Method for dyeing polyester fabric by using modified curcumin
By surface-modifying curcumin and combining it with polyester fabrics, the problem of insufficient application of curcumin in polyester fabric dyeing is solved, and the effect of improving fabric properties is achieved, including rubbing fastness, UV resistance and antibacterial properties. promote.
Patent Information
- Application Number
- CN202411193391.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-10-08
AI Technical Summary
In the existing technology, curcumin is rarely used in polyester fabric dyeing, and traditional methods require the use of organic solvents, which are costly and have poor environmental protection, resulting in poor dyeing effects and performance.
By surface modification of curcumin with chitosan and tannic acid, a nano-modified curcumin dispersion is generated, and combined with polyester fabric through soaking and baking processes to improve the dispersion and binding properties of the dye.
Significantly improves the rubbing fastness, UV resistance and antibacterial properties of polyester fabrics, and enhances the dyeing effect and color fastness.
Smart Images

Figure CN118745673A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile dyeing, and in particular to a method for dyeing polyester fabric by utilizing modified curcumin. Background Art
[0002] Curcuminoid is a general term for a yellow, slightly acidic diphenylheptane substance, mainly curcumin. It is a very rare diketone colored substance in nature, mainly including curcumin, demethoxycurcumin, bisdemethoxycurcumin, tetrahydrocurcumin, demethoxytetrahydrocurcumin, and bisdemethoxytetrahydrocurcumin. Curcumin has the characteristics of strong coloring power, bright color, strong thermal stability, safety and non-toxicity, and can be widely used as a colorant in industrial fields such as medicine, textile dyeing, and feed.
[0003] In 2023, Zhao Hudie and others published an article in the "Printing and Dyeing Auxiliary Agents" entitled "Research Progress on the Application and Performance Improvement of Natural Curcumin". The article mentioned that "as a natural compound, curcumin has a special aroma, a slightly bitter taste, a melting point of 179~182°C, is highly lipophilic, and has very poor water solubility. Because there are multiple double bonds, phenolic hydroxyl groups and carbonyl groups in the curcumin molecule, a relatively strong chemical reaction will occur. Therefore, curcumin is easily affected by physical and chemical factors such as light and heat during application." The article also summarizes the use of curcumin to dye wool, silk, cotton, viscose, hemp fiber, jute fabrics, and silk products. However, in the field of textile printing and dyeing, there is little research on the application of curcumin in polyester fabrics.
[0004] The patent announcement number is CN103952008B, and the patent titled "Water-soluble curcumin dye based on chemical structure modification, preparation method and application" discloses a water-soluble curcumin dye based on chemical structure modification. Curcumin is first reacted with 1,2-dibromoethane and then with triethylamine to obtain a water-soluble curcumin dye, which is then used to dye cotton fabrics to solve the problems of low dye uptake and color fastness, but does not involve the dyeing of polyester fabrics.
[0005] Patent publication number CN106758352A, entitled "Dyeing method of polyester fabric with curcumin", discloses that curcumin is dissolved in a carbon tetrachloride / phenol mixed solution, and then a surfactant, sodium dodecylbenzene sulfonate, is added to obtain a transparent solution under ultrasound; the polyester fabric is put into the dye solution, and oscillated and heated to 30-60°C for dyeing. However, this method requires the use of organic solvents, which is costly and environmentally unfriendly.
[0006] Therefore, it is necessary to provide a method for dyeing polyester fabrics using modified curcumin to solve the problems existing in the above-mentioned prior art. Summary of the invention
[0007] In view of this, the present invention provides a method for dyeing polyester fabric using modified curcumin, so as to achieve the purpose of dyeing polyester fabric with modified curcumin and improving the friction fastness, anti-ultraviolet and antibacterial properties of the fabric.
[0008] To achieve the above object, the present invention provides a method for dyeing polyester fabric using modified curcumin, comprising the following steps: S1. surface modification of curcumin using chitosan and tannic acid to obtain modified curcumin; S2. The modified curcumin is mixed evenly with the remaining additives and ground to obtain a nano-modified curcumin dispersion; S3. The polyester fabric is immersed in the nano-modified curcumin dispersion, and then pre-baked and baked to obtain a dyed polyester fabric.
