by 0.45 kg of rutile titanium dioxide.
[0079] Preparation Example 17
[0080] The difference between Preparation Example 17 and Preparation Example 15 is that 0.27 kg of rutile titanium dioxide is replaced by 0.36 kg of rutile titanium dioxide.
[0081] Preparation Example 18
[0082] The difference between Preparation Example 18 and Preparation Example 15 is that 0.27 kg of rutile titanium dioxide and 0.12 kg of silica aerogel are replaced by 0.36 kg of rutile titanium dioxide and 0.18 kg of silica aerogel.
[0083] Preparation Example 19
[0084] The difference between Preparation Example 19 and Preparation Example 15 is that 0.27 kg of rutile titanium dioxide and 0.12 kg of silica aerogel are replaced by 0.36 kg of rutile titanium dioxide and 0.15 kg of silica aerogel.
[0085] Preparation Example 20
[0086] The difference between Preparation Example 20 and Preparation Example 2 is that 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.3 kg of bisphenol A dihydroxyethyl ether.
[0087] Preparation Example 21
[0088] The difference between Preparation Example 21 and Preparation Example 2 is that 0.4 kg of bisphenol A dihydroxyethyl ether is replaced by 0.7 kg of bisphenol A dihydroxyethyl ether.
[0089] Preparation Example 22
[0090] The difference between Preparation Example 22 and Preparation Example 2 is that no double-terminal hydroxypropyl silicone oil is added in step 1.
[0091] Preparation Example 23
[0092] The difference between Preparation Example 23 and Preparation Example 15 is that 0.27 kg of rutile titanium dioxide is added to 3 kg of polyurethane solution, and then 0.1 kg of JFC penetrant is added dropwise, and stirred for 30 minutes to make it evenly dispersed, thereby preparing a thermal insulation coating.
[0093] Preparation Example 24
[0094] The difference between Preparation Example 24 and Preparation Example 15 is that 0.12 kg of silica aerogel is added to 3 kg of polyurethane solution, and then 0.1 kg of JFC penetrant is added dropwise, and stirred for 30 minutes to make it evenly dispersed, thereby preparing a thermal insulation coating.
[0095] Example
[0096] Example 1
[0097] A method for preparing a multifunctional tent cloth comprises the following steps:
[0098] Step 1: Take a polyester base fabric and apply the three-proof finishing liquid in Preparation Example 1 on the polyester base fabric at a temperature of 20°C and a coating amount of 60g / m 2 , the liquid carrying rate is 40%, then dried at 70-90℃ for 2min, and then baked at 145℃ for 2min to obtain the three-proof base fabric;
[0099] Step 2: Use normal temperature and pressure plasma equipment to perform plasma modification on the three-proof base fabric, and the normal temperature and pressure plasma process parameters are: time 120s, power 100W, ammonia 35L / min, ammonia 0.6L / min, to obtain a modified three-proof base fabric;
[0100] Step 3: The modified three-proof base fabric was washed in ethanol and deionized water for 15 minutes respectively, and then dried at 100°C, and then the multifunctional coating in Preparation Example 2 was coated on the outside of the modified three-proof base fabric, with a coating weight of 65g / m 2, After coating, it is dried at 120℃ for 2min, then dried at 150℃ for 2min, and finally dried at 120℃ for 2min to form a multifunctional coating on the outside of the three-proof base fabric;
[0101] Step 4: The heat-insulating coating in Preparation Example 15 is applied to the multifunctional coating surface of the three-proof base fabric, and then dried at 150°C for 60 seconds to form a heat-insulating coating on the surface of the surface-modified base fabric. The dry weight of the coating is controlled at 60 g / m 2 , to make multifunctional tent cloth.
[0102] Example 2
[0103] The difference between Example 2 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 3.
[0104] Example 3
[0105] The difference between Example 3 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 4.
[0106] Example 4
[0107] The difference between Example 4 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 5.
