Modified polyester elastomer and method for producing same

Through the titanium content control and structural design of the modified polyester elastomer, the problem of decomposition and deterioration of existing gas barrier materials at high temperatures is solved, excellent color tone and heat-resistant adhesion are achieved, and it is suitable for a variety of packaging and Industrial use.

CN118749005APending Publication Date: 2024-10-08MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022719.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-21
Filing Date
2023-03-10
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing gas barrier materials are prone to decomposition and deterioration in high-temperature environments, resulting in peeling of the interface between the adhesive layer and the gas barrier layer, and lack excellent color tone and heat-resistant adhesion.

Method used

By modifying a modified polyester elastomer with a titanium content of less than 250 wtppm and a polyester-polyether block copolymer composed of an aromatic polyester hard segment and a polyalkylene ether glycol soft segment, the unsaturated Carboxylic acid or its derivatives are modified to prepare a modified polyester elastomer with excellent color tone and heat-resistant adhesion, and are used in combination with polar polymers.

Benefits of technology

It achieves heat-resistant adhesion without interfacial peeling in high-temperature environments, and provides excellent color tone and transparency, making it suitable for food packaging and industrial uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001263140000261
    Figure BDA0005001263140000261
  • Figure BDA0005001263140000291
    Figure BDA0005001263140000291
  • Figure BDA0005001263140000321
    Figure BDA0005001263140000321
Patent Text Reader

Abstract

A modified polyester elastomer obtained by modifying a polyester-polyether block copolymer, which is composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol, with an unsaturated carboxylic acid and / or a derivative thereof, the modified polyester elastomer containing titanium and having a titanium content of less than 250 wtppm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a modified polyester elastomer having excellent color tone and heat-resistant adhesiveness and a method for producing the same.

[0002] The present invention also relates to a laminate, a modifier and a polar polymer composition obtained by using the modified polyester elastomer. Background Art

[0003] Laminated bodies containing gas barrier materials represented by polyamide and ethylene-vinyl alcohol copolymers are used in containers such as films, bottles, and cups in the field of food packaging due to their excellent mechanical properties, safety in food applications, and gas barrier properties such as water vapor and oxygen. In addition, in the non-food field, they are widely used in industrial piping, hoses, beverage and drug delivery pipes, and automotive parts. Furthermore, in order to impart functions such as aroma preservation, rigidity, heat resistance, cold resistance, and surface printability, there is a well-known technology of laminating gas barrier materials with ester polymers.

[0004] Since polyamide and ethylene-vinyl alcohol copolymers have poor adhesiveness with ester polymers, there is known a technique for providing an adhesive layer composed of an adhesive polymer composition in order to laminate them.

[0005] For example, Patent Document 1 describes an adhesive polymer composition composed of a modified polyester elastomer, wherein the modified polyester elastomer is obtained by modifying a saturated polyester thermoplastic elastomer having a polyalkylene ether glycol segment content of 58 to 73% by weight using an unsaturated carboxylic acid or a derivative thereof in the presence of a free radical generator.

[0006] In addition, polar polymers such as polyamide and ethylene-vinyl alcohol copolymer used as gas barrier materials lack flexibility, especially poor impact resistance. In order to solve this problem, for example, attempts have been made to add modified polyester elastomers to polar polymers to impart moderate flexibility and impact resistance while having high gas barrier properties. (Patent Document 2)

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2002-155135

[0010] Patent Document 2: Japanese Patent Application Publication No. 2004-2791 Summary of the invention

[0011] In the field of food packaging, which often requires good color tone and transparency, an adhesive polymer composition with excellent color tone is desired to avoid damage to the appearance and internal visibility of the laminate due to the color tone of the adhesive polymer composition or discoloration caused by heat during molding.

[0012] In the non-food field such as industrial piping and automobile parts, for applications exposed to high temperature environments, the adhesive layer may decompose and deteriorate due to heat, and peeling may occur at the interface between the adhesive layer and the polyamide or ethylene-vinyl alcohol copolymer layer as a gas barrier layer. Therefore, an adhesive polymer composition in which decomposition and degradation caused by heat are suppressed is desired.

[0013] Under such circumstances, an adhesive polymer composition having excellent color tone and heat-resistant adhesiveness has been desired.

[0014] However, the adhesive polymer composition described in Patent Document 1 is excellent in initial adhesiveness as shown in Comparative Example 1-1 described later, but has room for improvement in heat-resistant adhesiveness and is also inferior in color tone.

[0015] Furthermore, according to the research of the present inventors, the modified polyester elastomer described in Patent Document 2 has excellent modification effect, that is, flexibility of the polar polymer as shown in Comparative Examples 1-2 and 3 described below, but has room for improvement in color.

[0016] Although the titanium content of the modified polyester elastomer is not described in Patent Documents 1 and 2, at the time of filing Patent Documents 1 and 2, in order to produce the modified polyester elastomer, the elastomer produced on an industrial level as the polyester-based thermoplastic elastomer to be modified used only a titanium catalyst, and the titanium content thereof was 250 wtppm or more, which is equivalent to Comparative Examples 1-1 to 3 described later. Therefore, the titanium content of the modified polyester elastomer obtained by modifying such a polyester-based thermoplastic elastomer was also 250 wtppm or more.

[0017] An object of the present invention is to provide a modified polyester elastomer having excellent color tone and heat-resistant adhesiveness, a method for producing the same, and a laminate using the modified polyester elastomer.

[0018] The present invention also aims to provide a modifier and a polar polymer composition comprising the modified polyester elastomer.

[0019] The present inventors have repeatedly conducted studies to solve the above-mentioned problems and have found that by reducing the titanium content of the modified polyester elastomer to below a specified value, a modified polyester elastomer having excellent color tone and heat-resistant adhesion can be obtained, and that the modified polyester elastomer is effective as a modifier for polar polymers such as ethylene-vinyl alcohol copolymers and polyamide polymers, thereby completing the present invention.

[0020] That is, the gist of the present invention is as follows.

[0021] [1] A modified polyester elastomer, wherein a polyester polyether block copolymer composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol is modified with an unsaturated carboxylic acid and / or its derivatives, wherein the modified polyester elastomer contains titanium, and the titanium content is less than 250 wtppm.

[0022] [2] The modified polyester elastomer according to [1], wherein the content of the polyalkylene ether glycol segment in the polyester polyether block copolymer is 5 to 90% by mass.

[0023] [3] The modified polyester elastomer according to [1] or [2], wherein the MFR (based on JIS K7210, 230° C., 2.16 kg load) of the modified polyester elastomer is 1 to 300 g / 10 min.

[0024] [4] The modified polyester elastomer according to any one of [1] to [3], wherein the density of the modified polyester elastomer (based on JIS K7112) is 1.00 to 1.35 g / cm 3 .

[0025] [5] The modified polyester elastomer according to any one of [1] to [4], wherein the melting point of the modified polyester elastomer is 145 to 245°C.

[0026] [6] The modified polyester elastomer according to any one of [1] to [5], wherein the modified polyester elastomer has a JIS-D hardness (based on JIS K6253) of 10 to 80.

[0027] [7] The modified polyester elastomer according to any one of [1] to [6], wherein the titanium content of the modified polyester elastomer is 20 wtppm or more.

[0028] [8] The modified polyester elastomer according to [7], wherein the titanium content of the modified polyester elastomer is 20 wtppm to 248 wtppm.

[0029] [9] A laminate comprising: a substrate layer, a layer comprising the modified polyester elastomer according to any one of [1] to [8] or an adhesive polymer composition containing the modified polyester elastomer, and a resin layer.

[0030]

[10] A method for producing a modified polyester elastomer, comprising the steps of: modifying a polyester elastomer obtained by polymerization in the presence of a titanium compound with an unsaturated carboxylic acid and / or a derivative thereof;

[0031] The polyester elastomer is a polyester polyether block copolymer composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol.

[0032] The polyester elastomer has a titanium content of less than 250 wtppm.

[0033]

[11] The method for producing a modified polyester elastomer according to

[10] , wherein the content of the polyalkylene ether glycol segment in the polyester polyether block copolymer is 5 to 90% by mass.

[0034]

[12] The method for producing a modified polyester elastomer according to

[10] or

[11] , wherein the acid value of the modified polyester elastomer is 32 eq / T or less.

[0035]

[13] The method for producing a modified polyester elastomer according to any one of

[10] to

[12] , wherein the modification treatment is performed in the presence of a radical generator.

[0036]

[14] The method for producing a modified polyester elastomer according to

[13] , wherein the free radical generator is contained in an amount of 0.001 to 5 parts by mass based on 100 parts by mass of the polyester elastomer.

[0037]

[15] The method for producing a modified polyester elastomer according to any one of

[10] to

[14] , wherein the modification treatment is performed by a melt-kneading reaction.

[0038]

[16] A modifier comprising the modified polyester elastomer according to any one of [1] to [8].

[0039]

[17] A polar polymer composition, comprising a polar polymer and the modified polyester elastomer according to claim 1 or 2, wherein the content of the polar polymer is 70 to 99% by weight, and the content of the modified polyester elastomer is 1 to 30% by weight relative to the total of the polar polymer and the modified polyester elastomer, and the polar polymer comprises at least one selected from ethylene-vinyl alcohol copolymers and polyamide polymers.

[0040] The modified polyester elastomer of the present invention has excellent color tone and heat-resistant adhesiveness. Therefore, by using the modified polyester elastomer in the adhesive layer between the ester polymer layer and the gas barrier layer, a laminate having excellent color tone and transparency can be provided in the field of food packaging. In addition, in the field of non-food such as industrial piping and automobile parts, a laminate having excellent heat-resistant adhesiveness and no interface peeling problem can be provided.

[0041] The modified polyester elastomer of the present invention is also effective as a modifier for imparting properties such as flexibility to polar polymers such as ethylene-vinyl alcohol copolymers and polyamide polymers.

[0042] Therefore, a polar polymer composition is provided, wherein the polar polymer is modified in physical properties such as flexibility by using the polar polymer composition comprising the modified polyester elastomer of the present invention and a polar polymer. DETAILED DESCRIPTION

[0043] The present invention will be described in detail below. The following description is an example of an embodiment of the present invention, and the present invention is not limited to the following description unless it exceeds the gist of the present invention, and can be implemented with any modifications within the scope of the gist of the present invention.

