Super imitation leather artificial synthetic leather and processing method thereof
By adding anti-tear, anti-corrosion, flame retardant and waterproof agents to artificial synthetic leather, and adopting specific raw material formulas and processing methods, the problem of single performance of existing synthetic leather is solved, and its service life and performance are significantly improved.
Patent Information
- Application Number
- CN202411020381.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-08
AI Technical Summary
Existing artificial synthetic leather has relatively single performance, resulting in a limited service life.
By adding anti-tear additives, preservatives, flame retardants and waterproofing agents to the raw materials, combined with specific formulas and processing methods of microfiber non-woven fabrics, dips and fabrics, the tensile properties and anti-corrosion properties of synthetic leather can be improved , flame retardant performance and waterproof performance.
Significantly improves the service life of artificial synthetic leather and improves its tensile strength, anti-corrosion grade, waterproof grade and flame retardant grade.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of synthetic leather, in particular to a super-simulated leather artificial synthetic leather and a processing method thereof. Background Art
[0002] Artificial synthetic leather is made of foamed or laminated PVC and PU with various formulations on a textile or non-woven base. It can be processed according to different strength, color, gloss, pattern and other requirements. It has the characteristics of a wide variety of patterns, good waterproof performance, neat edges, high utilization rate and relatively cheaper price than genuine leather.
[0003] However, the existing artificial synthetic leather has a relatively simple performance, which will affect the service life of the artificial synthetic leather to a certain extent, and has limitations. Therefore, a super-simulated leather artificial synthetic leather and a processing method thereof are invented. Summary of the invention
[0004] In view of the above and / or existing problems in a prior art super-simulated leather artificial synthetic leather and a processing method thereof, the present invention is proposed.
[0005] Therefore, the purpose of this invention is to provide a kind of super-simulation leather artificial synthetic leather and processing method thereof, can solve the above-mentioned existing problems proposed.
[0006] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0007] A super-simulated leather artificial synthetic leather, comprising a superfine fiber non-woven fabric, a soaking material raw material, a fabric raw material and a preparation raw material, wherein the soaking material raw material comprises, by weight: 10-20 parts of polyurethane, 10-15 parts of dimethylformamide, 6-8 parts of toluene color resistant paste, 4-8 parts of soaking aid, 2-10 parts of tearing aid, 6-10 parts of hydrolysis resistance aid, 6-10 parts of preservative, and 4-8 parts of flame retardant;
[0008] The fabric raw materials include, by weight: 10-15 parts of wood fiber powder, 6-10 parts of pigment, 4-8 parts of additives, 6-10 parts of calcium carbonate, 2-6 parts of nonionic surfactant, and 6-8 parts of waterproofing agent;
[0009] The raw materials for preparation include, by weight: 8-12 parts of dimethylformamide, 4-8 parts of toluene solution, and 2-6 parts of oil agent.
[0010] As a preferred embodiment of the super-simulated leather artificial synthetic leather described in the present invention, the impregnation auxiliary agent is composed of alkaline protease, non-ionic surfactant and pH buffer.
[0011] As a preferred embodiment of the super-simulated leather artificial synthetic leather described in the present invention, the anti-tear additive is composed of graphene, chlorinated wax, anti-tear finishing liquid, dispersant, glyceryl monostearate, leveling agent, penetrant, thickener and deionized water.
[0012] As a preferred embodiment of the super-simulated leather artificial synthetic leather of the present invention, the hydrolysis-resistant auxiliary agent is composed of hydrolysis-resistant polyhexamethylene adipamide resin, polyketone resin and hydrolysis-resistant glass fiber.
[0013] As a preferred embodiment of the super-simulated leather artificial synthetic leather described in the present invention, the raw materials of the preservative include, by weight, 12-14 parts of sorbic acid, 6-10 parts of sucrose fatty acid ester, 4-8 parts of acetic acid, 2-6 parts of paraffin, 4-10 parts of sodium molybdate, 2-6 parts of diatomaceous earth, and 4-8 parts of epoxy resin.
[0014] As a preferred embodiment of the super-simulated leather artificial synthetic leather of the present invention, the preparation process of the preservative is as follows:
[0015] Process 1: placing sorbic acid, sucrose fatty acid ester, acetic acid and paraffin in a reaction kettle and mixing them;
[0016] Process 2: Sodium molybdate, diatomaceous earth and epoxy resin are placed in a reaction kettle and mixed;
[0017] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0018] As a preferred embodiment of the super-simulated leather artificial synthetic leather of the present invention, the flame retardant is composed of alkylphenol polyoxyethylene ether, pentaerythritol, tetrabromobisphenol, an active agent and an emulsifier.