[0009] The invention modifies curcumin, and a high-adhesion substance generated by the reaction of tannic acid and chitosan is adsorbed on the surface of curcumin particles, thereby enhancing the binding performance of curcumin and polyester fabric. On the other hand, curcumin has a weak negative charge and can be ionically bonded with the amino group of chitosan. In addition, curcumin molecules are rich in aromatic structures and can be bonded with tannic acid through supramolecular forces. Therefore, tannic acid and chitosan products as modifiers have strong interaction with curcumin particles. The modified curcumin has high compatibility with polyacrylic acid adhesive and high dispersibility in the polyacrylic acid adhesive, thereby improving the dispersibility and fastness on polyester fabric.
[0010] The invention grinds the modified curcumin and other additives to obtain a nano modified curcumin dispersion, further improves the dispersibility of the modified curcumin, improves the uniformity and dyeing rate of subsequent polyester fabric dyeing, and through the combination of raw materials and processes, the obtained dyed polyester fabric has good color fastness and antibacterial and anti-ultraviolet properties.
[0011] Optionally, the surface modification in S1 includes dissolving chitosan and curcumin in water to obtain a mixed solution, heating and stirring; gradually adding tannic acid solution, standing after the addition is complete, filtering and obtaining a precipitate, and washing to obtain modified curcumin.
[0012] Optionally, the concentration of chitosan in the mixed solution is 0.8-1.2 g / L, the concentration of curcumin is 3-5 g / L, the pH value of the mixed solution is 4-5; the concentration of tannic acid in the tannic acid solution is 2-3 g / L.
[0013] Optionally, the heating and stirring conditions are 65-75° C. and the stirring rate is 500-600 r / min.
[0014] Optionally, the tannic acid solution is added at a rate of 3 to 5 mL / min and allowed to stand for 60 to 90 minutes after the addition is completed.
[0015] Optionally, the additives in S2 include abrasives, adhesives and solvents.
[0016] Optionally, the abrasive is AL50, the adhesive is HF-901, and the solvent is water.
[0017] Optionally, the mixing in S2 is stirring mixing, and the conditions are stirring at 500-600 r / min for 10-15 min.
[0018] Optionally, the concentration of the modified curcumin in S2 is 3-5 wt %, the concentration of the binder is 10-15 wt %, and the average particle size of the nano-modified curcumin dispersion is 300-350 nm.
[0019] Optionally, S3 includes the polyester fabric being subjected to two dipping and two rolling, with the liquid volume being 90-110%; the pre-baking temperature being 90-100° C., and the time being 2-3 min; and the baking temperature being 165-175° C., and the time being 2-3 min.
[0020] The above technical solution of the present invention includes at least the following beneficial effects: The invention modifies curcumin and further grinds the modified curcumin, respectively processes the raw materials from the fields of chemistry and physics, and combines the padding-baking process to prepare the dyed polyester fabric. On the one hand, the combination of the dye and the polyester fabric is increased by the modification of the curcumin, and on the other hand, the dyed polyester fabric obtained after the introduction of the curcumin has multiple functions such as good color fastness and antibacterial and anti-ultraviolet properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is the electron microscope scanning image of the polyester fabric and the dyed polyester fabric in Example 3 of the present invention. DETAILED DESCRIPTION
[0022] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the following will be combined with the appended drawings of the embodiments of the present invention. Figure 1 , the technical scheme of the embodiment of the present invention is clearly and completely described. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0023] Example 1 Chitosan and curcumin were added to water to prepare solution A, the concentration of chitosan was 0.8 g / L, the pH of the solution was adjusted to 4 with citric acid, the concentration of curcumin was 5 g / L, the solution was heated and stirred to 65 ° C, and the stirring rate was 600 r / min; then solution B containing 3 g / L tannic acid was gradually added to solution A, the rate of dropwise addition was 5 mL / min, and the reaction was continued for 90 min after the dropwise addition was completed, and then the precipitate was filtered and washed with distilled water and ethanol to obtain modified curcumin. 3 wt% modified curcumin, abrasive AL50, and 15 wt% binder HF-901 were added to distilled water, stirred at 500 r / min for 10 min, and then added to a zirconium oxide grinder for grinding and filtration to obtain a nano-modified curcumin dispersion. The polyester fabric was immersed in a nano-modified curcumin dispersion having an average particle size of 300 nm, and then double-dipped and double-rolled with a liquid volume of 90%, and then pre-baked at 90°C for 3 minutes, and then baked at 175°C for 2 minutes to obtain a dyed polyester fabric.