[0044] In the present invention, when "to" is used and a numerical value or a physical property value is inserted before and after it, it is used as meaning including the values ​​before and after it.

[0045] In the present invention, the density, melting point, hardness and melt flow rate (MFR) of the polyester elastomer and the modified polyester elastomer are values ​​measured as follows.

[0046] <Density>

[0047] The density was measured by the water displacement method in accordance with JIS K7112.

[0048] <Melting point>

[0049] The melting point is measured using a differential scanning calorimeter (DSC). Specifically, the temperature is temporarily raised to 300°C to eliminate the thermal history, then the temperature is lowered to 40°C at a cooling rate of 10°C / min, and the temperature is again raised at a heating rate of 10°C / min for measurement, and the temperature at the top of the endothermic peak at this time is taken as the melting point. The unit is °C.

[0050] <Hardness>

[0051] The hardness is JIS-D hardness measured by a durometer in accordance with JIS K6253 (D hardness).

[0052] <MFR>

[0053] The MFR (melt flow rate) of the polyester elastomer and modified polyester elastomer described below is measured under the conditions of a temperature of 230° C., a load of 2.16 kg, and 10 minutes in accordance with JIS K7210. During the measurement, the polyester elastomer and modified polyester elastomer are vacuum dried at 100° C. for 4 hours in a pellet state to remove the contained moisture.

[0054] The modified polyester elastomer of the present invention is characterized in that it is a modified polyester elastomer obtained by modifying a polyester polyether block copolymer composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol using an unsaturated carboxylic acid and / or its derivatives, and the modified polyester elastomer contains titanium, and the titanium content of the modified polyester elastomer is less than 250wtppm.

[0055] Hereinafter, the polyester polyether block copolymer used for producing the modified polyester elastomer of the present invention by modification may be referred to as "polyester elastomer", "raw material polyester elastomer" or "component (A)".

[0056] In addition, the unsaturated carboxylic acid and / or its derivative used for modification of the polyester elastomer may be referred to as "component (B)", and the radical generator used for modification treatment may be referred to as "component (C)".

[0057] The modification in the present invention refers to the grafting modification of the polyester elastomer using unsaturated carboxylic acid and / or its derivatives, modification using terminal modification and transesterification reaction, modification using decomposition reaction, etc. Specifically, as the site to which the unsaturated carboxylic acid and / or its derivatives are bonded, terminal functional groups and alkyl chain parts are considered, and in particular, carbon atoms at the α-position and β-position relative to the terminal carboxyl group, terminal hydroxyl group and ether bond of the polyalkylene ether glycol segment can be cited. It is estimated that the unsaturated carboxylic acid and / or its derivatives are particularly often bonded at the α-position relative to the ether bond of the polyalkylene ether glycol segment.

[0058] When a polyester elastomer is modified with an unsaturated carboxylic acid and / or its derivatives, a modified polyester elastomer is generally obtained as a composition, the composition comprising the modified polyester elastomer modified with the polyester elastomer, and an unmodified polyester elastomer, the unsaturated carboxylic acid and / or its derivatives used in the modification, a free radical generator described below, etc. The modified polyester elastomer of the present invention refers to a modified polyester elastomer composition obtained by such a modification reaction and comprising residues such as an unmodified polyester elastomer and an unsaturated carboxylic acid and / or its derivatives.

[0059] As the modified polyester elastomer of the present invention, as long as it contains a polyester elastomer satisfying the titanium content specified in the present invention, preferably the content of the polyalkylene ether glycol segment further described below, and more preferably the appropriate acid value further described below, a mixture of a modified polyester elastomer obtained by modifying the polyester elastomer and an unmodified polyester elastomer may also be used.

[0060] [mechanism]

[0061] The modified polyester elastomer of the present invention has high compatibility with ester polymers because polyester is the main skeleton. In addition, the modified polyester elastomer can make the adhesion with gas barrier materials, especially polyamide polymers and ethylene-vinyl alcohol copolymers sufficient, and further, through the elastomer structure composed of hard segments (aromatic polyesters) and soft segments (polyalkylene ether glycol), the strain and residual stress generated between the layers of the laminate (between the gas barrier layer and the adhesive layer) during molding are alleviated, thereby making the adhesion strong.

[0062] The titanium content of the modified polyester elastomer of the present invention is below a prescribed value. In order to produce such a modified polyester elastomer, a polyester elastomer having a titanium content below a prescribed value is usually used as a raw material polyester elastomer for modification. Thus, by using a polyester elastomer having an active titanium content below a prescribed value, hydrolysis during modification can be suppressed, and a modified polyester elastomer having excellent color tone and heat-resistant adhesiveness can be obtained.

[0063] If the modified polyester-based elastomer has a titanium content of a predetermined value or less, hydrolysis during molding and processing is suppressed, and the color tone and heat-resistant adhesiveness can be maintained.

[0064] In addition, since the modified polyester elastomer of the present invention has excellent compatibility with ethylene-vinyl alcohol copolymers and polyamide polymers as polar polymers, when the modified polyester elastomer of the present invention is mixed with these polar polymers to prepare a polar polymer composition, the modified polyester elastomer and the polar polymer can be fully compatible. By reducing the dispersed particles of the modified polyester elastomer in the polar polymer composition, the effect of improving properties such as flexibility is achieved.

[0065] Therefore, the modified polyester elastomer of the present invention is also useful as a modifier for such polar polymers. Furthermore, by mixing the modified polyester elastomer of the present invention with a polar polymer, a polar polymer composition having excellent properties such as color tone and flexibility can be obtained.

[0066] Such a modified polyester elastomer of the present invention can be industrially advantageously produced by the method for producing a modified polyester elastomer of the present invention, which is characterized by comprising the steps of: modifying a polyester elastomer obtained by polymerization in the presence of a titanium compound with an unsaturated carboxylic acid and / or its derivative; the polyester elastomer is a polyester polyether block copolymer composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol, and the titanium content of the polyester elastomer is less than 250 wtppm. However, the method for producing the modified polyester elastomer of the present invention is not limited to the method for producing the modified polyester elastomer of the present invention.

[0067] Hereinafter, a method for producing the modified polyester elastomer of the present invention will be described, and then the modified polyester elastomer of the present invention will be described.

[0068] [Method for producing modified polyester elastomer]

[0069] [Polyester elastomer]

[0070] The raw material polyester elastomer used in the method for producing the modified polyester elastomer of the present invention is a polyester polyether block copolymer composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol.

[0071] Polyester elastomers can generally be obtained by polycondensing oligomers obtained by esterification or transesterification of i) aliphatic and / or alicyclic diols having 2 to 12 carbon atoms, ii) aromatic dicarboxylic acids and / or alkyl esters thereof, and iii) polyalkylene ether glycols having a number average molecular weight of 400 to 6000 as raw materials in the presence of a titanium compound.

[0072] As i) aliphatic and / or alicyclic diols having 2 to 12 carbon atoms, aliphatic and / or alicyclic diols commonly used as raw materials for ester polymers, particularly raw materials for polyester elastomers, can be used. For example, ethylene glycol, propylene glycol, trimethylene glycol, 1,4-butanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol can be mentioned, among which 1,4-butanediol and ethylene glycol are preferred, and 1,4-butanediol is particularly preferred. These diols can be used alone or as a mixture of two or more.

[0073] As ii) aromatic dicarboxylic acid, aromatic dicarboxylic acids generally used as raw materials for ester polymers, especially raw materials for polyester elastomers, can be used. For example, terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid can be mentioned. Among these, terephthalic acid and 2,6-naphthalenedicarboxylic acid are preferred, and terephthalic acid is particularly preferred. These dicarboxylic acids can also be used in combination of two or more. When using alkyl esters of aromatic dicarboxylic acids, dimethyl esters, diethyl esters, etc. of the above dicarboxylic acids can be used. Dimethyl terephthalate and 2,6-dimethyl naphthalene dicarboxylate are preferred.

[0074] Examples of the polyalkylene ether glycol iii) include polyethylene glycol, poly(1,2- and 1,3-propylene ether) glycol, poly(tetramethylene ether) glycol, poly(hexamethylene ether) glycol, and poly(decamethylene ether) glycol. Among these, poly(tetramethylene ether) glycol is particularly preferably used.

[0075] As the polyalkylene ether glycol, a polyalkylene ether glycol with a number average molecular weight of 400 to 6000 is generally used, preferably a polyalkylene ether glycol with a number average molecular weight of 600 to 4000, and more preferably a polyalkylene ether glycol with a number average molecular weight of 900 to 3000. When the number average molecular weight is at least the lower limit of the above range, there is a tendency that the degree of modification with unsaturated carboxylic acid and / or its derivatives is easily controlled to the desired range, and sufficient adhesion and the function as a modifier are easily exhibited. When the number average molecular weight is at most the upper limit of the above range, there is a tendency that the phase separation in the system can be suppressed, and the decrease in the physical properties of the obtained modified polyester-based elasticity can be suppressed.

[0076] Here, the "number average molecular weight" is measured by nuclear magnetic resonance (NMR) analysis.

[0077] As described later, the polyalkylene ether glycol is used in an amount of preferably 5 to 90% by mass, more preferably 10 to 85% by mass, and even more preferably 20 to 80% by mass in the polyester elastomer.

[0078] The polyester elastomer may be copolymerized with a small amount of trifunctional triol, tricarboxylic acid or esters thereof in addition to the above-mentioned components, and may further use an aliphatic dicarboxylic acid such as adipic acid or its dialkyl ester as a copolymerization component.

[0079] <Titanium content>

[0080] In the production of polyester elastomers, a titanium compound is sometimes used as a polymerization catalyst.