[0108] Example 5
[0109] The difference between Example 5 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 6.
[0110] Example 6
[0111] The difference between Example 6 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 7.
[0112] Example 7
[0113] The difference between Example 7 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 8.
[0114] Example 8
[0115] The difference between Example 8 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 9.
[0116] Example 9
[0117] The difference between Example 9 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 10.
[0118] Example 10
[0119] The difference between Example 10 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 11.
[0120] Embodiment 11
[0121] The difference between Example 11 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 12.
[0122] Example 12
[0123] The difference between Example 12 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 13.
[0124] Example 13
[0125] The difference between Example 13 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 14.
[0126] Embodiment 14
[0127] The difference between Example 14 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 14, and the thermal insulation coating in Preparation Example 15 used in step 4 is replaced by the thermal insulation coating in Preparation Example 16.
[0128] Embodiment 15
[0129] The difference between Example 15 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 14, and the thermal insulation coating in Preparation Example 15 used in step 4 is replaced by the thermal insulation coating in Preparation Example 17.
[0130] Example 16
[0131] The difference between Example 16 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 14, and the thermal insulation coating in Preparation Example 15 used in step 4 is replaced by the thermal insulation coating in Preparation Example 18.
[0132] Embodiment 17
[0133] The difference between Example 17 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 14, and the thermal insulation coating in Preparation Example 15 used in step 4 is replaced by the thermal insulation coating in Preparation Example 19.
[0134] Comparative Example
[0135] Comparative Example 1
[0136] The difference between Comparative Example 1 and Example 1 is that the polyester base fabric is not subjected to the three-proofing finishing in step 1, but is directly subjected to the plasma modification in step 2.
[0137] Comparative Example 2
[0138] The difference between Comparative Example 2 and Example 1 is that the three-proof base fabric is not subjected to plasma modification in step 2, and is directly subjected to forming a multifunctional coating in step 3.
[0139] Comparative Example 3
[0140] The difference between Comparative Example 3 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 20.
[0141] Comparative Example 4
[0142] The difference between Comparative Example 4 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 21.
[0143] Comparative Example 5
[0144] The difference between Comparative Example 5 and Example 1 is that the multifunctional coating in Preparation Example 2 used in step 3 is replaced by the multifunctional coating in Preparation Example 22.
[0145] Comparative Example 6
[0146] The difference between Comparative Example 6 and Example 1 is that the thermal insulation coating in Preparation Example 15 used in step 4 is replaced with the thermal insulation coating in Preparation Example 23.
[0147] Comparative Example 7
[0148] The difference between Comparative Example 7 and Example 1 is that the thermal insulation coating in Preparation Example 15 used in step 4 is replaced with the thermal insulation coating in Preparation Example 24.
[0149] Performance testing
[0150] Antibacterial properties: The antibacterial properties of Examples 1-17 and Comparative Examples 1-7 were tested according to the standard of GB / T20944.3-2008 “Evaluation of antibacterial properties of textiles”.
[0151] Flame retardant performance: Flame retardant performance test is carried out in accordance with GB / T5456-2009 "Determination of flame spread performance of vertical direction test specimens for combustion performance of textiles".
[0152] Thermal insulation performance: dig a hole with a diameter of 15c in a closed insulation foam box, place the cloth sample on it, place a 200W bulb 30cm above the cloth sample to simulate sunlight, place a heat probe inside and outside the cloth sample, connect a display to display the change of the temperature difference between the inside and outside over time, and calculate the temperature difference between the inside and outside at 30 minutes to evaluate the thermal insulation effect of the cloth sample.
[0153] Resistance to hydrostatic pressure: The multifunctional tent fabrics of Examples 1-17 and Comparative Examples 1-7 were washed 10 times according to the AATCC 135modify standard and then dried. Then, the hydrostatic pressure resistance of the tent fabrics was tested before and after washing using a digital water permeability tester in accordance with GB / T4744-2013 "Hydrostatic Pressure Method for Testing and Evaluation of Waterproof Properties of Textiles".
