Three-dimensional carbon nanotube-asphalt-based porous carbon composite material as well as preparation method and application thereof
Through the self-supporting cross network structure of three-dimensional carbon nanotube-pitch-based porous carbon composite materials, the problems of kinetic mismatch of lithium-ion capacitor cathode materials and poor controllability of electrochemical properties of porous carbon materials are solved, and efficient charge transport and Storage, suitable for applications in the field of new energy.
Patent Information
- Application Number
- CN202410729672.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
AI Technical Summary
The kinetic mismatch of lithium-ion capacitor cathode materials leads to insufficient capacity. Traditional metal compound cathode materials are costly, complex to prepare, and pollute the environment. Porous carbon materials suffer from poor structural controllability in electrochemical performance.
Using three-dimensional carbon nanotube-asphalt-based porous carbon composite materials, the carbon nanotube sponge and asphalt porous carbon are cross-linked to form a self-supporting cross network structure, which provides fast and orderly charge transfer channels and abundant adsorption sites, reducing electrolyte ions diffusion resistance.
It achieves high specific capacitance and high rate performance of the lithium ion capacitor cathode, has excellent high power density and long cycle life, is easy to operate and is suitable for large-scale production.
Smart Images

Figure CN118748128A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon materials, and specifically relates to a three-dimensional carbon nanotube-asphalt-based porous carbon composite material, a preparation method and an application thereof. Background Art
[0002] Lithium-ion capacitors are generally composed of three parts: lithium-ion battery electrode materials, supercapacitor electrode materials, and organic lithium salt electrolytes. They can be used for energy storage in wind power generation, street lighting, hybrid vehicles, etc. Lithium-ion battery electrode materials can provide high specific capacity, while supercapacitor electrode materials can increase the power capacity of the system. Therefore, lithium-ion capacitors have both high energy density and power density.
[0003] The main problem of lithium-ion capacitors is the kinetic mismatch between the battery-type negative electrode and the capacitor-type positive electrode due to the charge storage mechanism. In fact, the negative electrode capacity of lithium-ion capacitors is much larger than the positive electrode, and the capacity of the lithium-ion capacitor constructed by it depends on the lower positive electrode capacity, so it is necessary to study positive electrode materials with high specific capacity.
[0004] The positive electrode of a lithium-ion capacitor stores charge mainly through the adsorption of hexafluorophosphate ions, which requires the positive electrode material to have an ultra-high specific surface area.
[0005] In addition, the cathode materials of traditional metal compounds still face the problems of expensive raw materials, complex preparation process, high cost, serious volume expansion, environmental pollution, etc., and it is still difficult to achieve large-scale production. Since porous carbon materials have a wide range of sources, simple preparation process, and low cost, they meet the concept of sustainable development and have broad prospects for large-scale application in the future. With the widespread use of porous carbon materials, many methods for synthesizing porous carbon composite materials have emerged, such as electrostatic co-assembly, in-situ polymerization, chemical vapor deposition (CVD), electrochemical polymerization, and hydrothermal synthesis. Fu et al. used electrostatic co-assembly to assemble silica and graphene on the surface of carbon fiber through interlayer electrostatic action to form a composite. The obtained composite material has a hierarchical structure, and the high surface roughness increases the specific surface area, enhances stress, and steadily improves the electrochemical performance. Feng's research group used graphene oxide (GO) solution and aniline monomer to carry out electrochemical polymerization on stainless steel sheets to prepare graphene oxide / polyaniline (GO / PANI) composite materials. Different mass concentrations of GO are used to improve electrochemical performance. The large surface area of GO sheets provides active sites for the deposition of PANI, and the synergistic effect between PANI and GO accelerates the diffusion of electrolyte ions, showing high electrochemical performance. However, for these carbon-based composite materials, their microscopic pore richness and surface properties will greatly affect the electrochemical performance, and the morphology often shows problems such as monomer agglomeration and poor structural controllability, resulting in poor electrochemical performance.