[0019] As a preferred embodiment of the super-simulated leather artificial synthetic leather of the present invention, the waterproofing agent is composed of linoleic acid, vaseline, sodium hydroxide, aluminum oxide, ethanol, hydrogen silicone oil emulsion and soap powder.
[0020] As a preferred embodiment of the super-simulated leather artificial synthetic leather of the present invention, the preparation process of the waterproofing agent is as follows:
[0021] Process 1: linoleic acid, vaseline, sodium hydroxide and aluminum oxide are placed in a reaction kettle and mixed;
[0022] Process 2: placing ethanol, hydrogen silicone oil emulsion and soap powder in a reaction kettle for mixing;
[0023] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a waterproofing agent.
[0024] A method for processing super-simulated artificial synthetic leather comprises the following specific steps:
[0025] Step 1, preparing the impregnation material: mixing polyurethane, dimethylformamide, toluene-resistant paste, impregnation aid, tear-resistant aid, hydrolysis-resistant aid, preservative and flame retardant, specifically, stirring at a stirring speed of 1200 r / min at room temperature, and controlling the solution viscosity at 100 cps;
[0026] Step 2, fabric preparation: wood fiber powder, pigment, additive, calcium carbonate, non-ionic surfactant, and waterproofing agent are mixed. Specifically, stirring is performed at a stirring speed of 1400r / min at room temperature. After stirring evenly, the stirring speed is reduced to 500r / min for vacuum degassing for 60 minutes, and the solution viscosity is controlled at 15000cps;
[0027] Step 3: Using ultrafine fiber non-woven fabric as the base fabric, using a wet high-density one-step method, the impregnation and coating are carried out simultaneously, and then entering a coagulation tank containing dimethylformamide for coagulation, and after coagulation, entering a water washing tank for water washing;
[0028] Step 4, sending the semi-finished product after step 3 into a reduction tank, which is filled with a toluene solution. Under the action of the toluene solution, the sea component is dissolved. After multiple tanks of dissolution, the PET in the ultrafine fiber non-woven fabric is extracted and dissolved, and then washed with boiling water to achieve the opening of the ultrafine fiber, and obtain the opened semi-finished product;
[0029] Step 5: Apply oil to the semi-finished fiber-opening product to increase the softness of the bass, and then stretch, grind and polish the leather to obtain super-simulated leather artificial synthetic leather.
[0030] Compared with existing technologies:
[0031] By adding tear-resistant additives, preservatives, flame retardants and waterproof agents to the raw materials, the tensile strength, anti-corrosion, flame retardant and waterproof properties of artificial synthetic leather can be improved, thereby solving the problem of relatively single performance of existing artificial synthetic leather, thereby increasing the service life of artificial synthetic leather. DETAILED DESCRIPTION
[0032] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below.
[0033] Embodiment 1:
[0034] The invention provides a super-simulated leather artificial synthetic leather, comprising a superfine fiber non-woven fabric, a soaking material raw material, a fabric raw material and a preparation raw material, wherein the soaking material raw material comprises, by weight: 10 parts of polyurethane, 10 parts of dimethylformamide, 6 parts of toluene color resistant paste, 4 parts of soaking aid, 2 parts of tearing aid, 6 parts of hydrolysis resistance aid, 6 parts of preservative, and 4 parts of flame retardant;
[0035] The fabric raw materials include: 10 parts of wood fiber powder, 6 parts of pigment, 4 parts of additives, 6 parts of calcium carbonate, 2 parts of non-ionic surfactant, and 6 parts of waterproofing agent;
[0036] The raw materials for preparation include, by weight: 8 parts of dimethylformamide, 4 parts of toluene solution, and 2 parts of oil agent.
[0037] The impregnation aid is composed of alkaline protease, non-ionic surfactant and pH buffer.
[0038] The anti-tearing additive is composed of graphene, chlorinated wax, anti-tearing finishing liquid, dispersant, glyceryl monostearate, leveling agent, penetrant, thickener and deionized water.
[0039] The hydrolysis-resistant additive is composed of hydrolysis-resistant polyhexamethylene adipamide resin, polyketone resin and hydrolysis-resistant glass fiber.
