Ultrathin composite film hydrogen sensor based on semiconductor metal oxide and preparation method thereof
Using ALD technology to prepare ultra-thin composite oxide film hydrogen sensors without precious metal catalysts solves the problems of high operating temperature and poor selectivity of the sensor, achieves high sensitivity and fast response, reduces costs and is compatible with MEMS processes.
Patent Information
- Application Number
- CN202411232985.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-10-08
AI Technical Summary
Existing semiconductor metal oxide hydrogen sensors have problems such as high operating temperature, slow response recovery, and poor hydrogen selectivity. They often require the introduction of precious metal catalysts to increase cost and complexity.
Atomic layer deposition (ALD) technology is used to prepare ultra-thin composite oxide film hydrogen sensors without precious metal catalyst modification. By sequentially depositing SnO2 and In2O3 films on an insulating substrate, a conductive electrode is formed to achieve high sensitivity and low detection. Lower limit, ultra-fast response and excellent selectivity.
It achieves high-sensitivity response and rapid recovery to hydrogen in a wide operating temperature range, reduces the operating temperature, avoids the use of precious metal catalysts, reduces costs, and is compatible with micro-electromechanical system processes.
Smart Images

Figure CN118746604A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of hydrogen sensors and relates to an ultra-thin composite film hydrogen sensor based on semiconductor metal oxide and a preparation method thereof. Background Art
[0002] With the transformation of the global energy structure and the improvement of environmental protection awareness, hydrogen energy, as a clean and efficient renewable energy, is being widely used in various fields. Hydrogen has the advantages of high energy density and pollution-free combustion products, and is considered to be one of the most promising green energy sources in the 21st century. However, the flammable and explosive properties of hydrogen also bring serious safety hazards. Its explosion limit in the air ranges from 4% to 75% (volume fraction). Therefore, in order to ensure the safe production, storage, transportation and use of hydrogen energy, it is particularly important to develop hydrogen sensors with excellent performance. Hydrogen sensors with high sensitivity, fast response and good selectivity can not only detect leaks in time, but also provide reliable safety guarantees for the promotion and application of hydrogen energy technology.
[0003] Semiconductor metal oxide resistive hydrogen sensors have become a hot topic of current research due to their simple structure, low cost, and good stability. Among them, SnO2, as a typical n-type semiconductor material, has shown excellent sensitivity in the field of hydrogen sensors and has been used in commercial resistive hydrogen sensors. However, single SnO2 hydrogen sensors often have problems such as high operating temperature and poor selectivity. They need to work at a high temperature of about 300°C, which not only increases energy consumption, but also limits their application in certain special environments. In order to lower the operating temperature and improve selectivity, it is usually necessary to introduce expensive precious metal catalysts, such as Pd particles, to modify the semiconductor metal oxide sensor. However, this undoubtedly increases the complexity of the device and the cost of the sensor.
[0004] SnO2 / In2O3, as a semiconductor metal oxide composite gas-sensitive material, has been widely studied for reducing gas detection, most of which are used for the detection of carbon monoxide, ethanol, etc., and only a few studies are used for hydrogen detection. Moreover, most of the composite systems are SnO2 / In2O3 core-shell structures, nanotubes, nanoribbons, nanofibers and other powder samples synthesized by hydrothermal method, electrospinning method and other methods. There are fewer SnO2 / In2O3 composite film samples used for gas-sensitive detection, which are all prepared by physical vapor deposition such as magnetron sputtering and wet chemical methods such as sol-gel method. Moreover, most gas-sensitive samples often need to introduce precious metal catalysts such as Pt and Pd to obtain good gas-sensitive performance. In particular, the SnO2 / In2O3 composite hydrogen sensors that have been reported cannot be separated from the modification of Pt or Pd nanoparticles.
