High-density thermoelectric device and preparation method thereof

Through mask-assisted deposition and double-sided bonding methods, the problem of photoresist limiting the high-temperature deposition of thermoelectric materials is solved, the preparation of high-density thermoelectric devices is achieved, the process is simplified, the cost is reduced, and the device performance is improved.

CN118748904APending Publication Date: 2024-10-08SHANGHAI IND U TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410851554.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing thermoelectric device preparation methods rely on photoresist, which makes high-temperature deposition difficult and limits the performance improvement of thermoelectric materials. The process is complex and costly, making it difficult to achieve high-density array integration.

Method used

Using a mask-assisted deposition process and double-sided bonding method, patterned electrodes and thermoelectric arms are formed through magnetron sputtering deposition, combined with pressurized high-temperature bonding to avoid the limitations of photoresist and achieve high-density arrays of high-performance thermoelectric materials integrated.

Benefits of technology

It achieves high-density array integration of high-performance thermoelectric materials with simple process, easy operation and low cost, and improves the adhesion between the electrode and the substrate and the overall performance of the thermoelectric device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748904A_ABST
    Figure CN118748904A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-density thermoelectric device, and the method comprises the following steps: providing a plurality of mask plates, namely a first mask plate, a second mask plate, a third mask plate and a fourth mask plate, and providing a first substrate and a second substrate; using the first mask plate to deposit on the surface of the first substrate to form a patterned lower electrode, and using the second mask plate to deposit on the surface of the second substrate to form a patterned upper electrode; sequentially depositing an N-type thermoelectric arm and a first bonding layer on the surface of the first substrate by using the third mask plate; sequentially depositing a P-type thermoelectric arm and a second bonding layer on the surface of the second substrate by using the fourth mask plate; and carrying out pressurized high-temperature bonding on the first bonding layer and the second bonding layer to obtain the high-density thermoelectric device. According to the method, the limitation of the photoresist on the deposition temperature of the thermoelectric material is avoided, the high-density integration of the thermoelectric material is realized by matching with the high-precision mask, and the double-sided bonding process is simple and reliable and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a high-density thermoelectric device and a preparation method thereof. Background Art

[0002] Thermoelectric devices refer to functional electronic devices built based on thermoelectric materials. Through microelectronic processes such as electrode interconnection and packaging, the thermoelectric properties of thermoelectric materials can be effectively applied. Currently, the commercialized thermoelectric devices on the market usually adopt a hard bulk device structure. Compared with traditional bulk thermoelectric devices, thin-film thermoelectric devices have wider application potential and irreplaceability in application. The main feature of thin-film thermoelectric devices is that they are close to chips in geometric dimensions, and because their thickness can usually reach the micron level, the stress on the upper and lower surfaces is greatly reduced, and they have the possibility of flexibility. Because their size is comparable to that of chips, thin-film thermoelectric devices can be compatible with other microelectronic devices, whether as micro-refrigerators or temperature difference generators. At the same time, because they are easy to achieve flexible preparation, they also have high application potential in the fields of human body sensing and body temperature power generation.

[0003] In order to ensure the high precision of each part of the thermoelectric thin film device, the main preparation method of the out-of-plane thermoelectric thin film device is currently photolithography. Photolithography has become the most successful and widely used micro-machining technology to date, which can realize the patterning of complex microstructures. However, although photolithography has extremely high processing accuracy, the introduction of photoresist has greatly increased the integration cost, and photoresist cannot withstand high temperatures, resulting in the disadvantage of not being able to improve the performance of thermoelectric materials through high-temperature deposition, and it is also impossible to prepare high-performance thermoelectric arms, which will further affect the overall performance of the device. Therefore, it is necessary to develop a new method for preparing thermoelectric thin film power generation devices that can achieve high-density array integration, is compatible with high-temperature deposition, and has a simple preparation process, is easy to operate, and is low-cost. Summary of the invention

[0004] In order to solve the above problems, the present invention adopts a mask-assisted deposition process to carry out material integration of thermoelectric devices, and adopts a double-sided bonding method to prepare devices. The limitation of photoresist on the deposition temperature of thermoelectric materials is removed by magnetron sputtering deposition, and the device is prepared by a bonding process. The preparation process is simple, easy to operate and low in cost.

[0005] In order to solve the above problems, a high-density thermoelectric device and a preparation method thereof are provided below. The preparation method comprises the following steps:

[0006] S1. Provide a plurality of mask plates, namely a first mask plate, a second mask plate, a third mask plate and a fourth mask plate, and provide a first substrate and a second substrate;

[0007] S2, using the first mask plate to deposit a patterned lower electrode on the surface of the first substrate, and using the second mask plate to deposit a patterned upper electrode on the surface of the second substrate;

[0008] S3, using the third mask plate to sequentially deposit N-type thermoelectric arms and a first bonding layer on the first substrate surface after step S2; using the fourth mask plate to sequentially deposit P-type thermoelectric arms and a second bonding layer on the second substrate surface after step S2;

[0009] S4. Bonding the first bonding layer and the second bonding layer under pressure and at high temperature to obtain a high-density thermoelectric device.

[0010] The method avoids the limitation of the deposition temperature of the thermoelectric material by the photoresist through the mask-assisted deposition process and the double-sided bonding method, and can obtain high-performance thermoelectric materials through high-temperature deposition. With the help of high-precision masks, high-density array integration of thermoelectric materials can be achieved. The double-sided bonding process is simpler, more reliable, easier to operate and less costly.

[0011] In step S2, the first mask plate is used to sequentially deposit a first adhesion layer, a first transition layer and a lower electrode layer on the surface of the first substrate to form the patterned lower electrode; the second mask plate is used to sequentially deposit a second adhesion layer, a second transition layer and an upper electrode layer on the surface of the second substrate to form the patterned upper electrode; the first adhesion layer and the second adhesion layer are adhesion metal layers, the lower electrode layer and the upper electrode layer are conductive metal layers, and the first transition layer and the second transition layer are mixed metal layers of materials on both sides thereof. By designing a multi-film layer structure for the electrode, the adhesion layer and the transition layer can be used to effectively improve the adhesion between the electrode and the substrate, and the thermal expansion mismatch problem between the multi-layer films can also be adjusted by designing the intermediate transition layer, further ensuring the reliability of the combination between the electrode and the substrate.