[0040] The raw materials of the preservative include, by weight: 12 parts of sorbic acid, 6 parts of sucrose fatty acid ester, 4 parts of acetic acid, 2 parts of paraffin, 4 parts of sodium molybdate, 2 parts of diatomaceous earth, and 4 parts of epoxy resin;
[0041] The preparation process of the preservative is as follows:
[0042] Process 1: placing sorbic acid, sucrose fatty acid ester, acetic acid and paraffin in a reaction kettle and mixing them;
[0043] Process 2: Sodium molybdate, diatomaceous earth and epoxy resin are placed in a reaction kettle and mixed;
[0044] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0045] The flame retardant is composed of alkylphenol polyoxyethylene ether, pentaerythritol, tetrabromobisphenol, an active agent and an emulsifier.
[0046] The waterproofing agent is composed of linoleic acid, vaseline, sodium hydroxide, aluminum oxide, ethanol, hydrogen silicone oil emulsion and soap powder.
[0047] The preparation process of waterproofing agent is as follows:
[0048] Process 1: linoleic acid, vaseline, sodium hydroxide and aluminum oxide are placed in a reaction kettle and mixed;
[0049] Process 2: placing ethanol, hydrogen silicone oil emulsion and soap powder in a reaction kettle for mixing;
[0050] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a waterproofing agent.
[0051] A method for processing super-simulated artificial synthetic leather comprises the following specific steps:
[0052] Step 1, preparing the impregnation material: mixing polyurethane, dimethylformamide, toluene-resistant paste, impregnation aid, tear-resistant aid, hydrolysis-resistant aid, preservative and flame retardant, specifically, stirring at a stirring speed of 1200 r / min at room temperature, and controlling the solution viscosity at 100 cps;
[0053] Step 2, fabric preparation: wood fiber powder, pigment, additive, calcium carbonate, non-ionic surfactant, and waterproofing agent are mixed. Specifically, stirring is performed at a stirring speed of 1400r / min at room temperature. After stirring evenly, the stirring speed is reduced to 500r / min for vacuum degassing for 60 minutes, and the solution viscosity is controlled at 15000cps;
[0054] Step 3: Using ultrafine fiber non-woven fabric as the base fabric, using a wet high-density one-step method, the impregnation and coating are carried out simultaneously, and then entering a coagulation tank containing dimethylformamide for coagulation, and after coagulation, entering a water washing tank for water washing;
[0055] Step 4, sending the semi-finished product after step 3 into a reduction tank, which is filled with a toluene solution. Under the action of the toluene solution, the sea component is dissolved. After multiple tanks of dissolution, the PET in the ultrafine fiber non-woven fabric is extracted and dissolved, and then washed with boiling water to achieve the opening of the ultrafine fiber, and obtain the opened semi-finished product;
[0056] Step 5: Apply oil to the semi-finished fiber-opening product to increase the softness of the bass, and then stretch, grind and polish the leather to obtain super-simulated leather artificial synthetic leather.
[0057] Embodiment 2:
[0058] The invention provides a super-simulated leather artificial synthetic leather, comprising a superfine fiber non-woven fabric, a soaking material raw material, a fabric raw material and a preparation raw material, wherein the soaking material raw material comprises, by weight, 15 parts of polyurethane, 12.5 parts of dimethylformamide, 7 parts of toluene color resistant paste, 6 parts of soaking aid, 6 parts of tearing aid, 8 parts of hydrolysis resistance aid, 8 parts of preservative and 6 parts of flame retardant;
[0059] The fabric raw materials include: 12.5 parts of wood fiber powder, 8 parts of pigment, 6 parts of additives, 8 parts of calcium carbonate, 4 parts of non-ionic surfactant, and 7 parts of waterproofing agent.
[0060] The raw materials for preparation include, by weight: 10 parts of dimethylformamide, 6 parts of toluene solution, and 4 parts of oil agent.
[0061] The impregnation aid is composed of alkaline protease, non-ionic surfactant and pH buffer.
[0062] The anti-tearing additive is composed of graphene, chlorinated wax, anti-tearing finishing liquid, dispersant, glyceryl monostearate, leveling agent, penetrant, thickener and deionized water.
[0063] The hydrolysis-resistant additive is composed of hydrolysis-resistant polyhexamethylene adipamide resin, polyketone resin and hydrolysis-resistant glass fiber.