[0005] In recent years, Atomic Layer Deposition (ALD), as a new chemical vapor deposition material preparation technology, has attracted much attention in the field of thin film preparation due to its unique self-limiting and self-saturated growth mechanism and precise film thickness control capability. ALD technology achieves low-temperature film growth at the atomic level (angstrom level) by alternately introducing different precursors into the reaction chamber, and self-limiting surface chemical reactions occur on the substrate surface. It has large-area uniformity and excellent three-dimensional conformality. This growth mode enables ALD technology to accurately control the thickness and composition of the film at the atomic scale and tune the interface structure. ALD technology has been applied in the field of integrated circuit manufacturing and is highly compatible with microelectromechanical systems (MEMS) processes. ALD has shown broad application prospects in microelectronics, optoelectronics, nanotechnology, photovoltaics, energy storage, catalysis, packaging, biomedicine and other fields. However, there are relatively few studies on the application of ALD technology in the preparation of hydrogen sensors, especially in the case of eliminating precious metal catalysts, directly obtaining high-performance ultra-thin composite oxide film hydrogen sensors (low operating temperature range, high sensitivity, high selectivity and ultrafast response) by ALD, which has not been reported. Summary of the invention
[0006] The present invention provides an ultrathin composite film hydrogen sensor based on semiconductor metal oxide and a preparation method thereof. The hydrogen sensor is prepared by ALD technology. In the absence of modification with a precious metal catalyst, the sensor achieves high sensitivity response to hydrogen, a low detection limit, an ultrafast response, excellent hydrogen selectivity, and a wide operating temperature range, thereby solving the common problems of semiconductor oxide sensors, such as high operating temperature, slow response recovery, and poor hydrogen selectivity.
[0007] In order to achieve the above purpose, the present invention adopts the following technical solutions: A semiconductor metal oxide-based ultrathin composite film hydrogen sensor comprises, from bottom to top, an insulating substrate, a metal oxide gas-sensitive layer, and a conductive electrode layer; the metal oxide gas-sensitive layer has a thickness of 10-35 nm and is composed of a SnO2 film and an In2O3 film, and the upper and lower positions of the two films can be swapped.
[0008] The method for preparing the above-mentioned ultra-thin composite film hydrogen sensor based on semiconductor metal oxide comprises the following steps: (1) Ultrasonic cleaning of the insulating substrate was performed with acetone, isopropanol, anhydrous ethanol, and deionized water in sequence for 5 minutes, and then blown dry with high-purity nitrogen (99.999%) for later use; (2) Depositing an In2O3 film with a thickness of 5-15 nm or a SnO2 film with a thickness of 5-20 nm on the treated insulating substrate using ALD technology; (3) Depositing a 5-20 nm thick SnO2 film on the In2O3 film by ALD technology, or depositing a 5-15 nm thick In2O3 film on the SnO2 film by ALD technology; (4) Using a mask, deposit metal interdigital electrodes with a thickness of 100-200 nm as conductive electrodes on the prepared SnO2 / In2O3 / substrate or In2O3 / SnO2 / substrate. After wiring and packaging, a SnO2 / In2O3 ultra-thin composite film type hydrogen sensor can be obtained.
[0009] In the above steps, the insulating substrate is an inorganic substrate or a polymer substrate; the temperature of the ALD deposition is room temperature to 300°C, the indium source used is trimethyl indium, the tin source used is tin tetrachloride or tetrakis(dimethylamino)tin (TDMSn), and the oxygen source is water, ozone or plasma oxygen; the deposition temperature, pulse and cleaning time are determined according to the selected source, different sources have different deposition thicknesses per cycle, and films of different thicknesses are obtained by controlling the number of cycles.
[0010] Beneficial effects: The present invention provides an ultra-thin composite film hydrogen sensor based on semiconductor metal oxide and a preparation method thereof. An ultra-thin SnO2 / In2O3 semiconductor metal oxide heterostructure film is prepared on a substrate by ALD technology. The SnO2 / In2O3 thin film hydrogen sensor prepared by ALD technology has good uniformity and high precision. Its thickness is very thin at the nanometer level. Therefore, there is a two-dimensional conductive phenomenon at the interface of the SnO2 and In2O3 films, that is, there is a two-dimensional electron gas. The two-dimensional electron gas can significantly improve the response speed, selectivity and sensitivity of the sensor, and achieve a high sensitivity response to hydrogen (S Ra / Rg =687@1000 ppm), with a low detection limit as low as 1 ppm, ultrafast response (0.4 s@1000 ppm), excellent hydrogen selectivity (S H2 / S NH3 = ~38, S H2 / S H2S = ~15), a wide operating temperature range (75 ℃ - 225 ℃), effectively improving the selectivity for hydrogen and reducing the operating temperature; and the thin film structure of the gas sensor itself can provide a larger specific surface area for the adsorption of gas molecules, promote the migration of carriers in the sensing material, and help improve the sensitivity and response speed of the gas sensor.