[0024] Example 2 Chitosan and curcumin were added to water to prepare solution A, the concentration of chitosan was 1.2 g / L, the pH of the solution was adjusted to 4.5 with citric acid, the concentration of curcumin was 4 g / L, the solution was heated and stirred to 75 °C, and the stirring rate was 500 r / min; then solution B containing 2.5 g / L tannic acid was gradually added to solution A, the rate of dropwise addition was 3 mL / min, and the reaction was continued for 60 min after the dropwise addition was completed, and then the precipitate was filtered and washed with distilled water and ethanol to obtain modified curcumin. 5 wt% modified curcumin, abrasive AL50, and 10 wt% binder HF-901 were added to distilled water, stirred at 600 r / min for 10 min, and then added to a zirconium oxide grinder for grinding and filtration to obtain a nano-modified curcumin dispersion, and the average particle size of the nano-modified curcumin dispersion was 310 nm. The polyester fabric was immersed in the nano-modified curcumin dispersion, then double-dipped and double-rolled with a liquid volume of 110%, then pre-baked at 100°C for 3 minutes, and then baked at 165°C for 3 minutes to obtain the dyed polyester fabric.
[0025] Example 3 Chitosan and curcumin were added to water to prepare solution A, the concentration of chitosan was 1g / L, the pH of the solution was adjusted to 5 with citric acid, the concentration of curcumin was 3g / L, the solution was heated and stirred to 70°C, and the stirring rate was 550r / min; then solution B containing 2g / L tannic acid was gradually added to solution A at a rate of 4mL / min, and the reaction was continued for 70min after the addition was completed, and then the precipitate was filtered and washed with distilled water and ethanol to obtain modified curcumin. 5wt% modified curcumin, abrasive AL50, and 15wt% binder HF-901 were added to distilled water, stirred at 550r / min for 15min, and then added to a zirconium oxide grinder for grinding and filtering to obtain a nano-modified curcumin dispersion, and the average particle size of the nano-modified curcumin dispersion was 350nm. The polyester fabric was immersed in the nano-modified curcumin dispersion, then double-dipped and double-rolled with the liquid volume being 100%, and then pre-baked at 95°C for 2 minutes, and then baked at 170°C for 3 minutes to obtain the dyed polyester fabric.
[0026] Example 4 Chitosan and curcumin were added to water to prepare solution A, the concentration of chitosan was 1.1 g / L, the pH of the solution was adjusted to 4.8 with citric acid, the concentration of curcumin was 3.5 g / L, the solution was heated and stirred to 72°C, and the stirring rate was 520 r / min; then solution B containing 2.2 g / L tannic acid was gradually added to solution A, the rate of dropwise addition was 5 mL / min, and the reaction was continued for 80 min after the dropwise addition was completed, and then the precipitate was filtered and washed with distilled water and ethanol to obtain modified curcumin. 3.5 wt% modified curcumin, abrasive AL50, and 14 wt% binder HF-901 were added to distilled water, stirred at 570 r / min for 13 min, and then added to a zirconium oxide grinder for grinding and filtration to obtain a nano-modified curcumin dispersion, and the average particle size of the nano-modified curcumin dispersion was 300 nm. The polyester fabric was immersed in the nano-modified curcumin dispersion, then double-dipped and double-rolled with a liquid volume of 105%, then pre-baked at 94°C for 2.5 minutes, and then baked at 172°C for 2 minutes to obtain the dyed polyester fabric.
[0027] Example 5 Compared with Example 3, the only difference is that the concentration of chitosan is 0.9 g / L, the concentration of curcumin is 4.5 g / L, and the concentration of tannic acid is 2.8 g / L.
[0028] Comparative Example 1 Compared with Example 3, the only difference is that curcumin is used instead of modified curcumin, and the other raw materials and steps are consistent with Example 3.
[0029] Comparative Example 2 Compared with Example 3, the only difference is that grinding is not performed, and the other raw materials and steps are the same as those in Example 3.
[0030] Comparative Example 3 Compared with Example 3, the only difference is whether tannic acid is used, and the other raw materials and steps are the same as those in Example 3.
[0031] Comparative Example 4 Compared with Example 3, the only difference is whether chitosan is used or not, and the other raw materials and steps are the same as those in Example 3.