[0064] The raw materials of the preservative include, by weight: 13 parts of sorbic acid, 8 parts of sucrose fatty acid ester, 6 parts of acetic acid, 4 parts of paraffin, 7 parts of sodium molybdate, 4 parts of diatomaceous earth, and 6 parts of epoxy resin;
[0065] The preparation process of the preservative is as follows:
[0066] Process 1: placing sorbic acid, sucrose fatty acid ester, acetic acid and paraffin in a reaction kettle and mixing them;
[0067] Process 2: Sodium molybdate, diatomaceous earth and epoxy resin are placed in a reaction kettle and mixed;
[0068] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0069] The flame retardant is composed of alkylphenol polyoxyethylene ether, pentaerythritol, tetrabromobisphenol, an active agent and an emulsifier.
[0070] The waterproofing agent is composed of linoleic acid, vaseline, sodium hydroxide, aluminum oxide, ethanol, hydrogen silicone oil emulsion and soap powder.
[0071] The preparation process of waterproofing agent is as follows:
[0072] Process 1: linoleic acid, vaseline, sodium hydroxide and aluminum oxide are placed in a reaction kettle and mixed;
[0073] Process 2: placing ethanol, hydrogen silicone oil emulsion and soap powder in a reaction kettle for mixing;
[0074] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a waterproofing agent.
[0075] A method for processing super-simulated artificial synthetic leather comprises the following specific steps:
[0076] Step 1, preparing the impregnation material: mixing polyurethane, dimethylformamide, toluene-resistant paste, impregnation aid, tear-resistant aid, hydrolysis-resistant aid, preservative and flame retardant, specifically, stirring at a stirring speed of 1200 r / min at room temperature, and controlling the solution viscosity at 100 cps;
[0077] Step 2, fabric preparation: wood fiber powder, pigment, additive, calcium carbonate, non-ionic surfactant, and waterproofing agent are mixed. Specifically, stirring is performed at a stirring speed of 1400r / min at room temperature. After stirring evenly, the stirring speed is reduced to 500r / min for vacuum degassing for 60 minutes, and the solution viscosity is controlled at 15000cps;
[0078] Step 3: Using ultrafine fiber non-woven fabric as the base fabric, using a wet high-density one-step method, the impregnation and coating are carried out simultaneously, and then entering a coagulation tank containing dimethylformamide for coagulation, and after coagulation, entering a water washing tank for water washing;
[0079] Step 4, sending the semi-finished product after step 3 into a reduction tank, which is filled with a toluene solution. Under the action of the toluene solution, the sea component is dissolved. After multiple tanks of dissolution, the PET in the ultrafine fiber non-woven fabric is extracted and dissolved, and then washed with boiling water to achieve the opening of the ultrafine fiber, and obtain the opened semi-finished product;
[0080] Step 5: Apply oil to the semi-finished fiber-opening product to increase the softness of the bass, and then stretch, grind and polish the leather to obtain super-simulated leather artificial synthetic leather.
[0081] Embodiment 3:
[0082] The invention provides a super-simulated leather artificial synthetic leather, comprising a superfine fiber non-woven fabric, a soaking material raw material, a fabric raw material and a preparation raw material, wherein the soaking material raw material comprises, by weight: 20 parts of polyurethane, 15 parts of dimethylformamide, 8 parts of toluene color resistant paste, 8 parts of soaking aid, 10 parts of tearing aid, 10 parts of hydrolysis resistant aid, 10 parts of preservative, and 8 parts of flame retardant;
[0083] The fabric raw materials include: 15 parts of wood fiber powder, 10 parts of pigment, 8 parts of additives, 10 parts of calcium carbonate, 6 parts of non-ionic surfactant, and 8 parts of waterproofing agent;
[0084] The raw materials for preparation include, by weight: 12 parts of dimethylformamide, 8 parts of toluene solution, and 6 parts of oil agent.
[0085] The impregnation aid is composed of alkaline protease, non-ionic surfactant and pH buffer.
[0086] The anti-tearing additive is composed of graphene, chlorinated wax, anti-tearing finishing liquid, dispersant, glyceryl monostearate, leveling agent, penetrant, thickener and deionized water.
[0087] The hydrolysis-resistant additive is composed of hydrolysis-resistant polyhexamethylene adipamide resin, polyketone resin and hydrolysis-resistant glass fiber.