[0012] In step S3, the first barrier layer, N-type thermoelectric material and the third barrier layer are sequentially deposited on the first substrate surface after step S2 using the third mask plate to form the N-type thermoelectric arm; the second barrier layer, P-type thermoelectric material and the fourth barrier layer are sequentially deposited on the second substrate surface after step S2 using the fourth mask plate to form the P-type thermoelectric arm; the first barrier layer and the third barrier layer are Ti barrier layers, the second barrier layer and the fourth barrier layer are Ni barrier layers, the N-type thermoelectric material is Bi2Te3, and the P-type thermoelectric material is Sb2Te3. Interface matching between electrodes and thermoelectric materials is also a core issue of thermoelectric devices. In order to prevent diffusion between electrode materials and thermoelectric materials and matching problems between metal electrodes and semiconductor thermoelectric materials in work function, Ti with a lower work function is used to connect with N-type Bi2Te3, and Ni with a higher work function is used to connect with P-type Sb2Te3. Here, Ti and Ni not only have matching in work function, but also can improve the interface bonding strength between Cu and thermoelectric materials.

[0013] In step S2, the first adhesion layer and the second adhesion layer are Ti adhesion layers, and the Ti adhesion layer is prepared by magnetron sputtering, and the process is: deposition temperature is 100-200°C, sputtering power is 20-40W, deposition pressure is 1-2Pa, and deposition time is 20-30 minutes; the first transition layer and the second transition layer are Ti / Cu transition layers, and the Ti / Cu transition layers are obtained by co-sputtering Ti and Cu, and the magnetron sputtering process is: deposition temperature is 100-200°C, Cu sputtering power is 20-40W, Ti sputtering power is 20-40W, deposition pressure is 1-2Pa, and deposition time is 5-15 minutes; the lower electrode layer and the upper electrode layer are Cu electrode layers, and the Cu electrode layers are prepared by magnetron sputtering, and the process is: deposition temperature is 100-200°C, sputtering power is 30-60W, deposition pressure is 1-2Pa, and deposition time is 10-20 hours.

[0014] Before depositing the Ti adhesion layer, a substrate bias is applied to the first substrate and the second substrate to bombard and clean the substrates. By applying the bias, the surface energy of the substrate is improved by bombardment of high-energy particles, and the adhesion performance of the film to the substrate is also enhanced.

[0015] In step S3, the Ti barrier layer is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 100-200°C, the sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 5-15 minutes; the Ni barrier layer is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 100-200°C, the sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 5-15 minutes; the N-type thermoelectric material is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 100-200°C, the sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 5-15 minutes. The temperature is 350-450°C, the deposition pressure is 1-3Pa, the deposition time is 5-7h, the Bi2Te3 sputtering power is 40-80W, and Te compensation sputtering is performed simultaneously to form Bi2Te3 material; the P-type thermoelectric material is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 350-450°C, the deposition pressure is 1-3Pa, the deposition time is 5-7h, the Sb2Te3 sputtering power is 40-80W, and Te compensation sputtering is performed simultaneously to form Sb2Te3 material.

[0016] The first bonding layer and the second bonding layer are SnIn bonding layers, and the SnIn bonding layers are obtained by co-sputtering Sn and In, and the magnetron sputtering process is: deposition temperature is 80-120°C, Sn sputtering power is 20-40W, In sputtering power is 20-40W, deposition pressure is 1-3Pa, and deposition time is 20-40 minutes. A layer of SnIn material is deposited on the upper and lower electrode surfaces by sputtering deposition, thereby converting the Cu-SnIn welding bonding into SnIn-SnIn welding, so as to improve the bonding processability.

[0017] In step S4, the pressurized high temperature bonding process is: heating temperature is 100-300°C, pressure is 300-700g, and heating time is 3-7 minutes.

[0018] A fifth mask plate and a sixth mask plate are also provided. In step S3, the fifth mask plate is used to replace the third mask plate to deposit the first bonding layer, and the sixth mask plate is used to replace the fourth mask plate to deposit the second bonding layer; the design size of the electrode unit of the first mask plate and the second mask plate, the design size of the thermoelectric arm unit of the third mask plate and the fourth mask plate, and the design size of the bonding unit of the fifth mask plate and the sixth mask plate are successively reduced. By using mask plates of different sizes to deposit solder, process factors such as short circuits between electrodes and height differences of thermoelectric arms are effectively avoided, so that the welding bonding performance of thin film devices is greatly improved.

[0019] A high-density thermoelectric device is prepared according to any of the above-mentioned methods for preparing a high-density thermoelectric device.

[0020] A high-density thermoelectric device comprises a first substrate, a patterned lower electrode, an N-type thermoelectric arm and a P-type thermoelectric arm, a patterned upper electrode and a second substrate;

[0021] The bottom of the second substrate is relatively arranged above the top of the first substrate;

[0022] The patterned lower electrode is arranged on the top of the first substrate, and the patterned lower electrode is composed of a first adhesion layer, a first transition layer and a lower electrode layer which are arranged on the first substrate in sequence;

[0023] The patterned upper electrode is arranged at the bottom of the second substrate, and the patterned upper electrode is composed of a second adhesion layer, a second transition layer and an upper electrode layer which are arranged on the second substrate in sequence;

[0024] The N-type thermoelectric arm is arranged on the patterned lower electrode, and the N-type thermoelectric arm is composed of a first barrier layer, an N-type thermoelectric material and a third barrier layer;

[0025] The P-type thermoelectric arm is arranged on the patterned upper electrode, and the P-type thermoelectric arm is composed of a second barrier layer, a P-type thermoelectric material and a fourth barrier layer;

[0026] A bonding layer is provided at the other end of the N-type thermoelectric arm and the P-type thermoelectric arm, the N-type thermoelectric arm and the patterned upper electrode are connected through the bonding layer, and the P-type thermoelectric arm and the patterned lower electrode are connected through the bonding layer.

[0027] The invention has the following beneficial effects: the invention forms an electrode layer and a thermoelectric arm structure on two substrates respectively through a mask-assisted deposition process and a double-sided bonding method, and then realizes a thermoelectric device consisting of a lower electrode, a P-type / N-type thermoelectric arm and an upper electrode through a bonding process; the invention realizes patterning of electrodes and thermoelectric materials through a mask-assisted magnetron sputtering process, and compared with the photolithography technology, avoids the limitation of the deposition temperature of the thermoelectric material by the photoresist, can obtain high-performance thermoelectric materials through high-temperature deposition, and can realize high-density array integration of thermoelectric materials with a high-precision mask; the formation of the final structure of the thermoelectric device is realized through the double-sided bonding process, and the process is simple and reliable, easy to operate and low in cost; through the study of the Cu thin film deposition mechanism and the design of the multilayer film structure, the interface bonding between the electrode and the substrate is effectively improved, and the performance of the thermoelectric device is improved; through the magnetron sputtering process, the traditional Cu-SnIn bonding is transformed into a homogeneous SnIn-SnIn bonding, the bonding effect is improved, and the internal resistance of the device is effectively reduced; and the bonding process is further optimized by designing the mask with different sizes. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the specific embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 A flow chart for preparing a thermoelectric device provided by the present invention.