[0081] As titanium compounds, for example, potassium oxalate titanate, alkoxy or aryloxy titanate compounds, titanium carbonate compounds, halogenated titanium compounds, and titanium acetylacetonate can be cited. Among them, potassium oxalate titanate, alkoxy or aryloxy titanate compounds are preferred, and alkoxy or aryloxy titanate compounds are particularly preferred. Among the alkoxy or aryloxy titanate compounds, tetraalkyl titanate (tetraalkoxy titanium) or tetraaryl titanate (tetraaryloxy titanium) are preferred, and specifically, tetra-n-propyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, tetra-tert-butyl titanate, tetraphenyl titanate, tetracyclohexyl titanate, tetrabenzyl titanate, or mixtures thereof can be cited. Among these, tetra-n-propyl titanate, tetraisopropyl titanate, and tetra-n-butyl titanate are particularly preferred, and tetra-n-butyl titanate is most preferred. These titanium compounds can be used in combination of two or more.

[0082] In the production process of the polyester elastomer, titanium compounds remain in the obtained polyester elastomer due to the titanium compound used as a catalyst. The titanium (titanium atom) content of the raw material polyester elastomer used for modification in the present invention is less than 250 wtppm, preferably 245 wtppm or less, more preferably 240 wtppm or less, and further preferably 238 wtppm or less. The lower limit of the titanium content is preferably 10 wtppm or more, more preferably 30 wtppm or more, and further preferably 50 wtppm or more.

[0083] The titanium (titanium atom) content of the polyester elastomer refers to the titanium content of the polyester elastomer as a whole. For example, when the polyester elastomer is composed of a plurality of polyester polyether block copolymers having different titanium contents, it refers to the entire polyester polyether block copolymer as long as the titanium content is less than 250 wtppm.

[0084] The low titanium content in the polyester elastomer mainly refers to the low amount of titanium compound as a catalyst in the production process of the polyester elastomer, which may result in insufficient polymerization reactivity and failure to obtain the polyester elastomer. If the titanium content in the polyester elastomer is high, the decomposition reaction is accelerated, the amount of terminal carboxyl groups increases, and hydrolysis proceeds, so that the color tone of the modified polyester elastomer and the laminate containing the modified polyester elastomer deteriorates, and the heat-resistant adhesiveness and functionality as a modifier tend to be poor.

[0085] The titanium content of the polyester elastomer can be quantitatively determined by the ashing-alkali fusion-ICP / AES method.

[0086] When a plurality of polyester-based elastomers are mixed, the titanium content of the mixture is determined by adding and averaging the titanium contents of the respective polyester-based elastomers.

[0087] Regarding the titanium content of the polyester elastomer, the titanium content of the polyester elastomer as a whole can be made less than 250wtppm by using a single polyester elastomer or using a plurality of polyester elastomers having a titanium content of less than 250wtppm, or by using a polyester elastomer having a titanium content of 250wtppm or more and a polyester elastomer having a titanium content of less than 250wtppm in combination.

[0088] The titanium content of the polyester elastomer can be controlled by adjusting the amount of the titanium compound catalyst, the reaction temperature, the reaction time, etc. during the production.

[0089] <Polyalkylene ether glycol segment content>

[0090] The content of the polyalkylene ether glycol segment in the polyester polyether block copolymer, which is the raw material polyester elastomer for modification, is preferably 5 to 90% by mass, more preferably 10 to 85% by mass, and even more preferably 20 to 80% by mass.

[0091] When two or more polyester polyether block copolymers are used, even if a part of the polyester polyether block copolymers deviates from the polyalkylene ether glycol segment content of 5 to 90 mass %, the overall polyalkylene ether glycol segment content may be within the range of 5 to 90 mass %.

[0092] By making the content of the polyalkylene ether glycol chain segment of the polyester elastomer not less than the above lower limit, the strain and residual stress generated between the layers of the laminate are relieved, the adhesiveness is improved, and the function as a modifier is also excellent. By making the content of the polyalkylene ether glycol chain segment not more than the above upper limit, the decrease in the crystallinity of the polyester elastomer is suppressed, and the fusion of the polyester elastomer and the modified polyester elastomer is prevented, so that the workability at room temperature is improved.

[0093] The content of the polyalkylene ether glycol segment in the polyester elastomer was measured by dissolving the sample in a deuterated chloroform / hexafluoroisopropanol mixed solvent at room temperature using a nuclear magnetic resonance apparatus (AVANCE 400 spectrometer manufactured by Bruker Corporation). 1 The HNMR spectrum is calculated based on the chemical shift of its hydrogen spectrum.

[0094] When two or more polyester elastomers are used, the polyalkylene ether glycol segment content can be calculated by measuring each polyester elastomer as a sample in the same manner as above and calculating the content in proportion to the blending mass ratio of each polyester elastomer.

[0095] Theoretically, the content of the polyalkylene ether glycol segment in the modified polyester elastomer is the same as the content of the polyalkylene ether glycol segment in the polyester elastomer before modification. That is, it can be considered that the content of the polyalkylene ether glycol segment before and after modification does not change.

[0096] <Density>

[0097] The density of the polyester elastomer is preferably 1.00 to 1.35 g / cm 3 , more preferably 1.02 to 1.30 g / cm 3 , more preferably 1.04 to 1.25 g / cm 3 . The density of the polyester elastomer is related to the content of the polyalkylene ether glycol chain segment. If the content of the polyalkylene ether glycol chain segment increases, the density decreases. By making the density of the polyester elastomer above the lower limit of the above range, it is easy to suppress the reduction in the heat-resistant adhesion of the obtained modified polyester elastomer. By making the density of the polyester elastomer below the upper limit of the above range, it is easy to make the adhesion between the obtained modified polyester elastomer and the gas barrier material good. In addition, the effect as a modifier is also excellent.

[0098] <Melting point>

[0099] The melting point of the polyester elastomer is preferably 145 to 245°C, more preferably 150 to 230°C, and further preferably 160 to 215°C. By making the melting point above the lower limit of the above range, it is easy to suppress the reduction of heat resistance of the obtained modified polyester elastomer in the use environment, and by making the melting point below the upper limit of the above range, it is easy to make the co-extrusion moldability of the obtained modified polyester elastomer and the gas barrier material that will be thermally degraded at high temperature such as ethylene-vinyl alcohol copolymer good. In addition, the effect as a modifier is also excellent.

[0100] <D Hardness>

[0101] The D hardness (JIS-D hardness) of the polyester elastomer is preferably 10 to 80, more preferably 20 to 70, and further preferably 25 to 60. If the JIS-D hardness is above the lower limit of the above range, the obtained modified polyester elastomer tends to have excellent heat-resistant adhesiveness, and if it is below the upper limit of the above range, the obtained modified polyester elastomer tends to easily maintain the flexibility required when it is made into a laminate such as a film or a tube. In addition, the effect as a modifier is also excellent.

[0102] <MFR>

[0103] The MFR of the polyester elastomer measured under the conditions of a temperature of 230°C, a load of 2.16 kg, and 10 minutes in accordance with JIS K7210 is preferably 0.5 to 300 g / 10 minutes, more preferably 1 to 150 g / 10 minutes, and still more preferably 2 to 75 g / 10 minutes. When the MFR of the polyester elastomer is below the upper limit of the above range, the melt tension of the obtained modified polyester elastomer is increased, and the drawdown during molding is easily suppressed. When the MFR of the polyester elastomer is above the lower limit of the above range, the deterioration of moldability such as uneven thickness caused by insufficient fluidity of the obtained modified polyester elastomer is easily suppressed.

[0104] As the polyester elastomer, commercially available products may be used, such as “Tefabloc (registered trademark)” manufactured by Mitsubishi Chemical Corporation, “PELPRENE (registered trademark)” manufactured by Toyobo Co., Ltd., and “Hytrel (registered trademark)” manufactured by DuPont Toray Industries, Ltd.

[0105] The polyester elastomer may be one kind, or two or more kinds of polyester elastomers different in monomer composition, physical properties, etc. may be subjected to modification with an unsaturated carboxylic acid and / or its derivative.

[0106] [Unsaturated carboxylic acid and / or its derivatives]

[0107] As the unsaturated carboxylic acid used for modification of the polyester elastomer, α,β-ethylenically unsaturated carboxylic acid is preferred, for example, acrylic acid, methacrylic acid, ethacrylic acid, maleic acid, fumaric acid, tetrahydrofumaric acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid. As the derivatives of the unsaturated carboxylic acid, anhydrides and carboxylic acid esters of these unsaturated carboxylic acids can be exemplified, and further, derivatives such as acyl halides, amides, and imides can also be used. Among these derivatives, anhydrides are preferred.

[0108] As unsaturated carboxylic acid and / or its derivatives, maleic acid and / or its anhydride are particularly preferred among these. A variety of these compounds may also be used in combination. Furthermore, so-called vinyl silanes such as vinyltrimethoxysilane may also be used in combination with unsaturated carboxylic acid and / or its derivatives.

[0109] [Free radical generator]

[0110] The modification treatment in the production of the modified polyester elastomer of the present invention is preferably carried out in the presence of a radical generator.

[0111] The free radical generator is used to cause a free radical reaction when the polyester elastomer is modified with an unsaturated carboxylic acid and / or a derivative thereof.

[0112] As free radical generators, peroxyesters, dialkyl peroxides, diacyl peroxides, hydrogen peroxides, ketone peroxides, etc. can be cited. Among these, as diacyl peroxides, dibenzoyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane can be preferably used. These free radical generators can be appropriately selected according to the type of polyester elastomer, the type of unsaturated carboxylic acid and / or its derivatives, and the modification conditions. Free radical generators can be used in combination of two or more. The free radical generator can also be dissolved in an organic solvent and added.

[0113] [Modification treatment method of modified polyester elastomer]

[0114] The step of modifying the polyester elastomer with an unsaturated carboxylic acid and / or its derivative may be carried out by any known method, such as a melt kneading reaction method, a solution reaction method, or a suspension dispersion reaction method. In general, a melt kneading reaction method is preferred.

[0115] When the melt-kneading reaction method is adopted, the above-mentioned component (A) and component (B), as well as the component (C) as required, are uniformly mixed in a prescribed proportion and then melt-kneaded. Mixing can be performed using a Henschel mixer, a ribbon mixer, a V-type mixer, etc. Melt-kneading can generally be performed using a single-shaft or double-shaft extruder, a roll, a Banbury mixer, a kneader, a Brabender mixer, etc. Among them, a double-shaft extruder is particularly preferred.