[0154] Breaking strength: The multifunctional tent fabrics of Examples 1-17 and Comparative Examples 1-7 were cut into 5 cm × 20 cm warp and weft specimen strips along the yarn path, and then tested in accordance with GB / T 3923.1-2013 “Tensile properties of textile fabrics Part 1: Determination of breaking strength and elongation at break (strip method)”.
[0155]
[0156]
[0157] Table 1 Performance test of Examples 1-17 and Comparative Examples 1-7
[0158] Combining Examples 1-13 and Comparative Examples 1-4 and Table 1, it can be seen that as the proportion of polytetramethylene ether glycol increases, the hydrostatic pressure resistance of the tent cloth first increases and then decreases; when the ratio of polypropylene glycol to polytetramethylene ether glycol is 1:2, the hydrostatic pressure resistance, water washability, thermal insulation performance and breaking strength of the tent cloth all reach optimal values. Considering comprehensively, the ratio of polypropylene glycol to polytetramethylene ether glycol in Example 3 is optimal. It can be seen from Examples 4-12 that bisphenol A dihydroxyethyl ether can reduce the particle size of the aqueous polyurethane emulsion, thereby improving the dispersibility. The increase in the amount of bisphenol A dihydroxyethyl ether leads to an increase in the proportion of hard segments in the polyurethane molecular structure, and the intramolecular force of the polyurethane becomes larger, thereby improving the fracture strength and hydrostatic pressure resistance. In addition, bisphenol A dihydroxyethyl ether is better than other types of aromatic diol chain extenders, but when the amount of bisphenol A dihydroxyethyl ether is excessive, the fracture strength decreases to a certain extent. This may be because the proportion of hard segments in the polyurethane molecular chain is too high at this time, and the molecular chain movement is more difficult, and the hydrostatic pressure resistance of the tent cloth is affected. Another small molecule chain extender uses 1,4-butanediol for better results, and with the fine adjustment of the amount of 1,4-butanediol, the performance of the tent cloth also changes. The amount of graphene oxide powder and illite added has different effects on the antibacterial properties of the tent cloth. When the addition ratio of graphene oxide powder and illite in Example 13 is the best, the antibacterial property is the best. It can be seen from Comparative Examples 1-2 that whether the polyester base fabric is subjected to three-proof treatment and plasma treatment will affect the bonding strength of the subsequent coating and the performance of the base fabric itself, thereby affecting the antibacterial performance, thermal insulation performance, hydrostatic pressure resistance, washability, thermal insulation performance, and breaking strength. Therefore, it can be seen that the three-proof treatment and plasma treatment can effectively improve the performance of the tent fabric.
[0159] Combining Examples 14-17 and Comparative Examples 5-6 and Table 1, it can be seen that when the ratio of titanium dioxide to silicon dioxide in the thermal insulation coating is different, the thermal insulation performance and breaking strength of the tent cloth are affected to a certain extent. However, when too much titanium dioxide and silicon dioxide are added, it is easy to affect the mechanical properties of the tent cloth, thereby affecting the breaking strength. It can be seen from the comparative example that when titanium dioxide and silicon dioxide are used in combination, the thermal insulation performance is better than that of using titanium dioxide or silicon dioxide alone.
[0160] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A multifunctional tent cloth, characterized in that: The multifunctional tent fabric comprises a modified three-proof base fabric, a multifunctional coating coated on the three-proof base fabric, and a heat-insulating coating coated on the multifunctional coating. The multifunctional coating is prepared from the following raw materials in parts by weight: 80-100 parts of modified waterborne polyurethane, 1-3 parts of anti-ultraviolet absorber, 5-10 parts of antibacterial filler, 20-30 parts of flame retardant, 1-2 parts of defoamer, 1-2 parts of silane coupling agent, 2-3 parts of crosslinking agent, and 1-2 parts of thickener.