[0030] Figure 2 The following are photos of the thermoelectric device provided by the present invention during its preparation process. (a) is the second substrate after the upper electrode and the P-type thermoelectric arm are deposited, and (b) is the first substrate after the lower electrode and the N-type thermoelectric arm are deposited.

[0031] Figure 3 The surface peeling morphology comparison diagram of the Cu thin film electrode deposited with and without bias after the thermal shock resistance test provided by the present invention. (a) shows the result without substrate bias, and (b) shows the result after applying substrate bias.

[0032] Figure 4 Schematic diagram of bonding defects of thermoelectric devices provided by the present invention.

[0033] Figure 5 A schematic diagram of the improved bonding process provided by the present invention.

[0034] Figure 6 The results of thermal shock tests on the Cu thin film electrode provided by the present invention.

[0035] Figure 7 These are the results of thermal shock tests on the Bi2Te3 thin film thermoelectric material provided by the present invention. DETAILED DESCRIPTION

[0036] The above and other technical contents, features and effects of the present invention will be clearly presented in the following detailed description of a preferred embodiment with reference to the drawings. The directional terms mentioned in the following embodiments, such as up, down, left, right, front or back, etc., are only referenced to the directions of the attached drawings. Therefore, the directional terms used are used to illustrate and not to limit the present invention.

[0037] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.

[0038] The steps in the following embodiments do not correspond one to one with the summary of the invention.

[0039] Embodiment 1

[0040] The present invention uses a mask-assisted deposition process and a double-sided bonding method to carry out material integration and device preparation, thereby obtaining an out-of-plane high-density thin-film thermoelectric device.

[0041] The preparation process of out-of-plane high-density thin-film thermoelectric devices is much more complicated than that of in-plane thin-film devices. The main reason is that the thermoelectric arm length of out-of-plane thin-film devices is short and prone to diffusion failure, the temperature difference of the device is difficult to establish, and the out-of-plane devices used for power generation require the overall internal resistance of the device to be small, and the interface requirements between the electrode and the thermoelectric material are more stringent. Therefore, in the device preparation process, the thicker the electrode thickness, the better, so as to ensure that the overall internal resistance of the device is low, ensure that the device does not generate a lot of internal consumption when working, and improve the output efficiency of the battery.

[0042] The performance of thin-film thermoelectric devices is heavily dependent on the design of their structure. Based on the structural optimization of the previous device, the present invention designs an out-of-plane high-density thin-film thermoelectric device. It is composed of a lower electrode, a P-type thermoelectric arm, an N-type thermoelectric arm and an upper electrode. In this thermoelectric device, there are 200 pairs of thermoelectric arms (thermoelectric arms are N-type thermoelectric material units or P-type thermoelectric material units), and each thermoelectric arm has a diameter of 500μm. The actual photo of the preparation process is shown in the figure below. Figure 2 shown.

[0043] like Figure 1 Shown is a flow chart for preparing a high-density thermoelectric device provided by an embodiment of the present invention.

[0044] refer to Figure 1 The present invention provides a high-density thermoelectric device and a method for preparing the same. It should be noted that the scheme provided in this embodiment is a preferred scheme, and not all the steps and processes used below are necessarily consistent with those mentioned in this embodiment. Some processes or steps can be modified or omitted. The preparation method of this embodiment includes the following steps:

[0045] Step 1: providing a plurality of mask plates, namely a first mask plate, a second mask plate, a third mask plate and a fourth mask plate.

[0046] In this embodiment, specific patterns are formed on different mask plates, which are used for deposition of different parts of the thermoelectric device. The mask plates used are obtained by laser cutting, made of 304 stainless steel, with a minimum accuracy of 50 μm line width, and a thickness of 0.1 mm. The lower the thickness of the mask plate, the more conducive it is to reducing the shadow effect in magnetron sputtering.

[0047] Specifically, the first mask plate is used to make the lower electrode of the thermoelectric device, the second mask plate is used to make the upper electrode of the thermoelectric device, the third mask plate is used to make the N-type thermoelectric arm of the thermoelectric device, and the fourth mask plate is used to make the P-type thermoelectric arm of the thermoelectric device.

[0048] Alignment marks are provided on the above-mentioned mask, which can be used for subsequent alignment requirements.

[0049] Step 2: Provide a first substrate and a second substrate and clean them.

[0050] In this embodiment, the first substrate and the second substrate used are aluminum nitride (AlN) substrates, and the surface roughness Ra value of the substrates is ≤ 0.5. It can be understood that in other embodiments, aluminum oxide, zirconium oxide or silicon oxide sheets or other high thermal conductivity insulators can also be used to implement the present invention. The present invention does not limit the material of the substrate.

[0051] Similarly, alignment marks corresponding to each mask plate are arranged on the substrate, that is, Figure 2 The cross standard and dot marks shown in the figure are also provided with corresponding positioning marks on the mask plate. The alignment marks of the substrate and the mask plate can be used for subsequent alignment needs, which can help determine the position of the mask plate and ensure that the pattern of the mask plate can be accurately transferred to the corresponding position of the substrate.

[0052] The first substrate and the second substrate are cleaned by ultrasonically treating the substrates with acetone, anhydrous ethanol and deionized water for 15 minutes respectively, and then drying them with dry nitrogen for later use. The purpose of cleaning is to remove dirt on the substrates, increase cleanliness, and thus improve the adhesion between the substrates and the electrodes. This step is not necessary and can be omitted in other embodiments.

[0053] Step 3: depositing an adhesion layer, a transition layer and an electrode layer on the surfaces of the first substrate and the second substrate in sequence to form a patterned electrode.

[0054] In this embodiment, the patterned electrode is composed of a three-layer structure of an adhesion layer, a transition layer and an electrode layer. In other embodiments, the patterned electrode can also be composed of an adhesion layer and an electrode layer, or only a single electrode layer. In this embodiment, the design of the three-layer film structure can achieve better performance, as described below.