[0088] The raw materials of the preservative include, by weight: 14 parts of sorbic acid, 10 parts of sucrose fatty acid ester, 8 parts of acetic acid, 6 parts of paraffin, 10 parts of sodium molybdate, 6 parts of diatomaceous earth, and 8 parts of epoxy resin;
[0089] The preparation process of the preservative is as follows:
[0090] Process 1: placing sorbic acid, sucrose fatty acid ester, acetic acid and paraffin in a reaction kettle and mixing them;
[0091] Process 2: Sodium molybdate, diatomaceous earth and epoxy resin are placed in a reaction kettle and mixed;
[0092] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0093] The flame retardant is composed of alkylphenol polyoxyethylene ether, pentaerythritol, tetrabromobisphenol, an active agent and an emulsifier.
[0094] The waterproofing agent is composed of linoleic acid, vaseline, sodium hydroxide, aluminum oxide, ethanol, hydrogen silicone oil emulsion and soap powder.
[0095] The preparation process of waterproofing agent is as follows:
[0096] Process 1: linoleic acid, vaseline, sodium hydroxide and aluminum oxide are placed in a reaction kettle and mixed;
[0097] Process 2: placing ethanol, hydrogen silicone oil emulsion and soap powder in a reaction kettle for mixing;
[0098] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a waterproofing agent.
[0099] A method for processing super-simulated artificial synthetic leather comprises the following specific steps:
[0100] Step 1, preparing the impregnation material: mixing polyurethane, dimethylformamide, toluene-resistant paste, impregnation aid, tear-resistant aid, hydrolysis-resistant aid, preservative and flame retardant, specifically, stirring at a stirring speed of 1200 r / min at room temperature, and controlling the solution viscosity at 100 cps;
[0101] Step 2, fabric preparation: wood fiber powder, pigment, additive, calcium carbonate, non-ionic surfactant, and waterproofing agent are mixed. Specifically, stirring is performed at a stirring speed of 1400r / min at room temperature. After stirring evenly, the stirring speed is reduced to 500r / min for vacuum degassing for 60 minutes, and the solution viscosity is controlled at 15000cps;
[0102] Step 3: Using ultrafine fiber non-woven fabric as the base fabric, using a wet high-density one-step method, the impregnation and coating are carried out simultaneously, and then entering a coagulation tank containing dimethylformamide for coagulation, and after coagulation, entering a water washing tank for water washing;
[0103] Step 4, sending the semi-finished product after step 3 into a reduction tank, which is filled with a toluene solution. Under the action of the toluene solution, the sea component is dissolved. After multiple tanks of dissolution, the PET in the ultrafine fiber non-woven fabric is extracted and dissolved, and then washed with boiling water to achieve the opening of the ultrafine fiber, and obtain the opened semi-finished product;
[0104] Step 5: Apply oil to the semi-finished fiber-opening product to increase the softness of the bass, and then stretch, grind and polish the leather to obtain super-simulated leather artificial synthetic leather.
[0105] The super-simulated leather artificial synthetic leather prepared in the above Examples 1-3 was compared to obtain the following data:
[0106] Example 1 Example 2 Example 3 tensile strength 12.65 / MPa 17.32 / MPa 14.01 / MPa Corrosion resistance Sa2 Sa2.5 Sa2 Waterproof grade IPX8 IPX8 IPX8 Flame retardant grade V-1 V-1 V-1
[0107] It can be seen from the above table that the super-simulated leather artificial synthetic leathers prepared in Examples 1-3 have good performance in tensile strength, anti-corrosion level, waterproof level and flame retardant level. After use, Example 2 has the best effect.
[0108] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A super-simulated leather artificial synthetic leather, comprising ultra-fine fiber non-woven fabric, impregnation raw materials, fabric raw materials and preparation raw materials, characterized in that: The impregnation raw materials include, by weight: 10-20 parts of polyurethane, 10-15 parts of dimethylformamide, 6-8 parts of toluene-resistant paste, 4-8 parts of impregnation aid, 2-10 parts of tear-resistant aid, 6-10 parts of hydrolysis-resistant aid, 6-10 parts of preservative, and 4-8 parts of flame retardant; The fabric raw materials include, by weight: 10-15 parts of wood fiber powder, 6-10 parts of pigment, 4-8 parts of additives, 6-10 parts of calcium carbonate, 2-6 parts of nonionic surfactant, and 6-8 parts of waterproofing agent; The raw materials for preparation include, by weight: 8-12 parts of dimethylformamide, 4-8 parts of toluene solution, and 2-6 parts of oil agent.