[0011] Compared with traditional noble metal modified semiconductor oxide hydrogen sensors, the ALD technology cost of the present invention is greatly reduced; the low-temperature thin film growth technology of ALD can be used to prepare flexible hydrogen sensors, and the ALD preparation method is compatible with MEMS technology, providing a reliable technical foundation for the development of a new generation of integrated, miniaturized and intelligent hydrogen sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The schematic diagram of the structure of the ultra-thin composite film type hydrogen sensor of SnO2 / In2O3 semiconductor metal oxide in the present invention; in the figure, 1-insulating substrate, 2-ALD deposited In2O3 or SnO2 film, 3-ALD deposited SnO2 or In2O3 film, 4-interdigitated electrode; Figure 2 Schematic diagram of the mask of the interdigitated electrode in the present invention, in which 5-the white part represents the metal material of the mask, 6-the black part represents the gap of the mask, 7-the tooth length of the interdigitated electrode, 8-the gap length of the interdigitated electrode teeth, 9-the tooth width of the interdigitated electrode, 10-the width of the interdigitated electrode, and 11-the length of the interdigitated electrode; Figure 3 The sensing performance of the SnO2 / In2O3 sample to 1000 ppm hydrogen in the embodiment of the present invention, including (a) the test curve of the optimal working temperature, (b) the response-recovery curve at the optimal working temperature of 150°C, (c) the response-recovery time curve at different temperatures, and (d) the sensitivity curve of the SnO2 / In2O3 sample to 1-1000 ppm H2; Figure 4 (a) 7 consecutive reproducibility tests of the SnO2 / In2O3 sample in the embodiment of the present invention at the optimal working temperature of 150°C, and (b) sensitivity comparison to 100 ppm H2 and several 100 ppm interfering gases. DETAILED DESCRIPTION
[0013] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments: Example 1
[0014] An ultra-thin composite film type hydrogen sensor based on SnO2 / In2O3 semiconductor metal oxide comprises: a SiO2 / Si substrate, a SnO2 film, an In2O3 film, and a Pt interdigital electrode.
[0015] The method for preparing the above-mentioned sensor comprises the following steps: (1) Select SiO2 / Si as the sensor substrate, place it on a cleaning rack, then place the cleaning rack in a beaker, and then use acetone, isopropanol, anhydrous ethanol, and deionized water to ultrasonically clean it for 5 minutes respectively. Finally, blow dry the cleaned SiO2 / Si substrate with high-purity nitrogen (99.999%) and set it aside; (2) A 10 nm thick porous In2O3 film was deposited on the SiO2 / Si substrate cleaned in step (1) by ALD. The deposition temperature was 160°C. The precursor sources used were trimethylindium (TMIn) and ozone (O3). The pulse time and cleaning time of trimethylindium (TMIn) were 1.0 s and 10.0 s, respectively. The pulse time and cleaning time of ozone (O3) were 2.0 s and 10.0 s, respectively. The number of deposition cycles was 200. (3) Based on step (2), an 8 nm thick SnO2 film was deposited using ALD technology at a deposition temperature of 120 °C. The precursor sources used were tetrakis(dimethylamino)tin (TDMSn) and water (H2O). The pulse and cleaning times of tetrakis(dimethylamino)tin (TDMSn) and water (H2O) were 0.2 s and 6.0 s, respectively, and the number of deposition cycles was 80; (4) Place the interdigital electrode mask close to the sample after step (3), and use magnetron sputtering to sputter ~200 nm thick metal platinum (Pt) as a conductive electrode. After wiring and packaging, it can be used as a sensitive element for detecting hydrogen.