[0055] The first mask plate is aligned with the first substrate and then bonded together. Through the magnetron sputtering process, the first mask plate is used to sequentially deposit on the surface of the first substrate to form a first adhesion layer, a first transition layer and a lower electrode layer, and a lower electrode is formed on the surface of the first substrate. Similarly, the second mask plate is aligned with the second substrate and then bonded together. Through the magnetron sputtering process, the second mask plate is used to sequentially deposit on the surface of the second substrate to form a second adhesion layer, a second transition layer and an upper electrode layer, and an upper electrode is formed on the surface of the second substrate. The mask plate must be aligned using an alignment system with a magnification of more than 150 times. During alignment, it is necessary to ensure that the upper and lower cross-shaped alignment marks on the mask plate are all aligned, otherwise, even a very small tilt angle will cause the device to be scrapped.

[0056] Although in this embodiment, the deposition process used is a magnetron sputtering process, it is only an example and does not limit the deposition process. In other embodiments, thermal evaporation, electroplating, physical vapor deposition and other processes can be used. The same is true for the following steps, and the subsequent description will not be repeated.

[0057] In this embodiment, Ti is used as the adhesion layer material. The first adhesion layer is deposited on the surface of the first substrate, the deposition temperature is controlled at 200°C, the Ti sputtering power is 30W, the deposition pressure is 1Pa, and the deposition time is controlled at 30 minutes; the second Ti adhesion layer is deposited on the surface of the second substrate, the deposition temperature is controlled at 200°C, the Ti sputtering power is 30W, the deposition pressure is 1Pa, and the deposition time is controlled at 30 minutes.

[0058] In other embodiments, Ti is used as the adhesion layer material, and when the first adhesion layer is deposited on the surface of the first substrate or the second adhesion layer is deposited on the surface of the second substrate, the deposition temperature is 100-200°C, the Ti sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 20-30 minutes. In other embodiments, other deposition methods such as thermal evaporation and electroplating can also be used to prepare the adhesion layer, and the material of the adhesion layer can also be selected according to needs, such as Cr adhesion layer, Ni adhesion layer and other adhesion metal layers.

[0059] In order to enhance the interface strength between the electrode layer and the adhesion layer, a transition layer can be prepared after the adhesion layer is deposited. In this embodiment, the Ti / Cu mixed layer is prepared by co-sputtering Ti and Cu, and the first transition layer and the second transition layer are obtained respectively. Here, the process of the first transition layer and the second transition layer is as follows: the sputtering power is 40W, the deposition pressure is 1Pa, the co-sputtering time is 10 minutes, and the deposition temperature is 200°C. In other embodiments, the process of the first transition layer and the second transition layer is as follows: the sputtering power of Ti and Cu is 20-40W, the deposition pressure is 1-2Pa, the co-sputtering time is 5-15 minutes, and the deposition temperature is 100-200°C.

[0060] In this embodiment, Cu is used as the electrode layer material, and the lower electrode layer and the upper electrode layer are prepared by magnetron sputtering process. The preparation process of the lower electrode layer and the upper electrode layer is: Cu sputtering power is 50W, deposition pressure is 1Pa, deposition time is 20 hours, and deposition temperature is 200℃. The internal resistance design of the thermoelectric device requires that the thickness of its electrode layer must be at least 25μm. Increasing the thickness can effectively reduce the resistance of the electrode layer. In this embodiment, the thickness of the lower electrode layer and the upper electrode layer are both greater than 50μm.

[0061] In other embodiments, the preparation process of the lower electrode layer and the upper electrode layer is as follows: the sputtering power is 30-60W, the deposition pressure is 1-2Pa, the deposition time is 10-20 hours, and the deposition temperature is 100-200°C. In other embodiments, due to the large thickness of the electrode layer, the magnetron sputtering method takes a long time, and thermal evaporation, electroplating and other methods can also be used to prepare thick film electrodes. In other embodiments, after the lower electrode layer and the upper electrode layer are prepared, gold spraying can be performed to prevent electrode oxidation.

[0062] In other embodiments, the material of the adhesion layer can be selected according to needs, such as adhesion metal layers such as Cr and Ni; the same is true for the electrode layer material, which is not limited to Cu, and conductive metal layers such as Ag and Au can also be used. As for the transition layer between the adhesion layer and the electrode layer, the selection can be changed according to the materials of the two layers. The transition layer can use a mixed metal layer of the two layers of materials, such as using a Ti / Cu mixed metal layer as a transition layer between the Ti adhesion layer and the Cu electrode layer, such as using a Ni / Cu mixed metal layer as a transition layer between the Ni adhesion layer and the Cu electrode layer.

[0063] In this embodiment, the structure of the thermoelectric device and the selection of each layer structure are carefully considered. In order to improve the adhesion between the electrode and the substrate, a certain substrate bias voltage can be applied before depositing the Ti adhesion layer to bombard and clean the substrate (this step can also be used when other materials are selected as the adhesion layer). The bombardment of high-energy particles can improve the surface energy of the substrate, and also enhance the adhesion between the film and the substrate, further improving the performance of the thermoelectric device. Figure 3 As shown in FIG. 1 , the surface peeling morphology of the Cu film deposited under the conditions of no bias and bias (-100V) after the thermal shock resistance test is compared, and it can be clearly seen that the substrate bias improves the adhesion between the electrode and the substrate. For this reason, in this embodiment, a certain substrate bias is applied before depositing the adhesion layer to bombard and clean the substrate.

[0064] In addition, for thermoelectric devices, the thermal expansion coefficient of the aluminum nitride substrate selected in this embodiment is relatively small compared to Cu, which is about 0.25 times that of Cu. Therefore, during the preparation and use of thermoelectric devices, cracks and peeling may occur due to the huge difference in thermal expansion coefficients between them. Therefore, it is necessary to design a reasonable intermediate transition layer to adjust the thermal expansion mismatch between the multilayer films. By reasonably introducing the Ti adhesion layer and the Ti / Cu transition layer, the mismatch between the aluminum nitride substrate and Cu is well solved. At the same time, the adhesion of Ti to the substrate is much higher than that of Cu. The subsequent 3M tape peeling test confirmed that the Cu film with the Ti adhesion layer and the Ti / Cu transition layer has a 5B anti-peeling performance, which is suitable as a high-reliability thermoelectric device.

[0065] The thermoelectric device of the present invention belongs to a multilayer film system. During the layer-by-layer deposition process, the surface wettability will affect the growth mode of the subsequent film and the strength of the interface. In the present invention, by controlling the deposition temperature and time of the Cu electrode, the change of its surface energy and the formation of the surface geometric structure are changed. By selecting a suitable deposition temperature and deposition time, the performance of the thermoelectric device is improved. In this embodiment, a deposition temperature of 200°C is used to obtain the minimum microstrain and surface free energy of the Cu film, and the deposition time is increased to 20 hours (sputtering power 50W), which can reduce the surface energy and microstrain of the Cu film, thereby well controlling the geometric structure and energy state of its surface.