2. The super-simulated leather artificial synthetic leather according to claim 1, characterized in that: The impregnation auxiliary agent is composed of alkaline protease, non-ionic surfactant and pH buffer.
3. The super-simulated leather artificial synthetic leather according to claim 1, characterized in that: The anti-tearing auxiliary agent is composed of graphene, chlorinated wax, anti-tearing finishing liquid, dispersant, glyceryl monostearate, leveling agent, penetrant, thickener and deionized water.
4. The super-simulated leather artificial synthetic leather according to claim 1, characterized in that: The hydrolysis-resistant auxiliary agent is composed of hydrolysis-resistant polyhexamethylene adipamide resin, polyketone resin and hydrolysis-resistant glass fiber.
5. The super-simulated leather artificial synthetic leather according to claim 1, characterized in that: The raw materials of the preservative include, by weight: 12-14 parts of sorbic acid, 6-10 parts of sucrose fatty acid ester, 4-8 parts of acetic acid, 2-6 parts of paraffin, 4-10 parts of sodium molybdate, 2-6 parts of diatomaceous earth, and 4-8 parts of epoxy resin.
6. The super-simulated leather artificial synthetic leather according to claim 5, characterized in that: The preparation process of the preservative is as follows: Process 1: placing sorbic acid, sucrose fatty acid ester, acetic acid and paraffin in a reaction kettle and mixing them; Process 2: Sodium molybdate, diatomaceous earth and epoxy resin are placed in a reaction kettle and mixed; Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
7. The super-simulated leather artificial synthetic leather according to claim 1, characterized in that: The flame retardant is composed of alkylphenol polyoxyethylene ether, pentaerythritol, tetrabromobisphenol, an active agent and an emulsifier.
8. The super-simulated leather artificial synthetic leather according to claim 1, characterized in that: The waterproofing agent is composed of linoleic acid, vaseline, sodium hydroxide, aluminum oxide, ethanol, hydrogen silicone oil emulsion and soap powder.
9. The super-simulated leather artificial synthetic leather according to claim 8, characterized in that: The preparation process of the waterproofing agent is as follows: Process 1: linoleic acid, vaseline, sodium hydroxide and aluminum oxide are placed in a reaction kettle and mixed; Process 2: placing ethanol, hydrogen silicone oil emulsion and soap powder in a reaction kettle for mixing; Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a waterproofing agent.
10. A method for processing super-simulated artificial leather, characterized in that: The specific steps are as follows: Step 1, preparing the impregnation material: mixing polyurethane, dimethylformamide, toluene-resistant paste, impregnation aid, tear-resistant aid, hydrolysis-resistant aid, preservative and flame retardant, specifically, stirring at a stirring speed of 1200 r / min at room temperature, and controlling the solution viscosity at 100 cps; Step 2, fabric preparation: wood fiber powder, pigment, additive, calcium carbonate, non-ionic surfactant, and waterproofing agent are mixed. Specifically, stirring is performed at a stirring speed of 1400r / min at room temperature. After stirring evenly, the stirring speed is reduced to 500r / min for vacuum degassing for 60 minutes, and the solution viscosity is controlled at 15000cps; Step 3: Using ultrafine fiber non-woven fabric as the base fabric, using a wet high-density one-step method, the impregnation and coating are carried out simultaneously, and then entering a coagulation tank containing dimethylformamide for coagulation, and after coagulation, entering a water washing tank for water washing; Step 4, sending the semi-finished product after step 3 into a reduction tank, which is filled with a toluene solution. Under the action of the toluene solution, the sea component is dissolved. After multiple tanks of dissolution, the PET in the ultrafine fiber non-woven fabric is extracted and dissolved, and then washed with boiling water to achieve the opening of the ultrafine fiber, and obtain the opened semi-finished product; Step 5: Apply oil to the semi-finished fiber-opening product to increase the softness of the bass, and then stretch, grind and polish the leather to obtain super-simulated leather artificial synthetic leather.
Citation Information
Cited By
Outdoor jacket made of water-repellent and oil-repellent fabric and preparation method of outdoor jacket
CN119041220A
A jacket made of water-repellent and oil-repellent fabric and a preparation method thereof
CN119041220B