[0006] Therefore, it is urgent to study and prepare ordered pore structures that are conducive to improving charge transfer, rich porous structures that are conducive to lithium ion adsorption and desorption, and highly controllable porous carbon-based composite materials for use as supercapacitor electrode materials for efficient energy storage and utilization. Summary of the invention
[0007] In order to overcome the above problems existing in the prior art, the purpose of the present invention is to provide a three-dimensional carbon nanotube-asphalt-based porous carbon composite material and a preparation method and application thereof. The method can uniformly coat the asphalt-based porous carbon particles on the three-dimensional skeleton of carbon nanotubes, so that the electrode material has the characteristics of enhanced self-supporting three-dimensional network and high specific surface area, etc., can effectively reduce the diffusion resistance of electrolyte ions, shorten the diffusion path of ions, and provide a large number of active sites for the adsorption of hexafluorophosphate ions on the positive electrode side, thereby achieving high specific capacitance and high rate performance of the positive electrode of the lithium ion capacitor at high potential.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] A three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge material, in which the carbon nanotube sponge channels and the asphalt porous carbon are cross-linked to form a rich three-dimensional self-supporting cross-network structure, which provides a fast and orderly channel for charge transfer;
[0010] The area around the carbon nanotubes is occupied by micropores and mesoporous structures, and the surface of the carbon nanotube sponge is covered with a asphalt porous carbon layer, forming a porous structure with regular and orderly structure and dense distribution.
[0011] The channel can be quickly charged and discharged when used as a positive electrode material for a lithium ion capacitor.
[0012] The porous structure provides a large number of adsorption sites and a high specific surface area when used as a positive electrode material.
[0013] A method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite material comprises the following steps;
[0014] Step 1: Preparation of carbon nanotube sponge;
[0015] A clean quartz substrate is placed in the middle of the quartz tube of the reaction furnace and the quartz tube is sealed, and the temperature rise program of the reaction furnace is set. Argon gas is passed to remove residual air in the quartz tube. When the temperature of the reaction furnace is raised to 820-940° C., a ferrocene / dichlorobenzene carbon source solution is injected under a hydrogen / argon mixed atmosphere, and the reaction is carried out for 0.5-4 hours. After the reaction, the injection of the hydrogen-argon mixed gas and the ferrocene / dichlorobenzene carbon source solution is turned off, and the temperature is lowered with the furnace under argon protection to obtain a carbon nanotube sponge;
[0016] Step 2: Preparation of carbon nanotube-pitch-based mesoporous carbon composite sponge precursor;
[0017] Take medium-temperature asphalt powder (0.2-1 g) and potassium hydroxide (0.6-3 g) in a mass ratio of 1:3, add them to 15 mL of tetrahydrofuran solution and 15 mL of anhydrous ethanol respectively, and stir and dissolve them respectively;
[0018] Use a dropper to add the tetrahydrofuran solution containing the medium-temperature asphalt powder dropwise into the anhydrous ethanol solution containing potassium hydroxide, and stir evenly for several hours to obtain a mixed solution;
[0019] The carbon nanotube sponge obtained in step 1 is immersed in the mixed solution for 24 hours; the carbon nanotube sponge is pressed several times to fully absorb the asphalt and KOH, and a carbon nanotube-asphalt porous carbon precursor embedded with medium-temperature asphalt and KOH is obtained;
[0020] Step 3: Preparation of carbon nanotube-pitch-based porous carbon composite materials:
[0021] The carbon nanotube-asphalt-based porous carbon precursor was freeze-dried, then subjected to high-temperature carbonization and activation treatment in an inert atmosphere using a tubular furnace, and finally the residual hydroxide was washed away with hydrochloric acid and washed with deionized water until the pH value of the sample was neutral, thereby obtaining a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge material with a porous structure.
[0022] The argon flow rate for exhausting the residual air in the reaction chamber in step 1 is 100-200 mL min -1 Its purpose and effect is to remove the residual air in the tube furnace and ensure that the sample does not come into contact with or react with the air during the chemical vapor deposition process.