[0066] Step 4: After step 3, a barrier layer, a thermoelectric material, a barrier layer and a bonding layer are sequentially deposited on the surfaces of the first substrate and the second substrate respectively.

[0067] In this embodiment, the thermoelectric arm is composed of a three-layer structure of a barrier layer, a thermoelectric material and a barrier layer. In other embodiments, the thermoelectric arm may also be composed of a barrier layer and a thermoelectric material, or only a thermoelectric material. In this embodiment, the design of the barrier layer, the thermoelectric material and the barrier layer can effectively prevent the mutual diffusion of the thermoelectric material and the electrode material, thereby achieving better performance.

[0068] The third mask plate is aligned and bonded with the first substrate after step 3, and the first barrier layer, N-type thermoelectric material, third barrier layer and first bonding layer are sequentially deposited on the surface of the first substrate using the third mask plate through a magnetron sputtering process. Similarly, the fourth mask plate is aligned and bonded with the second substrate after step 3, and the second barrier layer, P-type thermoelectric material, fourth barrier layer and second bonding layer are sequentially deposited on the surface of the second substrate using the fourth mask plate through a magnetron sputtering process. The alignment requirements are as described above.

[0069] In the present invention, Ni barrier layer and Ti barrier layer are respectively provided to prevent the diffusion behavior of the interface. Specifically, in the present embodiment, for the selected N-type thermoelectric material Bi2Te3, Ti with a smaller work function is used as the material of the corresponding first barrier layer, and for the selected P-type thermoelectric material Sb2Te3, Ni with a higher work function is used as the material of the corresponding second barrier layer, so as to avoid Schottky contact at the metal / semiconductor interface. Among them, the sputtering power of Ti and Ni is 30W, the deposition pressure is 1Pa, the deposition temperature is 200℃, and the deposition time is 10 minutes. In other embodiments, the process of the Ti barrier layer is: the deposition temperature is 100-200℃, the sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 5-15 minutes; the process of the Ni barrier layer is: the deposition temperature is 100-200℃, the sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 5-15 minutes.

[0070] The interface matching between the Cu electrode and the thermoelectric material is also a core issue in the battery stack. In addition to requiring matching of the thermal expansion coefficient, it is also necessary to prevent diffusion between the electrode material and the thermoelectric material. The thermoelectric material is very likely to diffuse with the Cu electrode during the deposition process, which will lead to device failure. In addition, the metal electrode and the semiconductor thermoelectric material must also have a matching problem in work function. When the metal electrode contacts the semiconductor, it will cause the bending of the energy band at the interface, and the change in electrical properties caused by the bending of the energy band will greatly affect the performance of the battery stack. When the metal electrode contacts the N-type semiconductor, if its work function is less than the semiconductor work function, electrons will flow from the metal to the semiconductor, forming a negative space charge region on the surface of the semiconductor. At the same time, this is also a high conductivity area, which will form an ohmic contact; similarly, for P-type thermoelectric materials, metals with work functions greater than semiconductor materials should be selected to form ohmic contacts. Otherwise, a rectifying contact will be formed, which will greatly hinder the transport of electrons. In the design of the electrical properties of thermoelectric devices, the design principle of the metal semiconductor interface is to obtain the most ideal ohmic contact possible to reduce the contact resistance. To this end, in this embodiment, Ti with a lower work function is used to connect with the N-type thermoelectric material Bi2Te3, and Ni with a higher work function is used to connect with the P-type thermoelectric material Sb2Te3. The role of Ti and Ni is not only to match the work function, but also to strongly promote the improvement of the interface bonding strength between the Cu electrode and the thermoelectric material.

[0071] In this embodiment, the selected N-type thermoelectric material is Bi2Te3 thermoelectric material, and the deposition temperature is 400°C. Considering factors such as film peeling failure, the deposition time is set to 6 hours, the sputtering power is 60W, and the deposition pressure is 2Pa; in addition, high-temperature deposition will cause the volatilization of the Te element. While depositing the Bi2Te3 thermoelectric material, a Te single target is also used for sputtering to compensate for the lost Te element. It can be understood that the deposition temperature, deposition time and deposition pressure of the Te single substance should be consistent with the parameters of the deposited thermoelectric material, that is, the deposition temperature is also 400°C, the deposition time is 6 hours, the deposition pressure is 2Pa, and the Te compensation sputtering power is 55W. Subsequent experimental results show that the composition of the obtained thermoelectric film is basically in the normal range (the atomic ratio of Bi2Te3 is 2:3). The actual picture after the deposition of the N-type thermoelectric material array is as follows. Figure 2 As shown in (b), the black dot material is the N-type thermoelectric material Bi2Te3.

[0072] In other embodiments, the deposition temperature of Bi2Te3 thermoelectric material is 350-450°C, the deposition time is 5-7 hours, the deposition power is 40-80W, and the deposition pressure is 1-3Pa; while the deposition temperature of Te is 350-450°C, the deposition time is 5-7 hours, the deposition pressure is 1-3Pa, and the Te compensation sputtering power is 50-60W. It can be understood that in each deposition, the deposition temperature, deposition time and deposition pressure of Te single substance should be the same as those of the deposition of Bi2Te3 thermoelectric material. The experimental results show that within the above parameter range, the composition of the obtained thermoelectric film is basically in the normal range (the atomic ratio of Bi2Te3 is 2:3), which can ensure the normal function of the thermoelectric device.

[0073] In this embodiment, the selected P-type thermoelectric material is Sb2Te3 thermoelectric material, the deposition temperature is 400°C, the deposition time is 6 hours, the deposition power is 60W, and the deposition pressure is 2Pa; similarly, high-temperature deposition will cause the volatilization of the Te element. While depositing the Sb2Te3 thermoelectric material, a Te single target is also used for sputtering to compensate for the lost Te element. It can be understood that the deposition temperature, deposition time, and deposition pressure of the Te single substance should be consistent with the parameters of the deposited thermoelectric material, that is, the deposition temperature is also 400°C, the deposition time is 6 hours, the deposition pressure is 2Pa, and the Te compensation sputtering power is 45W. Subsequent experimental results show that the composition of the obtained thermoelectric film is basically within the normal range (the atomic ratio of Sb2Te3 is 2:3). The actual picture after the deposition of the P-type thermoelectric material array is as follows: Figure 2 As shown in (a), the black dot material is the P-type thermoelectric material Sb2Te3.