[0116] Melt kneading is performed in a range of usually 100°C or higher, preferably 120°C or higher, more preferably 150°C or higher, and usually 300°C or lower, preferably 280°C or lower, more preferably 250°C or lower so as not to thermally degrade the resin.

[0117] The amount of the unsaturated carboxylic acid and / or its derivatives used in the modification is usually 0.01 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and usually 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 1 part by mass or less, relative to a total of 100 parts by mass of the polyester elastomer of the component (A). By making the amount of the unsaturated carboxylic acid and / or its derivatives to be above the above lower limit, it is easy to implement sufficient modification, and by making the amount of the unsaturated carboxylic acid and / or its derivatives to be below the above upper limit, it is not only economical, but also easy to suppress the unsaturated carboxylic acid and / or its derivatives that do not contribute to the modification from acting as impurities and reducing the adhesion.

[0118] The amount of the radical generator of component (C) is usually 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and usually 5 parts by mass or less, preferably 3 parts by mass or less, more preferably 2 parts by mass or less, relative to 100 parts by mass of the total polyester elastomer of component (A). When the amount of the radical generator is above the lower limit, the modification reaction is easily and sufficiently generated, and when the amount of the radical generator is below the lower limit, it is possible to suppress a significant reduction in material strength due to the promotion of low molecular weight (reduction in viscosity) of component (A).

[0119] 〔Modified polyester elastomer〕

[0120] [Titanium content]

[0121] As described above, when a titanium compound is used as a polymerization catalyst in the production of polyester elastomers, the titanium compound remains in the produced polyester elastomer, and the raw polyester elastomer used for modification contains titanium (titanium atoms). As a result, the modified polyester elastomer also contains titanium.

[0122] The titanium content of the modified polyester elastomer of the present invention is less than 250 wtppm, preferably less than 248 wtppm, more preferably less than 245 wtppm, and particularly preferably less than 240 wtppm. The lower limit of the titanium content is preferably greater than 20 wtppm, more preferably greater than 40 wtppm, and further preferably greater than 60 wtppm.

[0123] The titanium (titanium atom) content of the modified polyester elastomer refers to the titanium content of the modified polyester elastomer as a whole. For example, when the modified polyester elastomer is composed of a plurality of modified polyester elastomers having different titanium contents, it refers to the modified polyester elastomer as a whole, as long as the titanium content is less than 250wtppm.

[0124] The low titanium content of the modified polyester elastomer mainly refers to the low amount of titanium compound as a catalyst in the production process of the raw polyester elastomer, which may not provide sufficient polymerization reactivity and fail to obtain the raw polyester elastomer. If the titanium content of the modified polyester elastomer is high, the decomposition reaction is promoted, the amount of terminal carboxyl groups increases, and hydrolysis proceeds, so the color tone of the modified polyester elastomer and the laminate containing the modified polyester elastomer tends to deteriorate and the heat-resistant adhesiveness tends to be poor. In addition, for the same reason, the function as a modifier tends to be poor.

[0125] Similar to the polyester elastomer, the titanium content of the modified polyester elastomer can also be quantified by the ashing-alkali fusion-ICP / AES method.

[0126] When a plurality of modified polyester elastomers are mixed, the titanium content of the mixture can be determined by adding and averaging the titanium contents of the respective modified polyester elastomers.

[0127] Regarding the titanium content of the modified polyester elastomer, the titanium content of the modified polyester elastomer as a whole can be made less than 250wtppm by using a single modified polyester elastomer or using a plurality of modified polyester elastomers having a titanium content of less than 250wtppm, or by using a modified polyester elastomer having a titanium content of 250wtppm or more and a modified polyester elastomer having a titanium content of less than 250wtppm in combination.

[0128] If the titanium content of the raw polyester elastomer is low, there is a tendency that the titanium content of the modified polyester elastomer obtained by modification is also low. In order to obtain a modified polyester elastomer with a titanium content of less than 250wtppm, it is preferred to use a polyester elastomer with a titanium content of less than 250wtppm as the raw polyester elastomer for modification. However, the titanium content of the raw polyester elastomer and the titanium content of the modified polyester elastomer are not necessarily proportional. This is because the titanium content of the modified polyester elastomer increases or decreases due to the mixing of metal from the extruder or removal by the mesh filter during the modification process. As described above, the titanium content of the polyester elastomer can be controlled by adjusting the amount of titanium compound catalyst, reaction temperature, reaction time, etc. during the production of the polyester elastomer, and the titanium content of the modified polyester elastomer can be controlled by adjusting the titanium content of the raw polyester elastomer. The titanium content of the modified polyester elastomer can also be controlled by the composition of the mesh filter during the modification process, the selection of the metal type of the extruder, etc.

[0129] [Acid value]

[0130] From the viewpoint of suppressing the formation of by-products during heating during molding, the lower limit of the acid value of the modified polyester elastomer of the present invention is preferably 1 eq / T (equivalent / ton) or more, more preferably 5 eq / T or more, and even more preferably 10 eq / T or more. From the viewpoint of color tone and heat-resistant adhesiveness, the upper limit of the acid value of the modified polyester elastomer is preferably 70 eq / T or less, more preferably 68 eq / T or less, and even more preferably 66 eq / T or less.

[0131] The acid value of the modified polyester elastomer can be determined by, for example, dissolving the modified polyester elastomer in a benzyl alcohol solvent by heating, and then titrating the solution with a 0.1 mol / L sodium hydroxide benzyl alcohol solution as an indicator. 6 The amount of carboxyl groups in g was quantitatively determined.

[0132] The acid value of the modified polyester elastomer can be adjusted to the above range by adjusting the temperature, time, degree of polymerization, etc. during the production of the modified polyester elastomer.

[0133] [density]

[0134] The density of the modified polyester elastomer of the present invention is preferably 1.00 to 1.35 g / cm 3 , more preferably 1.02 to 1.30 g / cm 3 , more preferably 1.04 to 1.25 g / cm 3 The density of the modified polyester elastomer is related to the content of the polyalkylene ether glycol segment. If the content of the polyalkylene ether glycol segment increases, the density decreases. That is, by making the density above the lower limit of the above range, it is easy to suppress the decrease in heat-resistant adhesiveness, and by making the density below the upper limit of the above range, it is easy to improve the adhesion with the gas barrier material and the functionality as a modifier.

[0135] [Melting point]

[0136] The melting point of the modified polyester elastomer of the present invention is preferably 145 to 245°C, more preferably 150 to 230°C, and further preferably 160 to 215°C. By making the melting point above the lower limit of the above range, it is easy to suppress the decrease in heat resistance under the use environment. By making the melting point below the upper limit of the above range, it is easy to improve the co-extrusion moldability with gas barrier materials that are thermally degraded at high temperatures such as ethylene-vinyl alcohol copolymers.

[0137] [D hardness]

[0138] The D hardness (JIS-D hardness) of the modified polyester elastomer of the present invention is preferably 10 to 80, more preferably 20 to 70, and even more preferably 25 to 60. If the JIS-D hardness is at least the lower limit of the above range, the heat-resistant adhesiveness and the functionality as a modifier tend to be excellent. If the JIS-D hardness is at most the upper limit of the above range, the flexibility required when forming a laminate such as a film or a tube tends to be easily maintained.

[0139] [MFR]

[0140] The MFR of the modified polyester elastomer of the present invention measured under the conditions of 230°C, 2.16 kg load, and 10 minutes in accordance with JIS K7210 is preferably 0.5 to 300 g / 10 minutes, more preferably 1 to 300 g / 10 minutes, further preferably 1 to 150 g / 10 minutes, and particularly preferably 2 to 75 g / 10 minutes. When the MFR of the modified polyester elastomer is below the upper limit of the above range, the melt tension is increased and the drawdown during molding is easily suppressed. When the MFR of the modified polyester elastomer is above the lower limit of the above range, it is easy to suppress the deterioration of moldability such as uneven thickness caused by insufficient fluidity.

[0141] [Polyalkylene ether glycol segment content]

[0142] As described above, the content of the polyalkylene ether glycol segment of the modified polyester elastomer is theoretically the same as the content of the polyalkylene ether glycol segment of the raw polyester elastomer before modification. The content of the polyalkylene ether glycol segment of 100% by mass of the modified polyester elastomer of the present invention is preferably 5 to 90% by mass, more preferably 10 to 85% by mass, and further preferably 20 to 80% by mass. By making the content of the polyalkylene ether glycol segment of the modified polyester elastomer 5 to 90% by mass, the operability becomes good, and when it is used as an adhesive layer, good adhesion can be satisfied. In addition, the functionality as a modifier is also excellent.

[0143] Here, the content of the polyalkylene ether glycol segments of the modified polyester elastomer refers to the content of the polyalkylene ether glycol segments of the modified polyester elastomer as a whole. That is, for example, when two or more modified polyester elastomers are mixed and used, even if one of them deviates from the polyalkylene ether glycol segment content of 5 to 90% by mass, the polyalkylene ether glycol segment content of the modified polyester elastomer as the mixture only needs to fall within the range of 5 to 90% by mass.

[0144] [Acid modification rate]

[0145] The acid modification rate of the modified polyester elastomer of the present invention is not particularly limited, and is preferably 0.01 to 10. As long as the acid modification rate is above the lower limit of the above range, sufficient adhesion to the gas barrier layer is obtained. In addition, the functionality as a modifier is also excellent. As long as the acid modification rate is below the upper limit of the above range, discoloration caused by unsaturated carboxylic acids and / or their derivatives can be suppressed. The lower limit of the acid modification rate is more preferably above 0.1, further preferably above 0.15, and particularly preferably above 0.16. The upper limit of the acid modification rate is more preferably below 4, and further preferably below 0.8.

[0146] In addition, the acid modification rate of the modified polyester-based elastomer is measured and calculated by the method described in the section of Examples described later.

[0147] [Adhesive polymer composition containing modified polyester elastomer]

[0148] The modified polyester elastomer of the present invention can be used to prepare an adhesive polymer composition. The adhesive polymer composition can be used for the adhesive layer of the laminate of the present invention described below.