[0023] During the reaction in step 1, the flow rate of hydrogen-argon mixed gas is 1500-2500 mL min -1 The argon flow rate is 200~400mL min -1 The purpose and effect is to avoid deformation and cracking of the generated carbon nanotube sponge during the sponge deposition process, thereby obtaining a sample with excellent mechanical properties.
[0024] The concentration of the ferrocene / dichlorobenzene carbon source solution in step 1 is 20-100 mg mL -1 , feed rate 0.1~0.4mL min -1 ; Its purpose and effect is to regulate the density of the generated carbon nanotube sponge by controlling the concentration and feed rate of the carbon source solution.
[0025] When cooling in step 1, the argon flow rate is 100-200 mL min -1The purpose and effect is to prevent gas back-inhalation during the cooling process and to avoid air entering the tube and reacting with the carbon nanotube sponge.
[0026] In the step 2, the stirring time of dissolving the medium-temperature asphalt powder into tetrahydrofuran is 3 to 15 minutes, the stirring time of dissolving potassium hydroxide into anhydrous ethanol is 3 to 15 minutes, the mixing stirring time of the tetrahydrofuran solution containing asphalt and the anhydrous ethanol solution containing potassium hydroxide is 5 hours, and the soaking time is 6 to 24 hours.
[0027] The mass ratio of the medium-temperature asphalt powder to potassium hydroxide is 1:3.
[0028] The temperature of high-temperature carbonization and activation in step three is 600-800°C, and the time is 30-120 minutes; its purpose and effect are to remove impurities such as tar in the medium-temperature asphalt on the one hand, and to decompose potassium hydroxide in the high-temperature process on the other hand, to etch and form holes in the asphalt attached to the surface of the carbon tube sponge, so as to achieve carbonization and activation of the material.
[0029] In step 3, the freeze drying temperature is -70 to -60°C and the freezing time is 12 to 24 hours. The purpose and effect of the freeze drying are to remove the tetrahydrofuran solvent and the anhydrous ethanol solvent in the sponge.
[0030] The inert atmosphere introduced into the tube furnace in step 3 is argon or nitrogen. Its purpose and effect is to remove the residual air in the tube furnace and ensure that the sample does not contact and react with air during the carbonization and activation process.
[0031] In step 3, the concentration of hydrochloric acid is 0.5-5M, and the pickling time is 1-5 hours. The purpose and effect is to remove the residual hydroxide in the sample by acid-base neutralization, so that the pH of the sample remains neutral.
[0032] The three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge material is applied to positive electrode materials of lithium ion capacitors.
[0033] Beneficial effects of the present invention:
[0034] 1. The three-dimensional carbon nanotube-pitch-based porous carbon composite sponge material prepared by the present invention is filled with a porous structure with regular and orderly structure and dense distribution, and the surface of the carbon nanotube is wrapped by a porous carbon layer, which provides a large number of adsorption sites and a high specific surface area. This structure is conducive to promoting the efficient transfer and storage of charge, thereby improving the rapid charging and discharging of lithium ion capacitors at high power.
[0035] 2. The carbon nanotube-mesoporous carbon composite sponge prepared by the present invention is a three-dimensional self-supporting cross-network structure. This orderly channel structure is conducive to the rapid transmission of charges and improves the rapid charging and discharging performance of lithium ion capacitors.
[0036] 3. The preparation method of the present invention is novel and easy to operate. The prepared three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge can be prepared in large quantities according to actual needs and is expected to be well applied in actual production.
[0037] 4. The three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge prepared by the present invention has excellent high power density and long cycle life when used as a positive electrode material for lithium ion capacitors, and has broad application prospects in the field of new energy. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a scanning electron microscope photograph of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1.
[0039] Figure 2 This is a transmission electron microscope photograph of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1.
[0040] Figure 3 This is the cyclic voltammetry curve of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1 as the positive electrode of a lithium ion capacitor.
[0041] Figure 4 This is the constant current charge and discharge curve of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1 as the positive electrode of a lithium ion capacitor.