[0016] Figure 3 This is the sensing performance diagram of SnO2 / In2O3 / SiO2 / Si sensor for 1000 ppm hydrogen. Figure 3 (a) shows that in the operating temperature range of 75 ℃ to 225 ℃, the sensitivity of the sensor to 1000 ppm H2 first increases and then decreases, and the sensitivity is highest at 150 ℃, indicating that the optimal operating temperature of the sensor is 150 ℃, and the sensor has a high sensitivity to H2 in the temperature range of 75 ℃ to 225 ℃, indicating that its operating temperature range is wide. Figure 3 (b) is the response-recovery curve of the sensor to 1000 ppm H2 at the optimal working temperature of 150 °C. The sensor has a fast response recovery speed and the highest sensitivity reaches ~658, indicating that the sensor has high sensitivity. Figure 3(c) and (c) are the changes in the response recovery time of the sensor to 1000 ppm H2 at different temperatures. At the optimal working temperature of 150°C, the response time of the sensor to 1000 ppm H2 is only 0.4 s, and the recovery time is 62 s. Even when the working temperature is reduced to 75°C, the response time of the sensor to 1000 ppm H2 is only 2.5 s, indicating that it has an extremely fast response speed. Figure 3 (d) is the sensitivity of the sample to 1-1000 ppm H2, and reflects that there is a certain linear relationship between H2 concentration and sensitivity.
[0017] Figure 4 (a) The reproducibility test of SnO2 / In2O3 / SiO2 / Si sensor at the optimal working temperature of 150℃ was performed for 7 times. After multiple tests, the hydrogen sensitivity of the sample can still remain stable, indicating that the sensor has good reproducibility for hydrogen. Figure 4 (b) Comparison of the sensitivity of the SnO2 / In2O3 / SiO2 / Si sensor to 100 ppm H2 and several 100 ppm interfering gases at the optimal working temperature of 150°C, confirming that the sample has excellent selectivity even without noble metal modification. Example 2
[0018] A composite thin film flexible hydrogen sensor based on SnO2 / In2O3 semiconductor metal oxides includes: a polyethylene terephthalate (PET) substrate, a SnO2 film, an In2O3 film, and an Au interdigital electrode.
[0019] The method for preparing the above-mentioned sensor comprises the following steps: (1) PET was selected as the sensor substrate, and ultrasonic cleaning was performed with acetone, isopropanol, anhydrous ethanol, and deionized water for 5 minutes respectively. Finally, the cleaned PET substrate was blown dry with high-purity nitrogen (99.999%) and set aside; (2) A 12 nm thick porous In2O3 film was deposited on the PET substrate cleaned in step (1) by ALD. The deposition temperature was 50 °C. The precursor sources used were trimethyl indium (TMIn) and plasma oxygen. The pulse time and cleaning time of trimethyl indium (TMIn) were 1.0 s and 10.0 s, respectively. The pulse time and cleaning time of plasma oxygen were 18.0 s and 10.0 s, respectively. The number of deposition cycles was 240. (3) Based on step (2), a 15 nm thick SnO2 film was deposited by ALD technology. The deposition temperature was 50 °C. The precursor sources used were SnCl4 and water (H2O). The pulse and cleaning time of SnCl4 and plasma oxygen were 18 s and 10.0 s, respectively. The number of deposition cycles was 150. (4) The interdigital electrode mask is placed tightly against the sample after step (3), and then gold (Au) with a thickness of ~150 nm is sputtered by magnetron sputtering as a conductive electrode. After wiring and packaging, it can be used as a sensitive element for detecting hydrogen. Example 3
[0020] A composite thin film flexible hydrogen sensor based on SnO2 / In2O3 semiconductor metal oxide includes: a polyimide (PI) substrate, a SnO2 film, an In2O3 film, and Ag interdigital electrodes.
[0021] The method for preparing the above-mentioned sensor comprises the following steps: (1) PI was selected as the sensor substrate, and ultrasonic cleaning was performed with acetone, isopropanol, anhydrous ethanol, and deionized water for 5 minutes respectively. Finally, the cleaned PI substrate was blown dry with high-purity nitrogen (99.999%) and set aside; (2) A layer of 8 nm thick porous In2O3 film was deposited on the PI substrate cleaned in step (1) by ALD. The deposition temperature was 120°C. The precursor sources used were trimethylindium (TMIn) and ozone (O3). The pulse time and cleaning time of trimethylindium (TMIn) were 1.0 s and 10.0 s, respectively. The pulse time and cleaning time of ozone (O3) were 2.0 s and 10.0 s, respectively. The number of deposition cycles was 160. (3) Based on step (2), an 18 nm thick SnO2 film was deposited by ALD technology. The deposition temperature was 120 °C. The precursor sources used were tetrakis(dimethylamino)tin (TDMSn) and water (H2O). The pulse and cleaning times of tetrakis(dimethylamino)tin (TDMSn) and water (H2O) were 0.2 s and 6.0 s, respectively. The number of deposition cycles was 180. (4) The interdigital electrode mask is placed tightly against the sample after step (3), and then silver (Ag) with a thickness of ~150 nm is sputtered by magnetron sputtering as a conductive electrode. After wiring and packaging, it can be used as a sensitive element for detecting hydrogen. Example 4
[0022] An ultra-thin composite film type hydrogen sensor based on SnO2 / In2O3 semiconductor metal oxide comprises: a glass substrate, a SnO2 film, an In2O3 film, and Al interdigital electrodes.