2. A multifunctional tent fabric according to claim 1, characterized in that: The modified waterborne polyurethane comprises the following raw materials in parts by weight: 25-75 parts of polypropylene glycol, 25-75 parts of polytetramethylene ether glycol, 4-11 parts of an organosilicon modifier, 4.5-7 parts of a chain extender, 0.5-1 parts of isophorone diisocyanate, and 1-3 parts of ethylenediamine, wherein the mass ratio of the polypropylene glycol to the polytetramethylene ether glycol is 1-3:1-3.
3. The multifunctional tent fabric according to claim 2, characterized in that: The organosilicon modifier comprises hydroxy silicone oil and double-terminal hydroxypropyl silicone oil, and the mass ratio of the hydroxy silicone oil to the double-terminal hydroxypropyl silicone oil is 1-4:3-7.
4. The multifunctional tent fabric according to claim 2, characterized in that: The chain extender is an alcohol polyurethane chain extender; Preferably, the alcohol polyurethane chain extender includes one or more combinations of bisphenol A dihydroxyethyl ether, bisphenol A dihydroxypropyl ether, dimethylolbutyric acid, 1,4-butanediol, diethylene glycol, ethylene glycol, 1,6-hexanediol, and 1,4-dimethylolcyclohexane; More preferably, the polyurethane chain extender includes bisphenol A dihydroxyethyl ether and 1,4-butanediol.
5. The multifunctional tent fabric according to claim 2, characterized in that: The mass ratio of the bisphenol A dihydroxyethyl ether to 1,4-butanediol is 4-6:0.5-1.
6. The multifunctional tent fabric according to claim 1, characterized in that: The heat-insulating coating comprises 25-35 parts of polyurethane solution, 2.5-4.5 parts of titanium dioxide, 1.5-1.8 parts of silicon dioxide, and 0.5-1 part of JFC penetrant.
7. The multifunctional tent fabric according to claim 6, characterized in that: The mass ratio of the polyurethane solution, titanium dioxide and silicon dioxide is 1:0.09-0.15:0.04-0.
06.
8. The multifunctional tent fabric according to claim 1, characterized in that: The antibacterial filler is graphene oxide powder and illite, and the mass ratio of the graphene oxide powder to the illite is 1:0.4-0.
6.
9. A method for preparing a multifunctional tent fabric, characterized in that: The following steps are involved: Step 1: Take a polyester base fabric, and perform a three-proof finishing on the polyester base fabric with a three-proof finishing liquid to obtain a three-proof base fabric; Step 2: subjecting the three-proof base fabric to plasma modification treatment to obtain a modified three-proof base fabric; Step 3: Wash the modified three-proof base fabric in ethanol and deionized water for 10-20 minutes respectively, then dry it at 80-100℃, and then apply multifunctional coating on the outside of the modified three-proof base fabric with a coating weight of 60-70g / m 2, After coating, dry at 110-160℃ for 5-7min to form a multifunctional coating on the outside of the three-proof base fabric; Step 4: Apply heat-insulating coating on the multifunctional coating surface of the three-proof base fabric, and then dry it at 140-160℃ for 40-80s to form a heat-insulating coating on the surface of the surface-modified base fabric. The dry weight of the coating is controlled at 60-65g / m 2 , to make multifunctional tent cloth.
10. The method for preparing a multifunctional tent fabric according to claim 9, characterized in that: The step of three-proof finishing in step 1 comprises: applying the three-proof finishing liquid on the polyester base fabric at a temperature of 10-30° C. and a coating amount of 50-75 g / m 2 , the liquid carrying rate is 35%-45%, and the base fabric after being soaked in liquid is obtained; Dry the soaked base fabric at 70-90℃ for 1-2min, and then bake at 140-150℃ for 1-3min. A three-proof base fabric is obtained.