[0042] Figure 5 This is a rate performance diagram of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1 as a positive electrode of a lithium ion capacitor.
[0043] Figure 6 This is the long cycle curve at a current density of 5 A / g when the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1 is used as the positive electrode of a lithium ion capacitor.
[0044] Figure 7 Energy-power density curve of a lithium ion capacitor assembled with the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1 as the positive electrode material and pure carbon nanotube sponge as the negative electrode.
[0045] Figure 8 This is a physical picture of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge obtained in Example 1 as the positive electrode material. DETAILED DESCRIPTION
[0046] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0047] Example 1
[0048] This embodiment provides a method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite sponge, which is implemented according to the following steps:
[0049] 1. Preparation of carbon nanotube sponge: Place a clean quartz substrate in the middle of the quartz tube of the reactor and seal the quartz tube. Set the heating program of the reactor and introduce 100 mL min -1 The argon gas was used to remove the air in the reaction chamber to keep the atmosphere stable. When the temperature rose to 880 °C, the argon flow rate was adjusted to 300 mL min -1 , and pass 2000mL min -1 The hydrogen-argon mixture was turned on and the precision injection pump was turned on to inject 60 mg mL -1 The ferrocene / dichlorobenzene carbon source reaction solution was fed at a rate of 0.26 mL min -1 After the reaction was completed, the ferrocene / dichlorobenzene carbon source reaction solution was stopped and the hydrogen-argon mixed gas was turned off. The reaction furnace was heated to 45 °C at a gas flow rate of 100 mL min -1 Cool down under the protection of argon atmosphere.
[0050] 2. Preparation of carbon nanotube-asphalt-based mesoporous carbon composite sponge precursor: Take 0.2g of medium-temperature asphalt powder and 0.6g of potassium hydroxide, add them into a beaker containing 15mL of tetrahydrofuran and 15mL of anhydrous ethanol respectively, and stir at room temperature until dissolved; use a dropper to add the tetrahydrofuran solution containing medium-temperature asphalt powder dropwise into the anhydrous ethanol solution containing potassium hydroxide, and obtain a mixed solution after stirring at room temperature; add the carbon nanotube sponge obtained in step 1, and let it stand and soak for 24 hours to obtain a carbon nanotube asphalt-based porous carbon precursor embedded with medium-temperature asphalt and KOH.
[0051] 3. Preparation of carbon nanotube-asphalt-based porous carbon composite sponge: The statically immersed carbon nanotube asphalt-based porous carbon precursor is taken out from the mixed solution, freeze-dried, and then carbonized and activated at 700°C for 2 hours in a nitrogen atmosphere. After the carbonization, the residual hydroxide is removed with hydrochloric acid, and the composite material is oscillated and washed with deionized water until the pH value is neutral, and freeze-dried to obtain a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge.
[0052] The three-dimensional carbon nanotube-mesoporous carbon composite sponge prepared in this example was characterized and its capacitance performance was tested. The scanning electron microscope (SEM) photos at different magnifications are shown in FIG. Figure 1 (a)(b) shows the transmission electron microscope (TEM) photos at different magnifications. Figure 2 (a)(b) shows the cyclic voltammetry curve, constant current charge-discharge curve, rate curve and long cycle curve when used as a positive electrode material for lithium ion capacitors. Figures 3 to 6As shown, the energy-power density curve when assembled into a lithium-ion capacitor is as follows Figure 7 The actual picture shown is as follows Figure 8 shown.
[0053] like Figure 1 As shown in the attached Figure 1 As shown, attached Figure 1 (a) Attachment Figure 1 (b) Scanning electron microscope photos of three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge materials at different magnifications
[0054] like Figure 2 Shown: Attached Figure 2 (a) Attachment Figure 2 (b) is a transmission electron microscope photograph of the three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge material prepared in step 3 at different magnifications.