[0149] The content of the modified polyester elastomer of the present invention in the adhesive polymer composition is preferably 50% by mass or more, more preferably 55% by mass or more, and further preferably 60% by mass or more. As long as the content of the modified polyester elastomer of the present invention in the adhesive polymer composition is greater than the above lower limit, the adhesion to the gas barrier layer, the ester polymer layer as another layer, etc. can be sufficiently improved. The upper limit of the content of the modified polyester elastomer of the present invention in the adhesive polymer composition is not particularly limited, but is less than 100% by mass.

[0150] The adhesive polymer composition may contain, in addition to the modified polyester elastomer of the present invention, any component (hereinafter sometimes referred to as other components) depending on the purpose. The other component may be used alone or in combination of two or more at any combination ratio.

[0151] As other components, specifically, polymers other than the modified polyester elastomer of the present invention, rubber components (ester polymers such as polyethylene terephthalate and polybutylene terephthalate, styrene (co)polymers such as polystyrene, acrylic acid / methacrylic acid copolymers such as polyolefin and polymethyl methacrylate, etc.), heat stabilizers, weather stabilizers (antioxidants, light stabilizers, ultraviolet absorbers, etc.), flame retardants, anti-blocking agents, slip agents, antistatic agents, fillers (inorganic and / or organic fillers, etc.), processing aids, plasticizers such as paraffin oil, crystal nucleating agents, impact modifiers, compatibilizers, neutralizers for catalyst residues, carbon black, colorants (pigments, dyes, etc.), antifogging agents, crosslinking agents, crosslinking aids, chain extenders, dispersants, antibacterial agents, antiviral agents, fluorescent whitening agents, etc. additives. Among them, it is preferred to add at least one of various antioxidants such as phenolic, phosphite, thioether, and aromatic amine. When these antioxidants are used, their content is not limited, but is usually 0.01% by mass or more, preferably 0.05% by mass or more, and usually 5% by mass or less, preferably 2% by mass or less, in 100% by mass of the adhesive polymer composition constituting the adhesive layer.

[0152] [Laminated body]

[0153] The adhesive layer composed of the modified polyester elastomer of the present invention or the adhesive polymer composition containing the modified polyester elastomer and the gas barrier layer can be laminated to form a laminate. That is, the modified polyester elastomer of the present invention or the adhesive polymer composition containing the modified polyester elastomer can be used to form the adhesive layer of the laminate.

[0154] The laminate using the modified polyester elastomer of the present invention is preferably a laminate having two or three or more layers laminated therein.

[0155] In particular, the laminate is preferably a laminate of the present invention comprising a substrate layer, a layer composed of the modified polyester elastomer of the present invention or an adhesive polymer composition containing the modified polyester elastomer of the present invention as an adhesive layer, and a resin layer such as a gas barrier layer.

[0156] Among them, the laminate of the present invention preferably has the above-mentioned gas barrier layer composed of a polyamide polymer and / or an ethylene-vinyl alcohol copolymer, and preferably has an ester polymer layer as needed. The laminate of the present invention more preferably has a gas barrier layer composed of a polyamide polymer and / or an ethylene-vinyl alcohol copolymer, an adhesive layer composed of a modified polyester elastomer of the present invention or an adhesive polymer composition containing the modified polyester elastomer, and a laminate composed of an ester polymer. Among these, it is preferred to use a laminate in which a substrate layer composed of an ester polymer, an adhesive layer composed of a modified polyester elastomer of the present invention or an adhesive polymer composition containing the modified polyester elastomer, and a gas barrier layer are stacked in sequence. In this case, for example, it can also be a laminate in which a portion of the layers are stacked in more than two layers, such as a substrate layer / adhesive layer / gas barrier layer / adhesive layer / substrate layer.

[0157] [Adhesive layer]

[0158] The adhesive layer composed of the modified polyester elastomer of the present invention or the adhesive polymer composition containing the modified polyester elastomer contains preferably 50% by mass or more, more preferably 55% by mass or more, and further preferably 60% by mass or more of the modified polyester elastomer of the present invention relative to the entire constituent components of the adhesive layer. As long as the content of the modified polyester elastomer is greater than the above lower limit, the adhesion with the gas barrier layer, the ester polymer layer as the substrate layer, etc. can be sufficiently improved. It should be noted that the upper limit of the content of the modified polyester elastomer of the present invention is not particularly limited and may be 100% by mass.

[0159] [Gas barrier layer]

[0160] Examples of the gas barrier layer of the present invention include polyamide polymer layers, ethylene-vinyl alcohol copolymer layers, polyvinyl alcohol layers, metal foils such as aluminum, aluminum vapor-deposited films, transparent vapor-deposited films such as alumina vapor-deposited films and silicon dioxide vapor-deposited films, and vinylidene chloride layers. Among them, layers containing polyamide and ethylene-vinyl alcohol copolymers as main components are preferred.

[0161] Polyamide polymers are usually produced by polycondensation of diamines and dicarboxylic acids, and can also be obtained by ring-opening polymerization of lactams. Specific examples of these polyamide polymers include polyamide 6,6, polyamide 6,9, polyamide 6,10, polyamide 6,12, polyamide 4,6, polyamide 6, polyamide 12, polyamide 11, and the like. In addition, copolymerized polyamides such as polyamide 6 / 6,6, polyamide 6 / 6,10, polyamide 6 / 12, polyamide 6 / 6,12, polyamide 6 / 6,6 / 6,10, and polyamide 6 / 6,6 / 12 can also be used. Furthermore, semi-aromatic polyamides such as polyamide 6 / 6,T (T: terephthalic acid component), polyamide 6,T / 6,I (I: isophthalic acid component), and polyamide MXD6 can also be used. Semi-aromatic polyamides can be produced, for example, by replacing dicarboxylic acid with aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid (in this case, diamine can also be replaced with alicyclic diamines), or by replacing diamine with aromatic diamines such as meta-xylylenediamine. Polyesteramides in which a portion of diamine is replaced with diols can also be used. Furthermore, polyamide polymers produced using diamines or dicarboxylic acids synthesized from plant raw materials can also be used. Particularly preferred polyamide polymers are polyamide 6, polyamide 6,6, polyamide 12, polyamide 11, and polyamide MXD6.

[0162] Examples of commercially available products of such polyamide-based polymers include “Novamid (registered trademark)” manufactured by DSM Japan Engineering Plastics, “Xencor (registered trademark)” and “Amodel (registered trademark)” manufactured by Solvay, “Rilsan (registered trademark)” manufactured by Arkema, “MX Nylon (registered trademark)” manufactured by Mitsubishi Gas Chemical Corporation, and “Reny (registered trademark)” manufactured by Mitsubishi Engineering-Plastics Corporation.

[0163] The gas barrier layer of the present invention may contain only one polyamide polymer, or may contain two or more polyamide polymers having different monomer compositions, etc., preferably a polyamide polymer as a main component, usually containing 50% by mass or more, particularly 65 to 100% by mass, and particularly 75 to 100% by mass. As long as the content of the polyamide polymer in the gas barrier layer is above the above lower limit, excellent mechanical strength and gas barrier properties can be obtained.

[0164] The ethylene-vinyl acetate copolymer is saponified in the presence of an alcohol to produce an ethylene-vinyl alcohol copolymer. As the ethylene-vinyl alcohol copolymer constituting the gas barrier layer, it is preferred to use an ethylene-vinyl acetate copolymer having an ethylene content of preferably 15 to 65 mol%, more preferably 20 to 50 mol%, and saponified in such a manner that the degree of saponification is preferably 50% or more, more preferably 90% or more.

[0165] Examples of commercially available products of such ethylene-vinyl alcohol-based copolymers include “Soarnol (registered trademark)” manufactured by Mitsubishi Chemical Corporation, “Eval (registered trademark)” manufactured by Kuraray Co., Ltd., and “Evasin (registered trademark)” manufactured by Changchun Group.

[0166] The gas barrier layer of the present invention may contain only one ethylene-vinyl alcohol copolymer, or may contain two or more ethylene-vinyl alcohol copolymers having different saponification degrees, monomer compositions, etc. The gas barrier layer preferably contains ethylene-vinyl alcohol copolymer as a main component and usually contains 50% by mass or more, particularly 65 to 100% by mass, and particularly 75 to 100% by mass. As long as the content of ethylene-vinyl alcohol copolymer in the gas barrier layer is above the above lower limit, excellent gas barrier properties can be obtained.

[0167] As components other than polyamide polymers and ethylene-vinyl alcohol copolymers that can be included in the gas barrier layer, there are no particular limitations, and examples thereof include polyolefins, styrene (co)polymers such as polystyrene, polymer components such as acrylic acid / methacrylic acid copolymers, heat stabilizers, weather stabilizers (antioxidants, light stabilizers, ultraviolet absorbers, etc.), flame retardants, anti-blocking agents, lubricants, fillers (inorganic and / or organic fillers, etc.), processing aids, plasticizers such as paraffin oil, crystal nucleating agents, impact modifiers, compatibilizers, catalyst residue neutralizers, colorants (pigments, dyes, etc.), and various additives. It should be noted that here, "(co)polymer" refers to one or both of "polymer" and "copolymer".

[0168] [Base material layer]

[0169] As constituent components constituting the substrate layer involved in the present invention, there can be mentioned ester polymers, styrene (co)polymers such as polystyrene, polyolefins, acrylic acid / methacrylic copolymers such as polymethyl methacrylate, polyvinyl chloride, ABS, thermoplastic polymers such as polycarbonates, etc. Among these, in order to impart functionalities such as aroma preservation, rigidity, heat resistance, cold resistance, and surface printability, a layer composed of an ester polymer is preferred.

[0170] The ester polymer is produced by dehydration condensation of a polycarboxylic acid and a polyol. For example, an ester polymer obtained by polycondensation of a dicarboxylic acid and a diol can be mentioned.

[0171] The carboxylic acid is not particularly limited, and examples thereof include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, diphenyl ether-4,4-dicarboxylic acid, and naphthalene-1,4- or 2,6-dicarboxylic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, and undecanedicarboxylic acid; and alicyclic dicarboxylic acids such as hexahydroterephthalic acid.

[0172] The diol is not particularly limited, and examples thereof include aliphatic diols such as ethylene glycol, propylene glycol, 1,4-butanediol, and neopentyl glycol; alicyclic diols such as cyclohexanedimethanol; and aromatic dihydroxy compounds such as bisphenol A.