[0032] The performance of the dyed polyester fabrics prepared in Examples 1 to 5 and Comparative Examples 1 to 4 was tested.
[0033] The rubbing fastness of the dyed polyester fabric was tested according to GB / T 3920-2008 "Textiles - Tests for Colour Fastness - Colour Fastness to Rubbing"; the UV resistance of the dyed polyester fabric was tested according to GB / T 18830-2009 "Determination of UV Protection of Textiles"; the UV resistance of the dyed polyester fabric was tested according to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles - Part 3: Oscillation Method". The results are shown in Table 1. The polyester fabric and the dyed polyester fabric in Example 3 were subjected to electron microscope scanning, and the results were Figure 1 .
[0034] Table 1 Performance test results of dyed polyester fabrics of Examples 1 to 5 and Comparative Examples 1 to 4
[0035] As shown in Table 1, the color fastness to rubbing, antibacterial effect and UV protection of the dyed polyester fabrics prepared in Examples 1 to 5 of the present invention are better than those of the undyed polyester fabric and the dyed polyester fabrics prepared in Comparative Examples 1 to 4.
[0036] Combining the performance comparison of Example 3 with Comparative Examples 1 to 4, it can be seen that the dyed polyester fabric prepared by the present invention is superior to the comparative examples in terms of rubbing color fastness, antibacterial and anti-ultraviolet performance. That is, the modified curcumin used in the present invention is combined with the process of dyeing polyester fabric to improve the color fastness of polyester fabric, and at the same time, it also increases the antibacterial and anti-ultraviolet performance of the dyed polyester fabric.
[0037] Depend on Figure 1 It can be seen that the surface of the undyed polyester fabric is smooth and neat, while a layer of film and particles can be found on the surface of the dyed fabric, indicating that the modified curcumin was successfully combined with the polyester fabric.
[0038] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for dyeing polyester fabric using modified curcumin, It is characterized in that The following steps are involved: S1. surface modification of curcumin using chitosan and tannic acid to obtain modified curcumin; S2. The modified curcumin is mixed evenly with the remaining additives and ground to obtain a nano-modified curcumin dispersion; S3. The polyester fabric is immersed in the nano-modified curcumin dispersion, and then pre-baked and baked to obtain a dyed polyester fabric.
2. The method for dyeing polyester fabric using modified curcumin according to claim 1, It is characterized in that The surface modification in S1 includes dissolving chitosan and curcumin in water to obtain a mixed solution, heating and stirring; gradually adding tannic acid solution, standing after the addition, filtering and obtaining a precipitate, and washing to obtain modified curcumin.
3. The method for dyeing polyester fabric using modified curcumin according to claim 2, It is characterized in that The concentration of chitosan in the mixed solution is 0.8-1.2 g / L, the concentration of curcumin is 3-5 g / L, the pH value of the mixed solution is 4-5; the concentration of tannic acid in the tannic acid solution is 2-3 g / L.
4. The method for dyeing polyester fabric using modified curcumin according to claim 2, It is characterized in that The heating and stirring conditions are 65-75° C. and the stirring rate is 500-600 r / min.
5. The method for dyeing polyester fabric using modified curcumin according to claim 2, It is characterized in that The dropping rate of the tannic acid solution is 3~5mL / min, and it is allowed to stand for 60~90min after the addition is completed.
6. The method for dyeing polyester fabric using modified curcumin according to claim 1, It is characterized in that The additives in S2 include abrasives, adhesives and solvents.
7. The method for dyeing polyester fabric using modified curcumin according to claim 6, It is characterized in that The abrasive is AL50, the adhesive is HF-901, and the solvent is water.
8. The method for dyeing polyester fabric using modified curcumin according to claim 1, It is characterized in that The mixing in S2 is performed by stirring at 500-600 r / min for 10-15 min.
9. The method for dyeing polyester fabric using modified curcumin according to claim 1, It is characterized in that The concentration of the modified curcumin in S2 is 3-5 wt %, the concentration of the binder is 10-15 wt %, and the average particle size of the nano-modified curcumin dispersion is 300-350 nm.
10. The method for dyeing polyester fabric using modified curcumin according to claim 1, It is characterized in that The S3 includes the polyester fabric being subjected to two dipping and two rolling, with the liquid volume being 90-110%; the pre-baking temperature being 90-100° C., the time being 2-3 minutes; the baking temperature being 165-175° C., the time being 2-3 minutes.