[0055] A three-dimensional carbon nanotube-pitch-based porous carbon composite sponge material, scanning electron microscope (SEM) photos at different magnifications; attached Figure 2 (a) Attachment Figure 2 (b) is a transmission electron microscope (TEM) photo of the three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge material prepared in step 3 at different magnifications. From the SEM image, it can be clearly seen that the area in the image is occupied by asphalt-based porous carbon, and the carbon nanotube sponge channels and asphalt porous carbon are cross-linked to form a rich three-dimensional self-supporting cross-network structure. The rich cross-network structure provides a fast and orderly channel for charge transfer, and can be quickly charged and discharged when it is used as a positive electrode material for lithium ion capacitors; from the TEM image, it can be clearly seen that the area around the carbon nanotubes is occupied by a large number of micropores and mesoporous structures, and the surface of the carbon nanotube sponge is coated with an asphalt porous carbon layer, forming a porous structure with regular and orderly structure and dense distribution. These porous structures provide a large number of adsorption sites and a high specific surface area when it is used as a positive electrode material, thereby improving the positive electrode performance.
[0056] like Figure 3 Shown: Attached Figure 3 The cyclic voltammetry curve of three-dimensional carbon nanotube-pitch-based porous carbon composite sponge as the positive electrode of lithium ion capacitor. It can be seen that the CV curve at different scan rates is a quasi-rectangular curve, which has typical capacitance characteristics.
[0057] like Figure 4 Shown is the constant current charge and discharge curve of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge as the positive electrode of the lithium ion capacitor. It can be seen that the image presents an isosceles triangle, indicating that it exhibits good performance at different rates.
[0058] like Figure 5Shown is the rate performance diagram of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge as the positive electrode of a lithium ion capacitor. It has a discharge specific capacity of 196 mAh / g at 0.1 A / g, and still has a discharge specific capacity of 125 mAh / g at a high current density of 10 A / g, indicating its excellent rate performance.
[0059] like Figure 6 Shown is a long cycle diagram of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge as the positive electrode of a lithium ion capacitor at 5A / g, showing its stability during 10,000 long cycles, indicating its high capacity retention rate and stable coulombic efficiency.
[0060] like Figure 7 Shown is the power density-energy density curve of a lithium ion capacitor assembled with a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge as the positive electrode of a lithium ion capacitor and pure carbon nanotube sponge as the negative electrode, achieving a high energy density of 168Wh / kg at 260W / kg and a high energy density of 57Wh / kg at a high power density of 26kW / kg.
[0061] Example 2
[0062] This embodiment provides a method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite sponge, which is implemented according to the following steps:
[0063] 1. Preparation of carbon nanotube sponge: Place a clean quartz substrate in the middle of the quartz tube of the reactor and seal the quartz tube. Set the heating program of the reactor and introduce 100 mL min -1 The argon gas was used to remove the air in the reaction chamber to keep the atmosphere stable. When the temperature rose to 880 °C, the argon flow rate was adjusted to 300 mL min -1 , and pass 2000mL min -1 The hydrogen-argon mixture was turned on and the precision injection pump was turned on to inject 60 mg mL -1 The ferrocene / dichlorobenzene carbon source reaction solution was fed at a rate of 0.26 mL min -1 After the reaction was completed, the ferrocene / dichlorobenzene carbon source reaction solution was stopped and the hydrogen-argon mixed gas was turned off. The reaction furnace was heated to 45 °C at a gas flow rate of 100 mL min -1 Cool down under the protection of argon atmosphere.
[0064] 2. Preparation of carbon nanotube-asphalt-based porous carbon composite sponge precursor: Take 0.2g of medium-temperature asphalt powder and 0.6g of potassium hydroxide, add them into a beaker containing 15mL of tetrahydrofuran and 15mL of anhydrous ethanol respectively, and stir at room temperature until dissolved; use a dropper to add the tetrahydrofuran solution containing medium-temperature asphalt powder dropwise into the anhydrous ethanol solution containing potassium hydroxide, and obtain a mixed solution after stirring at room temperature; add the carbon nanotube sponge obtained in step 1, let it stand and soak for 24 hours to obtain a carbon nanotube asphalt-based porous carbon precursor embedded with medium-temperature asphalt and KOH.