[0023] The method for preparing the above-mentioned sensor comprises the following steps: (1) Select glass as the substrate of the sensor, place it on the cleaning rack, then place the cleaning rack in a beaker, and then use acetone, isopropanol, anhydrous ethanol, and deionized water to ultrasonically clean it for 5 minutes respectively. Finally, blow the cleaned SiO2 / Si substrate dry with high-purity nitrogen (99.999%) and set it aside; (2) A 15 nm thick porous In2O3 film was deposited on the glass substrate cleaned in step (1) by ALD. The deposition temperature was 300°C. The precursor sources used were trimethylindium (TMIn) and ozone (O3). The pulse time and cleaning time of trimethylindium (TMIn) were 1.0 s and 10.0 s, respectively. The pulse time and cleaning time of ozone (O3) were 2.0 s and 10.0 s, respectively. The number of deposition cycles was 300. (3) Based on step (2), a 20 nm thick SnO2 film was deposited by ALD technology. The deposition temperature was 300 °C. The precursor sources used were SnCl4 and water (H2O). The pulse and cleaning time of SnCl4 and water (H2O) were 0.2 s and 6.0 s, respectively. The number of deposition cycles was 200. (4) The interdigital electrode mask is placed tightly against the sample after step (3), and then ~200 nm thick aluminum (Al) is sputtered by magnetron sputtering as a conductive electrode. After wiring and packaging, it can be used as a sensitive element for detecting hydrogen. Example 5
[0024] A composite thin film flexible hydrogen sensor based on In2O3 / SnO2 semiconductor metal oxide includes: a polyimide (PI) substrate, an In2O3 film, a SnO2 film, and an Au interdigital electrode.
[0025] The method for preparing the above-mentioned sensor comprises the following steps: (1) PI was selected as the sensor substrate, and ultrasonic cleaning was performed with acetone, isopropanol, anhydrous ethanol, and deionized water for 5 minutes respectively. Finally, the cleaned PI substrate was blown dry with high-purity nitrogen (99.999%) and set aside; (2) A 14 nm thick SnO2 film was deposited on the PI substrate cleaned in step (1) by ALD. The deposition temperature was 120 °C. The precursor sources used were tetrakis(dimethylamino)tin (TDMSn) and water (H2O). The pulse and cleaning times of tetrakis(dimethylamino)tin (TDMSn) and water (H2O) were 0.2 s and 6.0 s, respectively. The number of deposition cycles was 140. (3) Based on step (2), a 10 nm thick porous In2O3 film was deposited by ALD technology at a deposition temperature of 120 °C. The precursor sources used were trimethyl indium (TMIn) and ozone (O3). The pulse time and cleaning time of trimethyl indium (TMIn) were 1.0 s and 10.0 s, respectively, and the pulse time and cleaning time of ozone (O3) were 2.0 s and 10.0 s, respectively. The number of deposition cycles was 200 cycles. (4) The interdigital electrode mask is placed tightly against the sample after step (3), and then gold (Au) with a thickness of ~200 nm is sputtered by magnetron sputtering as a conductive electrode. After wiring and packaging, it can be used as a sensitive element for detecting hydrogen. Example 6
[0026] An ultra-thin composite film type hydrogen sensor based on In2O3 / SnO2 semiconductor metal oxide comprises: a quartz substrate, an In2O3 film, a SnO2 film, and Ag interdigital electrodes.