[0173] Examples of the ester polymer include polyethylene terephthalate (PET), copolymerized PET, polybutylene terephthalate, polyethylene naphthalate, polycyclohexyl terephthalate, and polyester elastomers. These ester polymers may be used alone or in combination with a plurality of ester polymers.

[0174] Polyamide, ethylene-vinyl alcohol copolymer and ester copolymer may contain any one of components derived from biomass, chemically recycled polymer components obtained by polymerizing recycled monomers and recycled oligomers obtained by depolymerizing plastic waste, etc. as starting materials, and recycled material components obtained by crushing trimming scraps, slitting scraps, etc. generated during film manufacturing or re-melting and granulating the above scraps and defective films, or a combination of these components.

[0175] [Morphology of Gas Barrier Layer and Substrate Layer]

[0176] The gas barrier layer and the substrate layer are not limited to the form of a film or a sheet, but may also be in the form of a fabric or a nonwoven fabric. The gas barrier layer and the substrate layer may be a single layer structure or a multilayer structure. The method for preparing the substrate of the multilayer structure is not particularly limited, and examples thereof include a co-pressed film method, a dry lamination method, a wet lamination method, a hot melt lamination method, an extrusion lamination method, a hot lamination method, and the like.

[0177] [Other constituent layers]

[0178] The laminate of the present invention may include any layer other than the adhesive layer composed of the modified polyester elastomer of the present invention or the adhesive polymer composition containing the modified polyester elastomer of the present invention, the gas barrier layer, and the substrate layer.

[0179] [Layer composition]

[0180] The laminate of the present invention may be a laminate having three or four or more layers further including the above-mentioned adhesive layer, a resin layer such as a gas barrier layer, and / or a substrate layer.

[0181] Examples of the form of the laminate of the present invention include laminate films, laminate sheets, laminate tubes, etc. Here, "film" and "sheet" both refer to planar molded bodies and have the same meaning.

[0182] [thickness]

[0183] The overall thickness of the laminate of the present invention is not particularly limited and can be appropriately adjusted according to the application. The overall thickness of the laminate of the present invention is preferably 20 μm or more, more preferably 50 μm or more, and further preferably 100 μm or more, preferably 10 mm or less, more preferably 6 mm or less, and further preferably 1 mm or less. By having a thickness within the above range, it is easy to manufacture a laminate without wrinkles, cracks, etc.

[0184] The thickness of the adhesive layer composed of the modified polyester elastomer of the present invention or the adhesive polymer composition containing the modified polyester elastomer of the present invention is preferably 1 μm or more, more preferably 2 μm or more, further preferably 10 μm or more, preferably 1 mm or less, more preferably 0.5 mm or less, further preferably 0.1 mm or less.

[0185] The thickness of the gas barrier layer is generally 0.002 to 1 mm.

[0186] The thickness of the substrate layer is generally 0.01 to 5 mm.

[0187] [Method for producing laminated body]

[0188] As a method for manufacturing the laminate of the present invention, various methods known in the past can be used. For example, a blown film, cast film, sheet, tube, pipe, or bottle can be made by a co-extrusion method in which each molten polymer melted in an extruder is supplied to a multilayer die and laminated in the die, or by co-injection molding in which each molten polymer is injected into the same metal mold in sequence, or by co-extrusion lamination of an unstretched test tube-shaped parison or the like.

[0189] 〔Modifier〕

[0190] The modifier of the present invention includes the modified polyester elastomer of the present invention described above, and is particularly useful as a modifier for improving the properties such as flexibility of polar polymers such as ethylene-vinyl alcohol copolymers and polyamide polymers.

[0191] When the modified polyester elastomer of the present invention is used as a modifier for these polar polymers, the mixing ratio of the modified polyester elastomer of the present invention to the polar polymer is not particularly limited, but the modified polyester elastomer of the present invention is preferably used in an amount of preferably 1% by mass or more, more preferably 3% by mass or more, further preferably 5% by mass or more, preferably 30% by mass or less, more preferably 25% by mass or less, further preferably 23% by mass or less, and particularly preferably 20% by mass or less, based on the total of the polar polymer and the modified polyester elastomer of the present invention.

[0192] When the ratio of the modified polyester elastomer of the present invention is within the above range, the modification effect of the modified polyester elastomer of the present invention can be sufficiently obtained without impairing the characteristics as a polar polymer.

[0193] [Polar polymer composition]

[0194] The polar polymer composition of the present invention is a polar polymer composition containing 1 to 30 mass % of the above-mentioned modified polyester elastomer of the present invention relative to the total of the polar polymer and the modified polyester elastomer of the present invention, and the above-mentioned polar polymer contains at least one selected from ethylene-vinyl alcohol copolymers and polyamide polymers.

[0195] [Polar polymer]

[0196] As the ethylene-vinyl alcohol copolymer and the polyamide polymer contained in the polar polymer composition of the present invention, there can be mentioned the ethylene-vinyl alcohol copolymer and the polyamide polymer respectively exemplified as the ethylene-vinyl alcohol copolymer and the polyamide polymer contained in the gas barrier layer of the laminate of the present invention mentioned above, and the preferred examples are also the same.

[0197] The ethylene-vinyl alcohol copolymer and the polyamide polymer may be used alone or in combination of two or more. One or more ethylene-vinyl alcohol copolymers and one or more polyamide polymers may be mixed for use.

[0198] [Content of modified polyester elastomer]

[0199] In the polar polymer composition of the present invention, as long as the content of the modified polyester elastomer of the present invention is 1% by mass or more relative to the total of the polar polymer and the modified polyester elastomer of the present invention, the modification effect brought about by containing the modified polyester elastomer of the present invention can be fully obtained. As long as the content of the modified polyester elastomer of the present invention is 30% by mass or less relative to the total of the polar polymer and the modified polyester elastomer of the present invention, the original characteristics of the polar polymer can be fully obtained. From this viewpoint, the content of the modified polyester elastomer of the present invention is preferably 3% by mass or more, more preferably 5% by mass or more relative to the total of the polar polymer and the modified polyester elastomer of the present invention. On the other hand, it is preferably 25% by mass or less, more preferably 23% by mass or less, and further preferably 20% by mass or less. From the same viewpoint, the content of the polar polymer is 70% by mass or more, preferably 75% by mass or more, more preferably 77% by mass or more, and further preferably 80% by mass relative to the total of the polar polymer and the modified polyester elastomer. On the other hand, it is 99% by mass or less, preferably 97% by mass or less, and more preferably 95% by mass or less.

[0200] [Other ingredients]

[0201] The polar polymer composition of the present invention may contain polymers other than the polar polymer and the modified polyester elastomer of the present invention, arbitrary additives, etc. (hereinafter referred to as "other components") according to various purposes within a range that does not significantly impair the effects of the present invention. The other components may be used alone or in any combination and ratio.

[0202] Examples of additives include antioxidants, ultraviolet absorbers, plasticizers, lubricants, fillers, and antistatic agents. The total content of these additives in the polar polymer composition of the present invention is usually 50% by mass or less, preferably 20% by mass or less, and more preferably 10% by mass or less.

[0203] [Method for producing polar polymer composition]

[0204] There is no particular limitation on the mixing method for obtaining the components of the polar polymer composition of the present invention, and examples include a method in which the polar polymer, the modified polyester elastomer of the present invention and other components used as required are dry-blended and melt-kneaded at one time; a method in which the polar polymer, the modified polyester elastomer of the present invention and a part of other components used as required are melt-kneaded in advance, and then melt-kneaded with other components.

[0205] As a specific method for melt kneading, there can be exemplified a method in which each component is uniformly mixed at a predetermined mixing ratio using a Henschel mixer, a ribbon mixer, a V-type mixer or the like, and then kneaded using a multi-screw kneading extruder, for example, PCM30, which is a twin-screw kneading extruder manufactured by Ikegai Corporation.

[0206] The temperature for melt kneading the components is the same as the temperature for modification of the modified polyester elastomer of the present invention with an unsaturated carboxylic acid and / or its derivative, and is usually 100 to 300°C, preferably 120 to 280°C, more preferably 150 to 250°C.

[0207] [Molding products]

[0208] The polar polymer composition of the present invention can be molded into a molded article (hereinafter, sometimes referred to as a "polar polymer molded article").

[0209] Examples of the shape of the polar polymer molded article include films, sheets, tapes, cups, trays, tubes, bottles, pipes, filaments, extrudates with irregular cross sections, and various amorphous molded products.

[0210] The molding method of the polar polymer composition of the present invention is not particularly limited, and any molding method applicable to general polymer compositions may be used.

[0211] For example, extrusion molding, blow molding, injection molding, thermoforming, etc. are mentioned.

[0212] Furthermore, in the molding process, in order to improve the physical properties of the molded product or to mold it into any desired container shape, a heat stretching treatment is often performed. Here, the heat stretching treatment refers to the operation of uniformly molding a film, sheet, or parison-shaped molded product that has been uniformly heated by heat into a cup, plate, tube, bottle, or film-shaped product using a chuck, a mandrel, a vacuum force, a compressed air force, or a blow molding. Moreover, as the stretching method, roller stretching, tentering stretching, tubular stretching, stretch blow molding, vacuum molding, compressed air molding, and vacuum compressed air molding can be cited. Stretching can be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, any of simultaneous biaxial stretching and sequential biaxial stretching can also be used. The stretching temperature is usually 60 to 170°C, and more preferably 80 to 160°C.

[0213] Example

[0214] Hereinafter, the content of the present invention is described in more detail using examples. The present invention is not limited by the following examples as long as it does not exceed its purport. The values ​​of various manufacturing conditions and evaluation results in the following examples have the meaning of the preferred values ​​as the upper or lower limits in the embodiments of the present invention, and the preferred range can be the range specified by the combination of the values ​​of the above-mentioned upper or lower limits and the values ​​of the following examples or the values ​​of the examples.

[0215] [raw materials]

[0216] The raw materials used in the production of the adhesive polymer composition containing the modified polyester elastomer in the following Examples and Comparative Examples are as follows.