[0065] 3. Preparation of carbon nanotube-asphalt-based porous carbon composite sponge: The statically immersed carbon nanotube asphalt-based porous carbon precursor is taken out from the mixed solution, freeze-dried, and then carbonized and activated at 700°C for 2 hours in a nitrogen atmosphere. After the carbonization, the residual hydroxide is removed with hydrochloric acid, and the composite material is oscillated and washed with deionized water until the pH value is neutral, and freeze-dried to obtain a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge.
[0066] Example 3
[0067] This embodiment provides a method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite sponge, which is implemented according to the following steps:
[0068] 1. Preparation of carbon nanotube sponge: Place a clean quartz substrate in the middle of the quartz tube of the reactor and seal the quartz tube. Set the heating program of the reactor and introduce 100 mL min -1 The argon gas was used to remove the air in the reaction chamber to keep the atmosphere stable. When the temperature rose to 880 °C, the argon flow rate was adjusted to 300 mL min -1 , and pass 2000mL min -1 The hydrogen-argon mixture was turned on and the precision injection pump was turned on to inject 60 mg mL -1 The ferrocene / dichlorobenzene carbon source reaction solution was fed at a rate of 0.26 mL min -1 After the reaction was completed, the ferrocene / dichlorobenzene carbon source reaction solution was stopped and the hydrogen-argon mixed gas was turned off. The reaction furnace was heated to 45 °C at a gas flow rate of 100 mL min -1 Cool down under the protection of argon atmosphere.
[0069] 2. Preparation of carbon nanotube-asphalt porous carbon composite sponge precursor: Take 0.6g of medium-temperature asphalt powder and 1.8g of potassium hydroxide, add them into beakers containing 15mL of tetrahydrofuran and 15mL of anhydrous ethanol respectively, and stir at room temperature until dissolved; use a dropper to add the tetrahydrofuran solution containing medium-temperature asphalt powder dropwise into the anhydrous ethanol solution containing potassium hydroxide, and obtain a mixed solution after stirring at room temperature; add the carbon nanotube sponge obtained in step 1, and let it stand and soak for 24 hours to obtain a carbon nanotube asphalt-based porous carbon precursor embedded with medium-temperature asphalt and KOH.
[0070] 3. Preparation of carbon nanotube-asphalt-based porous carbon composite materials: The statically immersed carbon nanotube asphalt-based porous carbon precursor is taken out from the mixed solution, freeze-dried, and then carbonized and activated at 700°C for 2 hours in a nitrogen atmosphere. After the carbonization, the residual hydroxide is removed with hydrochloric acid, and the composite material is oscillated and washed with deionized water until the pH value is neutral, and freeze-dried to obtain a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge.
[0071] Example 4
[0072] This embodiment provides a method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite sponge, which is implemented according to the following steps:
[0073] 1. Preparation of carbon nanotube sponge: Place a clean quartz substrate in the middle of the quartz tube of the reactor and seal the quartz tube. Set the heating program of the reactor and introduce 100 mL min -1 The argon gas was used to remove the air in the reaction chamber to keep the atmosphere stable. When the temperature rose to 880 °C, the argon flow rate was adjusted to 300 mL min -1 , and pass 2000mL min -1 The hydrogen-argon mixture was turned on and the precision injection pump was turned on to inject 60 mg mL -1 The ferrocene / dichlorobenzene carbon source reaction solution was fed at a rate of 0.26 mL min -1 After the reaction was completed, the ferrocene / dichlorobenzene carbon source reaction solution was stopped and the hydrogen-argon mixed gas was turned off. The reaction furnace was heated to 45 °C at a gas flow rate of 100 mL min -1 Cool down under the protection of argon atmosphere.