[0074] In other embodiments, the deposition temperature of the Sb2Te3 thermoelectric material is 350-450°C, the deposition time is 5-7 hours, the deposition power is 40-80W, and the deposition pressure is 1-3Pa; while the deposition temperature of Te is 350-450°C, the deposition time is 5-7 hours, the deposition pressure is 1-3Pa, and the Te compensation sputtering power is 40-50W. It can be understood that in each deposition, the deposition temperature, deposition time and deposition pressure of the Te element should be the same as those of the Bi2Te3 thermoelectric material. The experimental results show that within the above parameter range, the composition of the obtained thermoelectric film is basically in the normal range (the atomic ratio of Sb2Te3 is 2:3), which can ensure the normal function of the thermoelectric device.

[0075] After the sputtering of the thermoelectric material is completed, a barrier layer is also sputtered to control the interface diffusion behavior of the metal / semiconductor. To this end, Ti is continuously deposited on the surface of the first substrate after the N-type thermoelectric material is deposited to form a third barrier layer, and Ti is continuously deposited on the surface of the second substrate after the P-type thermoelectric material is deposited to form a fourth barrier layer. The detailed process of depositing the Ti barrier layer and the Ni barrier layer is the same as that described above and will not be repeated here.

[0076] In this embodiment, in order to improve the bonding effect of the thermoelectric device, a first bonding layer and a second bonding layer are formed on the surface of the first substrate and the second substrate respectively by a magnetron sputtering process. A low melting point eutectic alloy SnIn alloy (eutectic temperature is about 150°C) is used as a material for forming the bonding layer. Specifically, the bonding layer is obtained by thin film deposition by co-sputtering of single Sn and In targets. The specific magnetron sputtering process is as follows: the sputtering power of the single Sn and In targets is 30W, the deposition temperature is 100°C, the deposition pressure is 2Pa, and the deposition time is 30 minutes. In other embodiments, the sputtering power of the single Sn and In targets is 20-40W, the deposition temperature is 80-120°C, the deposition pressure is 1-3Pa, and the deposition time is 20-40 minutes. In other embodiments, printing can also be used to print solder to form a bonding layer, such as printing by a template method.

[0077] Step 5: Bond the first substrate and the second substrate after step 4.

[0078] In this embodiment, the thermoelectric device is assembled by top-bottom bonding. After the device surface bonding layer is prepared, the first substrate surface and the second substrate surface after step 4 are aligned and heated for bonding. The heating temperature is 200°C, the heating time is 5 minutes, the pressure is 500g, and the bonding is completed and slowly cooled. At this point, the thermoelectric device of the present invention is completed.

[0079] In other embodiments, the heating temperature is 100-300° C., the heating time is 3-7 minutes, and the pressure is 300-700 g.

[0080] SnIn solder is a new type of lead-free low-melting solder with a eutectic temperature of 393K, which is used in low-temperature welding processes. The thin film device prepared by the present invention is used near room temperature, so SnIn with a lower melting point is selected for device bonding. According to the study of the wettability of the Cu electrode surface, the surface energy of the film with a longer deposition time is lower, which is not conducive to the welding of foreign solder. The wettability of the electrode surface can be changed in a variety of ways to improve the welding ability between the electrode / solder: one is to control the geometric morphology and surface energy of the Cu surface, such as changing the temperature or deposition speed at the last deposition, to increase its surface energy and increase the adhesion of foreign particles (i.e., to select a suitable Cu electrode deposition temperature and time); the second is to appropriately modify the Cu electrode surface. In this embodiment, a layer of easily welded solder is deposited on the Cu electrode surface by sputtering deposition.

[0081] In the traditional welding bonding process, the actual bonding interface is the contact surface between the Cu electrode and the SnIn solder, that is, the Cu-SnIn welding. In order to study the bonding process, the bonding welding experiments were carried out on the untreated Cu surface (that is, the welding of Cu film and SnIn film) and the surface modified Cu surface (that is, the welding of SnIn film and SnIn film).

[0082] First, the solderability of SnIn was tested, and the Cu film deposited for 5 hours was selected for relevant solderability experiments:

[0083] (1) SnIn material is deposited on the Cu film to obtain a SnIn film. The SnIn film was deposited by co-sputtering of a single Sn and In target, and a series of tests were conducted within the following parameter ranges: the sputtering power of the single Sn and In targets was 20-40W, the deposition temperature was 80-120°C, the sputtering pressure was 1-3Pa, and the deposition time was 20-40min;

[0084] (2) The prepared SnIn film was cut into long strips, and the Cu film and the SnIn film were pressure-heated and welded on a heating device. The test was conducted within the following parameter ranges: welding pressure was 300-700 g, welding temperature was 100-300° C., and heat preservation was 20-40 min. During the welding process, the resistance during welding was measured in real time;

[0085] (3) After welding unloading, it was found that the Cu film and the SnIn film were separated, indicating that the Cu film and the SnIn film could not be well welded together;

[0086] (4) The Cu film is surface treated and a layer of SnIn material is deposited thereon to obtain a SnIn film; then, the SnIn film is homogeneously welded with the SnIn film, and it is found that the two can be well welded together.

[0087] From the above analysis, it can be seen that the surface energy of the Cu electrode will become lower and lower with the increase of deposition time, so it is not conducive to the adhesion of the solder. In the traditional process, the bonding is Cu-SnIn welding. Through the above experiments, it is found that the solderability between the simple Cu electrode and the SnIn solder is very poor, which is not conducive to the bonding of the device. Therefore, it is necessary to modify the surface of the Cu film before welding. For this reason, the present method proposes to deposit SnIn film on the upper and lower Cu electrode surfaces, so that when the upper and lower devices are welded, the Cu-SnIn welding is converted to SnIn-SnIn welding, so as to improve the bonding processability. In this embodiment, after the deposition of the thermoelectric material is completed, the SnIn film is pre-deposited on the Cu surface to be welded for 30 minutes by a mask method to adjust the state and solderability of the Cu surface.