[0217] [Material for adhesive layer: adhesive polymer composition containing modified polyester elastomer]

[0218] <Ingredients (A)>

[0219] A-1: Polyester elastomer

[0220] A polyester-polyether block copolymer having polybutylene terephthalate as a hard segment and polytetramethylene ether glycol having a number average molecular weight of 2000 as a soft segment, wherein the content of the polytetramethylene ether glycol segment in the copolymer is 73% by mass, was used. 3 , melting point: 160.1℃, JIS-D hardness: 24, MFR: 20g / 10min).

[0221] A-2: Polyester elastomer

[0222] A polyester-polyether block copolymer having polybutylene terephthalate as a hard segment and polytetramethylene ether glycol having a number average molecular weight of 2,000 as a soft segment, wherein the content of the polytetramethylene ether glycol segment in the copolymer is 64% by mass, was used. 3 , melting point: 186.1℃, JIS-D hardness: 31, MFR: 21g / 10min).

[0223] A-3: Polyester elastomer

[0224] A polyester-based elastomer (density: 1.10 g / cm2) was used, which had a polybutylene terephthalate as a hard segment and a polytetramethylene ether glycol with a number average molecular weight of 1000 as a soft segment, and a polytetramethylene ether glycol segment content of 61% by mass. 3 , melting point: 160.6℃, JIS-D hardness: 38, MFR: 17g / 10min).

[0225] A-4: Polyester elastomer

[0226] A polyester-polyether block copolymer having polybutylene terephthalate as a hard segment and polytetramethylene ether glycol having a number average molecular weight of 2000 as a soft segment, wherein the content of the polytetramethylene ether glycol segment in the copolymer is 64% by mass, was used. 3 , melting point: 184.8℃, JIS-D hardness: 31, MFR: 26g / 10min).

[0227] A-5: Polyester elastomer

[0228] A polyester-polyether block copolymer having polybutylene terephthalate as a hard segment and polytetramethylene ether glycol having a number average molecular weight of 2000 as a soft segment, wherein the content of the polytetramethylene ether glycol segment in the copolymer is 75% by mass, was used. 3 , melting point: 147.2.0℃, JIS-D hardness: 22, MFR: 25g / 10min).

[0229] A-6: Polyester elastomer

[0230] A polyester-polyether block copolymer having polybutylene terephthalate as a hard segment and polytetramethylene ether glycol having a number average molecular weight of 1000 as a soft segment, wherein the content of the polytetramethylene ether glycol segment in the copolymer is 58% by mass, was used. 3 , melting point: 165°C, JIS-D hardness: 33, MFR: 29g / 10 minutes).

[0231] <Ingredient (B)>

[0232] B: Unsaturated carboxylic anhydride

[0233] A material obtained by pulverizing "Maleic Anhydride (reagent special grade)" (particle size 5 to 10 mm) manufactured by Wako Pure Chemical Industries, Ltd. into particles of 1 mm or less using a small mixer was used.

[0234] <Ingredient (C)>

[0235] C: Benzoyl peroxide

[0236] "NYPER (registered trademark) BMTK-40" manufactured by NOF Corporation was used.

[0237] <Additives (anti-blocking agents)>

[0238] X used: Polyethylene wax "ACumist B-6 (registered trademark)" manufactured by Honeywell.

[0239] [Materials for gas barrier layers]

[0240] Polyamide (PA6)

[0241] “Novamid (registered trademark) 1020” manufactured by DSM Japan Engineering Plastics Co., Ltd. was used.

[0242] [Material for base layer]

[0243] Ester polymer

[0244] "Novaduran (registered trademark) 5505S" manufactured by Mitsubishi Engineering-Plastics Corporation was used.

[0245] [Polar polymer]

[0246] <Polyamide polymer: Polyamide (PA6)>

[0247] “Novamid (registered trademark) 1020” manufactured by DSM Japan Engineering Plastics Co., Ltd. was used.

[0248] <Ethylene-vinyl alcohol copolymer (EVOH)>

[0249] "SOARNOL (registered trademark) DC3203RB" manufactured by Mitsubishi Chemical Corporation was used.

[0250] [Evaluation Method]

[0251] In the examples and comparative examples, physical properties were evaluated by the following methods. Note that Examples 1-3 and Comparative Examples 1-3 evaluated physical properties of modified polyester elastomers, and the other examples and comparative examples evaluated physical properties of adhesive polymer compositions containing modified polyester elastomers.

[0252] In the adhesive polymer compositions containing modified polyester elastomers produced in the examples and comparative examples, the content of additives (anti-blocking agents) other than the modified polyester elastomer is very small, so the evaluation results of the adhesive polymer compositions can be regarded as the evaluation results of the modified polyester elastomer, and are therefore expressed as values ​​of the modified polyester elastomer.

[0253] [Titanium content]

[0254] The titanium content of the polyester elastomer and the modified polyester elastomer / adhesive polymer composition containing the modified polyester elastomer was measured by the above-mentioned method.

[0255] [Polyalkylene ether glycol segment content]

[0256] The polyalkylene ether glycol content in the polyester elastomer and the modified polyester elastomer / adhesive polymer composition containing the modified polyester elastomer is measured by the above-mentioned method.

[0257] [MFR]

[0258] MFR is measured by vacuum drying the adhesive polymer composition containing the modified polyester elastomer in a pellet state at 100° C. for 4 hours to remove the contained water, and then measuring the temperature at 230° C. and a load of 2.16 kg for 10 minutes in accordance with JIS K7210.

[0259] [Acid value]

[0260] The acid value is measured by neutralization titration. Specifically, the sample is placed in a benzyl alcohol solvent, heated and dissolved in an oil bath at 195°C, and then a chloroform solvent is added to cool the mixture. The indicator titration is performed using a 0.1 mol / L sodium hydroxide benzyl alcohol solution of known titer. The point at which the sample solution changes from yellow to red is taken as the end point, and the acid (carboxyl) value is calculated by the following formula.

[0261]

[0262] In the above formula,

[0263] S: mass of the sample (g),

[0264] V0: The amount of 0.1 mol / L sodium hydroxide benzyl alcohol solution required for the blank test (mL),

[0265] V1: the amount (mL) of 0.1 mol / L sodium hydroxide benzyl alcohol solution required for the titration of this test, f: the titer of 0.1 mol / L sodium hydroxide benzyl alcohol solution.

[0266] [density]

[0267] The density was measured by the water displacement method in accordance with JIS K7112.

[0268] [Melting point]

[0269] The melting point is measured using a differential scanning calorimeter (DSC). Specifically, the temperature is temporarily raised to 300°C to eliminate the thermal history, then the temperature is lowered to 40°C at a cooling rate of 10°C / min, and the temperature is again raised at a heating rate of 10°C / min for measurement, and the temperature at the endothermic peak at this time is taken as the melting point. The unit is °C.

[0270] [hardness]

[0271] The hardness was measured using a durometer in accordance with JIS K6253 (D hardness).

[0272] [Acid modification rate]

[0273] The acid modification rate refers to the content of the unsaturated carboxylic acid component in the modified polyester elastomer when measured by an infrared spectrometer (JASCOFT / IR610, manufactured by JASCO Corporation). The acid modification rate is determined by measuring the absorption (1900-1600 cm-1) specific to the unsaturated carboxylic acid and / or its derivative in a sample obtained by press-molding the pellets of the adhesive polymer composition containing the modified polyester elastomer into a sheet with a thickness of 20-50 μm at 230°C. -1 ) and the unique absorption of the aromatic ring in the hard segment (1000~800cm -1 ) is measured and found.

[0274] [Color tone (grain YI)]

[0275] The color tone (particle YI) was measured using "ZE-2000" manufactured by Nippon Denshoku Industries Co., Ltd. The lower the YI value, the less yellowish the color tone is, and the better the color tone is.

[0276] [Adhesion of laminated body]

[0277] Generally, a laminate having an interlaminar strength of 2 N / 15 mm or more is considered to have sufficient strength for practical use, and a laminate having an adhesive retention rate after a heat resistance test exceeding 80% is considered acceptable.

[0278] <Initial Adhesion>

[0279] The five-layer film obtained in each example was cut into a strip with a width of 15 mm parallel to the molding direction to prepare a test piece, and a T peel test was performed at a speed of 300 mm / min in a constant temperature atmosphere of 23°C to measure the adhesive strength. Here, the adhesive strength of Examples 1 to 6 and Comparative Examples 1 to 3 is the adhesive strength of the interface between the PA6 layer and the adhesive layer.

[0280] <Heat-resistant adhesiveness>

[0281] For the five-layer film obtained in each example, a long strip test piece prepared in the same manner as above was placed in a gear oven (Toyo Seiki) at 150°C for 16 hours, taken out, and subjected to a T-type peel test at a speed of 300 mm / min in a constant temperature atmosphere of 23°C to measure the adhesive strength. As above, the adhesive strength of Examples 1 to 6 and Comparative Examples 1 to 3 is the adhesive strength of the interface between PA6 and the adhesive layer.

[0282] [Adhesion retention rate]

[0283] The ratio (percentage) of the adhesive strength of the heat-resistant adhesive property to the adhesive strength of the initial adhesive property was calculated.

[0284] [Flexural modulus]

[0285] The flexural modulus was measured in accordance with ISO178.

[0286] [Izod impact strength]

[0287] The Izod impact strength was measured under four temperature conditions (23°C, 0°C, -30°C, and -50°C) according to ISO 180 / 1A.

[0288] [Example 1-1]

[0289] <Production of Adhesive Polymer Composition Containing Modified Polyester Elastomer>

[0290] As shown in Table 1, 100 parts by mass of polyester elastomer A-1, 0.5 parts by mass of maleic anhydride B, and 0.1 parts by mass of dibenzoyl peroxide C were dry-blended and mixed, and the mixture was extruded using a twin-screw extruder (TEX25αIII, manufactured by Nippon Steel Works, Ltd.). The mixture was melt-kneaded at a set temperature of 180 to 240° C., a screw speed of 200 to 400 rpm, and an extrusion rate of 15 to 30 kg / h, and pellets were obtained by strand cutting. In order to prevent mutual fusion of the pellets, 0.1 parts by mass of an anti-blocking agent X was added to the obtained modified polyester elastomer, and dry-blended, thereby obtaining pellets of an adhesive polymer composition containing a modified polyester elastomer.