[0074] 2. Preparation of carbon nanotube-asphalt porous carbon composite sponge precursor: Take 1g of medium-temperature asphalt powder and 3g of potassium hydroxide, add them into beakers containing 15mL of tetrahydrofuran and 15mL of anhydrous ethanol respectively, and stir at room temperature until dissolved; use a dropper to add the tetrahydrofuran solution containing medium-temperature asphalt powder dropwise into the anhydrous ethanol solution containing potassium hydroxide, and obtain a mixed solution after stirring at room temperature; add the carbon nanotube sponge obtained in step 1, and let it stand and soak for 24 hours to obtain a carbon nanotube asphalt-based porous carbon precursor embedded with medium-temperature asphalt and KOH.
[0075] 3. Preparation of carbon nanotube-asphalt-based porous carbon composite sponge: The statically immersed carbon nanotube asphalt-based porous carbon precursor is taken out from the mixed solution, freeze-dried, and then carbonized and activated at 700°C for 2 hours in a nitrogen atmosphere. After the carbonization, the residual hydroxide is removed with hydrochloric acid, and the composite material is oscillated and washed with deionized water until the pH value is neutral, and freeze-dried to obtain a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge.
[0076] Example 5
[0077] This embodiment provides a method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite sponge, which is implemented according to the following steps:
[0078] 1. Preparation of carbon nanotube sponge: Place a clean quartz substrate in the middle of the quartz tube of the reactor and seal the quartz tube. Set the heating program of the reactor and introduce 100 mL min -1 The argon gas was used to remove the air in the reaction chamber to keep the atmosphere stable. When the temperature rose to 880 °C, the argon flow rate was adjusted to 300 mL min -1 , and pass 2000mL min -1 The hydrogen-argon mixture was turned on and the precision injection pump was turned on to inject 60 mg mL -1 The ferrocene / dichlorobenzene carbon source reaction solution was fed at a rate of 0.26 mL min -1 After the reaction was completed, the ferrocene / dichlorobenzene carbon source reaction solution was stopped and the hydrogen-argon mixed gas was turned off. The reaction furnace was heated to 45 °C at a gas flow rate of 100 mL min -1 Cool down under the protection of argon atmosphere.
[0079] 2. Preparation of carbon nanotube-asphalt porous carbon composite sponge precursor: Take 0.6g of medium-temperature asphalt powder and 1.8g of potassium hydroxide, add them into beakers containing 15mL of tetrahydrofuran and 15mL of anhydrous ethanol respectively, and stir at room temperature until dissolved; use a dropper to add the tetrahydrofuran solution containing medium-temperature asphalt powder dropwise into the anhydrous ethanol solution containing potassium hydroxide, and obtain a mixed solution after stirring at room temperature; add the carbon nanotube sponge obtained in step 1, and let it stand and soak for 24 hours to obtain a carbon nanotube asphalt-based porous carbon precursor embedded with medium-temperature asphalt and KOH.
[0080] 3. Preparation of carbon nanotube-asphalt-based porous carbon composite sponge: The statically immersed carbon nanotube asphalt-based porous carbon precursor is taken out from the mixed solution, freeze-dried, and then carbonized and activated at 700°C for 2 hours in a nitrogen atmosphere. After the carbonization, the residual hydroxide is removed with hydrochloric acid, and the composite material is oscillated and washed with deionized water until the pH value is neutral, and freeze-dried to obtain a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge.
Claims
1. A three-dimensional carbon nanotube-pitch-based porous carbon composite sponge material, characterized in that: The carbon nanotube sponge channels and the asphalt porous carbon are cross-linked to form a rich three-dimensional self-supporting cross-network structure, which provides a fast and orderly channel for charge transfer. The area around the carbon nanotubes is occupied by micropores and mesoporous structures, and the surface of the carbon nanotube sponge is covered with a asphalt porous carbon layer, forming a porous structure with regular and orderly structure and dense distribution.
2. The three-dimensional carbon nanotube-pitch-based porous carbon composite sponge material according to claim 1, characterized in that: The channel can be quickly charged and discharged when used as a positive electrode material for a lithium ion capacitor.