[0088] During the research, the internal resistance of the thermoelectric device after preparation was tested. It was found that before the pressure was unloaded, the internal resistance of the device was 16.5Ω, but after the pressure was unloaded, the internal resistance of the device increased to nearly 1000Ω. Preliminary analysis showed that the reason for the large internal resistance was that the thermoelectric arm was very short, and the flatness of the 200 pairs of thermoelectric arms during welding was very high. The thickness of the welding layer was thin, and the tolerance after welding could not meet the gap between the thermoelectric arm and the electrode. Figure 4 As shown in the figure, the brown part represents the electrode material, and the blue and red materials are thermoelectric materials. There may be two basic reasons for the high welding internal resistance: one is that the thickness of the thermoelectric arm is uneven, and there is a poor contact phenomenon during the bonding process; the other may be due to the low surface energy and poor wettability of the Cu film, which makes the molten solder unable to weld it well. Therefore, the bonding process can be further improved.

[0089] In order to solve the contact problem during welding, the present invention proposes two process solutions. First, the solder is deposited on the surface of the Cu film for processing. By sputtering a thicker solder on the surface of the Cu film, the tolerance between the thermoelectric material and the Cu electrode after welding is increased; second, Figure 5 As shown in Figure 1, using masks of different sizes to deposit solder can effectively avoid process factors such as short circuits between electrodes and height differences between thermoelectric arms. Figure 5 As shown, the design size of the Cu electrode can be slightly larger ( Figure 5 The brown part in the middle), and then the thermoelectric arm with slightly smaller design size is deposited on it ( Figure 5 The middle blue part is the N-type thermoelectric material or the P-type thermoelectric material), and finally the solder with a smaller design size is deposited ( Figure 5The black part in the figure is the SnIn material. Of course, when using screen printing for bonding, you can also refer to this method to design components of different sizes.

[0090] Based on the second improved process, in other embodiments, a fifth mask plate and a sixth mask plate are further provided. The first mask plate and the second mask plate are changed to form the lower electrode and the upper electrode, the third mask plate and the fourth mask plate are respectively used to form the N-type thermoelectric arm and the P-type thermoelectric arm, and the fifth mask plate and the sixth mask plate are respectively used to form the first bonding layer and the second bonding layer. Figure 5 As shown in the figure, the design size of the Cu electrode unit of the first mask plate and the second mask plate is slightly larger, the design size of the thermoelectric arm unit of the third mask plate and the fourth mask plate is slightly smaller than the corresponding Cu electrode unit, and the design size of the bonding unit of the fifth mask plate and the sixth mask plate is smaller than the design size of the thermoelectric arm unit. By using mask plates of different sizes to deposit solder, process factors such as short circuits between electrodes and height differences of thermoelectric arms can be effectively avoided.

[0091] The improved welding process can weld the upper and lower device plates together very well. In the embodiment, the designed internal resistance of the 200 pairs of thin-film thermoelectric devices prepared is 0.96Ω. Due to the difference in process, the internal resistance of the devices after welding is in the range of 1.05-3.0Ω. This result shows the importance of surface modification for the welding of thin-film devices. Through certain process design and surface treatment, the weldability of thin-film devices is greatly improved.

[0092] The reliability of device electrodes has a significant impact on the performance and life of the device. In order to obtain long-term stable thermoelectric thin film devices, through substrate cleaning, substrate bias bombardment, adhesion layer design, and optimization of deposition temperature and time, a highly conductive and reliable patterned thin film electrode was prepared using a mask method. The thermal stability of the patterned copper thin film was verified by conducting a thermal shock test on the patterned copper thin film electrode. Figure 6 As shown in the figure, the patterned Cu electrode material was subjected to 2000 thermal shock tests in the atmosphere, with the shock temperature ranging from -40 to 150°C, and the cold and hot end temperatures were kept for 3 minutes. During the experiment, the DMM-6500 multimeter was used to test the change in resistance before and after the thermal shock every 400 cycles. After 2000 thermal shock cycles, the resistance change rate was 4.82%. It can be seen that the copper film electrode has high thermal stability.

[0093] In order to explore the performance reliability of thin-film thermoelectric materials during service, a hot and cold shock experiment was designed in atmospheric atmosphere. The experiment first used magnetron sputtering technology to prepare Bi2Te3 thin-film thermoelectric materials on AlN substrates, and then placed the thermoelectric film in a hot and cold shock test chamber for hot and cold shock experiments in atmospheric environment. The shock temperature was -40 to 150°C, and the hot and cold end temperatures were kept for 3 minutes. After every 400 temperature cycles, the DMM-6500 multimeter was used to test the change in resistance of the material before and after the hot and cold shocks. The experimental results obtained Figure 7 As shown in the figure, after 2000 cycles, the resistance change rate of the Bi2Te3 thermoelectric film is only 1.38%. It can be seen that the Bi2Te3 thermoelectric film material has good thermal stability when subjected to thermal shock in the atmosphere.

[0094] A high-density thermoelectric device is prepared according to the above-mentioned method for preparing a high-density thermoelectric device.

[0095] A high-density thermoelectric device comprises a first substrate, a patterned lower electrode, an N-type thermoelectric arm and a P-type thermoelectric arm, a patterned upper electrode and a second substrate;

[0096] The bottom of the second substrate is relatively arranged above the top of the first substrate;

[0097] The patterned lower electrode is arranged on the top of the first substrate, and the patterned lower electrode is composed of a first adhesion layer, a first transition layer and a lower electrode layer which are arranged on the first substrate in sequence;

[0098] The patterned upper electrode is arranged at the bottom of the second substrate, and the patterned upper electrode is composed of a second adhesion layer, a second transition layer and an upper electrode layer which are arranged in sequence on the second substrate;

[0099] The N-type thermoelectric arm is arranged on the patterned lower electrode, and the N-type thermoelectric arm is composed of a first barrier layer, an N-type thermoelectric material and a third barrier layer;

[0100] The P-type thermoelectric arm is arranged on the patterned upper electrode, and the P-type thermoelectric arm is composed of a second barrier layer, a P-type thermoelectric material and a fourth barrier layer;

[0101] A bonding layer is provided at the other end of the N-type thermoelectric arm and the P-type thermoelectric arm, the N-type thermoelectric arm and the patterned upper electrode are connected through the bonding layer, and the P-type thermoelectric arm and the patterned lower electrode are connected through the bonding layer.

[0102] In order to facilitate the description, some common English nouns or letters used in the present invention are only used for exemplary reference rather than restrictive interpretation or specific usage, and the protection scope of the present invention should not be limited by their possible Chinese translations or specific letters.

[0103] It should also be noted that, in this document, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations.