[0291] The MFR and color tone of the adhesive polymer composition containing the modified polyester elastomer were measured.

[0292] <Manufacturing of laminated body>

[0293] The adhesive polymer composition containing the modified polyester elastomer obtained above is used as an adhesive layer material to produce a laminate.

[0294] A five-layer film was produced in the form of a laminate of ester polymer layer / adhesive layer composed of an adhesive polymer composition containing a modified polyester elastomer / polyamide (PA6) layer / adhesive layer composed of an adhesive polymer composition containing a modified polyester elastomer / ester polymer layer using a multilayer film forming machine (Labtech Engineering Co.) having three types of five-layer feed block T-die with a width of 350 mm. The temperature of the T-die was set to 240° C., and a film having a total thickness of 120 μm was obtained with a forming speed of 6 m / min and a casting roll temperature of 80° C. wherein the thickness of each layer was 40 μm / 10 μm / 20 μm / 10 μm / 40 μm.

[0295] The adhesive strength of the obtained five-layer film was measured.

[0296] Table 1 shows the above measurement results.

[0297] [Examples 1-2 to 1-6, Comparative Examples 1-1 to 1-3]

[0298] In the production of the adhesive polymer composition containing a modified polyester elastomer, pellets of the adhesive polymer composition containing a modified polyester elastomer were obtained in the same manner as in Example 1-1, and a laminate was produced in the same manner and measured. The results are shown in Table 1.

[0299] Table 1 lists the content of the polyalkylene ether glycol segment and the titanium content of the polyester elastomer used in the production of the modified polyester elastomer, as well as the content of the polyalkylene ether glycol segment, the titanium content, the acid value, the melt flow rate, the density, the melting point, the hardness and the acid modification rate of the modified polyester elastomer.

[0300] [Table 1]

[0301]

[0302] From Table 1, it can be seen that Examples 1-1 to 1-6 using the modified polyester elastomer of the present invention having a titanium content of less than 250 wtppm exhibited high heat-resistant adhesiveness (retention rate) to the polyamide layer.

[0303] On the other hand, in Comparative Examples 1-1 to 1-3 using modified polyester elastomers having a titanium content of 250 wtppm or more, the heat-resistant adhesiveness was inferior.

[0304] In Table 1, the examples where the adhesiveness retention rate exceeded 100% are because the heat applied during the heat resistance test promoted the reaction and improved the adhesiveness.

[0305] [Example 2-1]

[0306] <Production of modified ethylene-vinyl alcohol copolymer (EVOH) composition and production of test piece>

[0307] 20 parts by mass of the particles of the adhesive polymer composition containing the modified polyester elastomer obtained in Example 1-1 and 80 parts by mass of ethylene-vinyl alcohol copolymer (EVOH) "SOARNOL (registered trademark) DC3203RB" manufactured by Mitsubishi Chemical Corporation were dry-blended and mixed, and kneaded and molded at a set temperature of 230°C using a multi-purpose small molding machine (Micro 15cc Twin Screw Compounder manufactured by RHEOLABO Co., Ltd.) to obtain a test piece for measuring the Izod impact strength and bending elastic modulus with a thickness of 4mm×width of 10mm×length of 80mm. Then, the test piece for measuring the Izod impact strength was notched using a notch forming tool (the size of the notch was referred to JIS K7110). The bending elastic modulus and Izod impact strength of the obtained test piece were measured.

[0308] Table 2 shows the above measurement results.

[0309] [Example 3-1]

[0310] <Production of modified polyamide polymer (PA) composition>

[0311] 5 parts by mass of the pellets of the adhesive polymer composition containing the modified polyester elastomer obtained in Example 1-1 and 95 parts by mass of polyamide (PA6) "Novamid (registered trademark) 1020" manufactured by DSM Japan Engineering Plastics Co., Ltd. were dry blended and mixed using a twin-screw extruder (manufactured by Ikegai Co., Ltd., PCM30, The mixture was melt-kneaded at a set temperature of 180 to 240° C., a screw speed of 200 rpm, and an extrusion rate of 10 kg / h, and pellets were obtained by strand cutting.

[0312] <Production of Test Specimens of Modified Polyamide-Based Polymer (PA) Composition>

[0313] The modified polyamide polymer (PA) composition obtained above was kneaded and molded by an injection molding machine (IS130GN-5A manufactured by Toshiba Machine Co., Ltd.) at an injection temperature of 260°C and a mold temperature of 80°C to prepare a test piece in the same manner as in Example 2-1. The flexural modulus and Izod impact strength of the obtained test piece were measured.

[0314] Table 2 shows the above measurement results.

[0315] [Example 2-2, Comparative Examples 2-1 to 2-3]

[0316] In the production of the modified ethylene-vinyl alcohol copolymer (EVOH) composition, a test piece of the modified ethylene-vinyl alcohol copolymer composition was obtained in the same manner as in Example 2-1 except that the formulation described in Table 2 was used, and the test pieces were measured.

[0317] [Comparative Examples 3-1 to 3-2]

[0318] In the production of the modified polyamide polymer (PA) composition, a test piece of the modified polyamide polymer (PA) composition was obtained in the same manner as in Example 3-1 except that the formulation described in Table 2 was used, and the test pieces were measured.

[0319] In addition, Table 2 also shows the color tone (particle YI) measured for each modified polyester elastomer.

[0320] [Table 2]

[0321]

[0322] According to Table 2, the modified ethylene-vinyl alcohol copolymer (EVOH) compositions of Examples 2-1 and 2, which are compounded with the modified polyester elastomer of the present invention having a titanium content of less than 250 wtppm, have improved flexibility compared to Comparative Example 2-3, which is not compounded with the modified polyester elastomer. In addition, the modified polyamide polymer (PA) composition of Example 3-1, which is compounded with the modified polyester elastomer of the present invention having a titanium content of less than 250 wtppm, has improved flexibility compared to Comparative Example 3-2, which is not compounded with the modified polyester elastomer.

[0323] In contrast, the modified ethylene-vinyl alcohol copolymer (EVOH) compositions of Comparative Examples 2-1 to 2 and the modified polyamide polymer (PA) composition of Comparative Example 3-1, which are formulated with modified polyester elastomers having a titanium content of 250 wtppm or more, have improved softness, but the color tone of the modified polyester elastomers is poor compared to that of Examples 2-1 to 2 and Example 3-1. Therefore, it is believed that the color tone of the modified ethylene-vinyl alcohol copolymer composition and the modified polyamide polymer (PA) composition is poor.

[0324] Although the present invention has been described in detail using specific embodiments, it will be apparent to one skilled in the art that various modifications can be made without departing from the spirit and scope of the present invention.

[0325] This application is based on Japanese Patent Application No. 2022-038261 filed on March 11, 2022 and Japanese Patent Application No. 2022-099720 filed on June 21, 2022, the entireties of which are incorporated herein by reference.

Claims

1. A modified polyester elastomer, which is a polyester polyether block copolymer composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol, modified by using an unsaturated carboxylic acid and / or its derivatives, wherein the modified polyester elastomer contains titanium, and the titanium content is less than 250wtppm.

2. The modified polyester elastomer according to claim 1, wherein The content of the polyalkylene ether glycol segment in the polyester polyether block copolymer is 5 to 90% by mass.

3. The modified polyester elastomer according to claim 1 or 2, wherein The modified polyester elastomer has an MFR of 1 to 300 g / 10 minutes, which is measured at 230° C. and a load of 2.16 kg in accordance with JIS K7210.

4. The modified polyester elastomer according to claim 1 or 2, wherein The density of the modified polyester elastomer is 1.00 to 1.35 g / cm 3 , the density is measured according to JIS K7112.

5. The modified polyester elastomer according to claim 1 or 2, wherein The melting point of the modified polyester elastomer is 145-245°C.

6. The modified polyester elastomer according to claim 1 or 2, wherein The JIS-D hardness of the modified polyester elastomer is 10 to 80, and the JIS-D hardness is measured according to JIS K6253.

7. The modified polyester elastomer according to claim 1 or 2, wherein The titanium content of the modified polyester-based elastomer is 20 wtppm or more.

8. The modified polyester elastomer according to claim 7, wherein The titanium content of the modified polyester-based elastomer is 20 wtppm to 248 wtppm.

9. A laminate comprising: a substrate layer, a layer consisting of the modified polyester elastomer according to claim 1 or 2 or an adhesive polymer composition containing the modified polyester elastomer, and a resin layer.

10. A method for producing a modified polyester elastomer, comprising the following steps: modifying a polyester elastomer obtained by polymerization in the presence of a titanium compound with an unsaturated carboxylic acid and / or a derivative thereof; The polyester elastomer is a polyester polyether block copolymer composed of a hard segment containing an aromatic polyester and a soft segment containing a polyalkylene ether glycol. The polyester elastomer has a titanium content of less than 250 wtppm.

11. The method for producing a modified polyester elastomer according to claim 10, wherein: The content of the polyalkylene ether glycol segment in the polyester polyether block copolymer is 5 to 90% by mass.

12. The method for producing a modified polyester elastomer according to claim 10 or 11, wherein: The acid value of the polyester elastomer is 32 eq / T or less.

13. The method for producing a modified polyester elastomer according to claim 10 or 11, wherein: The modification treatment is carried out in the presence of a free radical generator.

14. The method for producing a modified polyester elastomer according to claim 13, wherein: The blending ratio of the radical generator is 0.001 to 5 parts by mass based on 100 parts by mass of the polyester elastomer.

15. The method for producing a modified polyester elastomer according to claim 10 or 11, wherein: The modification treatment is performed by melt-kneading reaction.

16. A modifier comprising the modified polyester elastomer according to claim 1 or 2.

17. A polar polymer composition, comprising a polar polymer and a modified polyester elastomer as described in claim 1 or 2, wherein the content of the polar polymer is 70 to 99% by weight, and the content of the modified polyester elastomer is 1 to 30% by weight relative to the total of the polar polymer and the modified polyester elastomer, and the polar polymer comprises at least one selected from ethylene-vinyl alcohol copolymers and polyamide polymers.