[0027] The method for preparing the above-mentioned sensor comprises the following steps: (1) Select quartz as the substrate of the sensor, place it on the cleaning rack, then place the cleaning rack in a beaker, and then use acetone, isopropanol, anhydrous ethanol, and deionized water to ultrasonically clean it for 5 minutes respectively. Finally, blow dry the cleaned SiO2 / Si substrate with high-purity nitrogen (99.999%) and set it aside; (2) A 10 nm thick SnO2 film was deposited on the quartz substrate cleaned in step (1) by ALD. The deposition temperature was 200°C. The precursor sources used were SnCl4 and water (H2O). The pulse and cleaning times of SnCl4 and water (H2O) were 0.2 s and 6.0 s, respectively. The number of deposition cycles was 100. (3) Based on step (2), an 8 nm thick porous In2O3 film was deposited by ALD technology at a deposition temperature of 120 °C. The precursor sources used were trimethyl indium (TMIn) and ozone (O3). The pulse time and cleaning time of trimethyl indium (TMIn) were 1.0 s and 10.0 s, respectively, and the pulse time and cleaning time of ozone (O3) were 2.0 s and 10.0 s, respectively. The number of deposition cycles was 160. (4) The interdigital electrode mask is placed tightly against the sample after step (3), and then ~200 nm of silver (Ag) is sputtered as a conductive electrode using magnetron sputtering. After wiring and packaging, it can be used as a sensitive element for detecting hydrogen.
[0028] The above are only preferred embodiments of the present invention, which will help those skilled in the art to further understand the present invention, but do not limit the present invention in any form. It should be pointed out that for those skilled in the art, without departing from the concept of the present invention, several modifications and improvements made are all protected by the present invention.
Claims
1. An ultra-thin composite film hydrogen sensor based on semiconductor metal oxide, characterized in that: From bottom to top, there are an insulating substrate, a metal oxide gas-sensitive layer, and a conductive electrode layer; the metal oxide gas-sensitive layer is composed of a SnO2 film and an In2O3 film, and the upper and lower positions of the SnO2 film and the In2O3 film can be swapped.
2. The ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 1 is characterized in that: The thickness of the In2O3 film is 5-15 nm.
3. The ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 1 or 2, characterized in that: The SnO2 film thickness is 5-20 nm.
4. The ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 1, characterized in that: The thickness of the conductive electrode layer is 100-200 nm.
5. A method for preparing an ultra-thin composite film hydrogen sensor based on semiconductor metal oxide, characterized in that: The following steps are involved: Deposition of In2O3 or SnO2 thin films on insulating substrates by ALD technology; Depositing a SnO2 film on an In2O3 film by ALD technology, or depositing an In2O3 film on a SnO2 film by ALD technology; A metal interdigital electrode is deposited on the prepared SnO2 / In2O3 / substrate or In2O3 / SnO2 / substrate using a mask as a conductive electrode, and a SnO2 / In2O3 ultra-thin composite film hydrogen sensor can be obtained after wiring and packaging.
6. The method for preparing the ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 5, characterized in that: The insulating substrate is an inorganic substrate or a polymer substrate.
7. The method for preparing the ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 5, characterized in that: The ALD deposition temperature is from room temperature to 300° C.
8. The method for preparing the ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 5 or 7, characterized in that: The indium source used in ALD is trimethylindium.
9. The method for preparing the ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 5 or 7, characterized in that: The tin source used in ALD is tin tetrachloride or tetrakis(dimethylamino)tin.
10. The method for preparing the ultra-thin composite film hydrogen sensor based on semiconductor metal oxide according to claim 5 or 7, characterized in that: The ALD oxygen source is water, ozone or plasma oxygen.
Citation Information
Patent Citations
Semiconductor film gas sensor and preparation method thereof
CN111624236A
Preparation method of integrated MEMS hydrogen sensor
CN114152652A
Hydrogen gas detecting element and method of manufacturing the same
JP2002328108A
ITO thin-film hydrogen gas sensor and method of manufacturing the same capable of increasing sensitivity of sensor
KR100589660B1
Semiconductor oxide nanofiber-nanorod hybrid structure and environmental gas sensor using the same
US20110227061A1
Cited By
In2O3 nano material oriented growth method, device, sensor and electronic nose
CN120272877A
In2o3 nanomaterial directional growth method and device, sensor and electronic nose
CN120272877B