Claims

1. A method for preparing a high-density thermoelectric device, characterized in that: The steps include: S1. Provide a plurality of mask plates, namely a first mask plate, a second mask plate, a third mask plate and a fourth mask plate, and provide a first substrate and a second substrate; S2, using the first mask plate to deposit a patterned lower electrode on the surface of the first substrate, and using the second mask plate to deposit a patterned upper electrode on the surface of the second substrate; S3, using the third mask plate to sequentially deposit N-type thermoelectric arms and a first bonding layer on the first substrate surface after step S2; using the fourth mask plate to sequentially deposit P-type thermoelectric arms and a second bonding layer on the second substrate surface after step S2; S4. Bonding the first bonding layer and the second bonding layer under pressure and at high temperature to obtain a high-density thermoelectric device.

2. The method for preparing a high-density thermoelectric device according to claim 1, characterized in that: In step S2, a first adhesion layer, a first transition layer and a lower electrode layer are sequentially deposited on the surface of the first substrate using the first mask plate to form the patterned lower electrode; Using the second mask plate, sequentially depositing a second adhesion layer, a second transition layer and an upper electrode layer on the surface of the second substrate to form the patterned upper electrode; The first adhesion layer and the second adhesion layer are adhesive metal layers, the lower electrode layer and the upper electrode layer are conductive metal layers, and the first transition layer and the second transition layer are mixed metal layers of materials on both sides thereof.

3. The method for preparing a high-density thermoelectric device according to claim 1, characterized in that: In step S3, a first barrier layer, an N-type thermoelectric material and a third barrier layer are sequentially deposited on the surface of the first substrate after step S2 using the third mask to form the N-type thermoelectric arm; Using the fourth mask plate, sequentially depositing a second barrier layer, a P-type thermoelectric material and a fourth barrier layer on the surface of the second substrate after step S2 to form the P-type thermoelectric arm; The first barrier layer and the third barrier layer are Ti barrier layers, the second barrier layer and the fourth barrier layer are Ni barrier layers, the N-type thermoelectric material is Bi2Te3, and the P-type thermoelectric material is Sb2Te3.

4. The method for preparing a high-density thermoelectric device according to claim 2, characterized in that: In step S2, the first adhesion layer and the second adhesion layer are Ti adhesion layers, and the Ti adhesion layer is prepared by magnetron sputtering, and the process is: deposition temperature is 100-200° C., sputtering power is 20-40 W, deposition pressure is 1-2 Pa, and deposition time is 20-30 minutes; The first transition layer and the second transition layer are Ti / Cu transition layers, and the Ti / Cu transition layers are obtained by co-sputtering Ti and Cu, and the magnetron sputtering process is: deposition temperature is 100-200°C, Cu sputtering power is 20-40W, Ti sputtering power is 20-40W, deposition pressure is 1-2Pa, and deposition time is 5-15 minutes; The lower electrode layer and the upper electrode layer are Cu electrode layers, and the Cu electrode layers are prepared by magnetron sputtering, and the process is: deposition temperature is 100-200° C., sputtering power is 30-60W, deposition pressure is 1-2Pa, and deposition time is 10-20 hours.

5. The method for preparing a high-density thermoelectric device according to claim 4, characterized in that: Before depositing the Ti adhesion layer, a substrate bias is applied to the first substrate and the second substrate to bombard and clean the substrates.

6. The method for preparing a high-density thermoelectric device according to claim 3, characterized in that: In step S3, the Ti barrier layer is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 100-200°C, the sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 5-15 minutes; The Ni barrier layer is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 100-200°C, the sputtering power is 20-40W, the deposition pressure is 1-2Pa, and the deposition time is 5-15 minutes; The N-type thermoelectric material is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 350-450°C, the deposition pressure is 1-3Pa, the deposition time is 5-7h, the Bi2Te3 sputtering power is 40-80W, and Te compensation sputtering is performed simultaneously to form Bi2Te3 material; The P-type thermoelectric material is prepared by magnetron sputtering, and the process is as follows: the deposition temperature is 350-450°C, the deposition pressure is 1-3Pa, the deposition time is 5-7h, the Sb2Te3 sputtering power is 40-80W, and Te compensation sputtering is performed simultaneously to form Sb2Te3 material.

7. The method for preparing a high-density thermoelectric device according to claim 3, characterized in that: The first bonding layer and the second bonding layer are SnIn bonding layers, and the SnIn bonding layers are obtained by co-sputtering Sn and In, and the magnetron sputtering process is: deposition temperature is 80-120°C, Sn sputtering power is 20-40W, In sputtering power is 20-40W, deposition pressure is 1-3Pa, and deposition time is 20-40 minutes.

8. The method for preparing a high-density thermoelectric device according to claim 7, characterized in that: In step S4, the pressurized high temperature bonding process is: heating temperature is 100-300°C, pressure is 300-700g, and heating time is 3-7 minutes.

9. The method for preparing a high-density thermoelectric device according to claim 1, characterized in that: A fifth mask plate and a sixth mask plate are also provided. In step S3, the fifth mask plate is used to replace the third mask plate to deposit the first bonding layer, and the sixth mask plate is used to replace the fourth mask plate to deposit the second bonding layer; the design dimensions of the electrode units of the first mask plate and the second mask plate, the design dimensions of the thermoelectric arm units of the third mask plate and the fourth mask plate, and the design dimensions of the bonding units of the fifth mask plate and the sixth mask plate are reduced in sequence.

10. A high-density thermoelectric device, prepared according to the method for preparing a high-density thermoelectric device according to any one of claims 1 to 9.

11. A high-density thermoelectric device, characterized in that: It includes a first substrate, a patterned lower electrode, an N-type thermoelectric arm and a P-type thermoelectric arm, a patterned upper electrode and a second substrate; The bottom of the second substrate is relatively arranged above the top of the first substrate; The patterned lower electrode is arranged on the top of the first substrate, and the patterned lower electrode is composed of a first adhesion layer, a first transition layer and a lower electrode layer which are arranged on the first substrate in sequence; The patterned upper electrode is arranged at the bottom of the second substrate, and the patterned upper electrode is composed of a second adhesion layer, a second transition layer and an upper electrode layer which are arranged in sequence on the second substrate; The N-type thermoelectric arm is arranged on the patterned lower electrode, and the N-type thermoelectric arm is composed of a first barrier layer, an N-type thermoelectric material and a third barrier layer; The P-type thermoelectric arm is arranged on the patterned upper electrode, and the P-type thermoelectric arm is composed of a second barrier layer, a P-type thermoelectric material and a fourth barrier layer; A bonding layer is provided at the other end of the N-type thermoelectric arm and the P-type thermoelectric arm, the N-type thermoelectric arm and the patterned upper electrode are connected through the bonding layer, and the P-type thermoelectric arm and the patterned lower electrode are connected through the bonding layer.