3. The three-dimensional carbon nanotube-pitch-based porous carbon composite sponge material according to claim 1, characterized in that: The porous structure provides a large number of adsorption sites and a high specific surface area when used as a positive electrode material.
4. A method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite material according to any one of claims 1 to 3, characterized in that: The steps include: Step 1: Preparation of carbon nanotube sponge; A clean quartz substrate is placed in the middle of the quartz tube of the reaction furnace and the quartz tube is sealed, the temperature rise program of the reaction furnace is set, argon gas is passed to remove residual air in the quartz tube, and when the temperature of the reaction furnace is raised to 820-940°C, a ferrocene / dichlorobenzene carbon source solution is injected in a hydrogen / argon mixed atmosphere, and the reaction is carried out for 0.5-4h. After the reaction, the injection of the hydrogen-argon mixed gas and the ferrocene / dichlorobenzene carbon source solution is turned off, and the temperature is lowered with the furnace under the protection of argon gas to obtain a carbon nanotube sponge; Step 2: Preparation of carbon nanotube-pitch-based mesoporous carbon composite sponge precursor; Take medium-temperature asphalt powder and potassium hydroxide in a mass ratio of 1:3, add them into tetrahydrofuran solution and anhydrous ethanol respectively, and stir and dissolve them respectively; Use a dropper to add the tetrahydrofuran solution containing the medium-temperature asphalt powder dropwise into the anhydrous ethanol solution containing potassium hydroxide, and stir evenly for several hours to obtain a mixed solution; Soaking the carbon nanotube sponge obtained in step 1 in the mixed solution; Press the carbon nanotube sponge several times to fully absorb the asphalt and KOH, and obtain a carbon nanotube-asphalt porous carbon precursor embedded with medium-temperature asphalt and KOH; Step 3: Preparation of carbon nanotube-pitch-based porous carbon composite materials: The carbon nanotube-asphalt-based porous carbon precursor was freeze-dried, then subjected to high-temperature carbonization and activation treatment in an inert atmosphere using a tubular furnace, and finally the residual hydroxide was washed away with hydrochloric acid and washed with deionized water until the pH value of the sample was neutral, thereby obtaining a three-dimensional carbon nanotube-asphalt-based porous carbon composite sponge material with a porous structure.
5. The method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite material according to claim 4, characterized in that: The argon flow rate for exhausting the residual air in the reaction chamber in step 1 is 100-200 mL min -1 ; During the reaction in step 1, the flow rate of hydrogen-argon mixed gas is 1500-2500 mL min -1 The argon flow rate is 200~400mL min -1 ; The concentration of the ferrocene / dichlorobenzene carbon source solution in step 1 is 20-100 mg mL -1 , feed rate 0.1~0.4mL min -1 ; When cooling in step 1, the argon flow rate is 100-200 mL min -1 .
6. The method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite material according to claim 4, characterized in that: In the step 2, the stirring time of dissolving the medium-temperature asphalt powder into tetrahydrofuran is 3 to 15 minutes, the stirring time of dissolving potassium hydroxide into anhydrous ethanol is 3 to 15 minutes, and the soaking time is 6 to 24 hours.
7. The method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite material according to claim 6, characterized in that: The mass ratio of the medium-temperature asphalt powder to potassium hydroxide is 1:
3.
8. The method for preparing a three-dimensional carbon nanotube-pitch-based porous carbon composite material according to claim 4, characterized in that: In the step 3, the temperature of high temperature carbonization and activation is 600-800°C and the time is 30-120min; In step 3, the freeze drying temperature is -70 to -60°C, and the freezing time is 12 to 24 hours; The inert atmosphere introduced into the tubular furnace in step 3 is argon or nitrogen; In step 3, the concentration of hydrochloric acid is 0.5-5M, and the pickling time is 1-5h.
9. The use of the three-dimensional carbon nanotube-pitch-based porous carbon composite sponge material according to any one of claims 1 to 8, characterized in that: Positive electrode material for lithium-ion capacitors.