Sweat-absorbent antibacterial sports bandage material and preparation method thereof
Through the combination of Tencel fiber, hemp fiber and functional copolymers, sweat-absorbent and antibacterial sports bandage materials are prepared, which solves the problems of poor sweat-absorbing ability and insufficient antibacterial stability of sports bandages, and achieves better wearing comfort and service life. extend.
Patent Information
- Application Number
- CN202410729447.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing sports bandages have poor sweat-absorbing ability during exercise, are prone to breed bacteria and produce odor, affect wearing comfort and antibacterial stability, and have a short service life.
Tencel fiber and hemp fiber combined with functional copolymer, zinc pyrithione, titanium dioxide quantum dots and sodium alginate are used to prepare sweat-absorbent and antibacterial sports bandage materials through free radical copolymerization and spinning technology to improve the material's sweat absorption, breathability and Antibacterial properties.
It significantly improves sweat absorption capacity, breathability and wearing comfort, enhances antibacterial stability, extends service life, has a simple process and is easy to operate, making it suitable for large-scale production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bandages, and in particular to a sweat-absorbing and antibacterial sports bandage material and a preparation method thereof. Background Art
[0002] Sports bandages are medical products that are usually worn during sports to fix or protect injured muscles, joints or ligaments. They are one of the effective means of protecting ankles, wrists, fingers and other parts that are prone to injury. They are usually made of elastic materials and provide lightweight and flexible support. Sports bandages help reduce pain, swelling and limited joint movement, while improving blood flow to the injured area and promoting the healing process. In addition, it can help athletes prevent re-injury, improve sports performance and reduce the risk of injury.
[0003] Sports bandages are widely used in various sports and fitness activities, such as football, basketball, running, etc. However, the sports bandages currently on the market have poor adsorption of a large amount of sweat during exercise, and are very likely to breed bacteria and produce odor after being soaked in sweat, which brings unpleasant feelings to people, and is also easy to cause skin allergies, affecting the quality of exercise.
[0004] In order to solve the above problems, the Chinese invention patent with authorization announcement number CN109125783B discloses a sweat-absorbing and antibacterial sports bandage, which is made of the following raw materials: chlorofiber 66-68, modified nylon 37-39, bamboo fiber 14-16, chitosan fiber 10-12, and carbon fiber 6-8; the sweat-absorbing and antibacterial sports bandage is flexible and elastic, can fit closely to the joints, play a full protective role, and can quickly absorb the water generated during exercise, with an antibacterial rate of 86.3%, which can effectively inhibit the odor caused by contact with the bandage, avoid mold, and extend the service life of the bandage; chlorofiber, bamboo fiber and 1 / 2 chitosan fiber are mixed and added to a titanium dioxide suspension for immersion. The mixture of multiple fibers can improve the elasticity and water absorption of the bandage, make it soft and skin-friendly, and enhance the protection of the joints. After the mixed fiber is soaked in the titanium dioxide suspension, the titanium dioxide can be evenly distributed between the fibers, thereby improving the smoothness and antibacterial properties of the fabric and avoiding the generation of odor after sweat absorption. However, its breathability, wearing comfort and antibacterial stability still need to be further improved.
[0005] It can be seen that the development of a sweat-absorbing and antibacterial sports bandage material with strong sweat absorption ability, good breathability and wearing comfort, excellent antibacterial and antibacterial stability, and long service life and its preparation method meet the market demand, have broad market value and application prospects, and are of great significance to promoting the development of the bandage material field. Summary of the invention
[0006] In view of the above problems, the object of the present invention is to provide a sweat-absorbing and antibacterial sports bandage material with strong sweat absorption ability, good air permeability and wearing comfort, excellent antibacterial and antibacterial stability, and long service life, and a preparation method thereof.
[0007] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: a sweat-absorbing and antibacterial sports bandage material is made of the following raw materials in percentage by weight: 20-30wt% of Tencel fiber, 15-20wt% of hemp fiber, and the balance is functional fiber; the functional fiber is made of the following components in parts by weight: 70-80 parts of functional copolymer, 3-5 parts of zinc pyrithione, 3-5 parts of titanium dioxide quantum dots, 1-2 parts of coupling agent, and 1-2 parts of sodium alginate; the functional copolymer includes the following monomers The structural unit introduced by free radical copolymerization: 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile.
[0008] Preferably, the Tencel fiber is Tencel A100.
[0009] Preferably, the hemp fiber is any one of hemp fiber, ramie fiber, crown fiber and abaca fiber.
[0010] Preferably, the preparation method of the functional copolymer comprises the following steps: adding 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, and an initiator to a high boiling point solvent, stirring and reacting at 60-70° C. in an inert gas atmosphere for 4-6 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying in a vacuum drying oven at 85-95° C. to constant weight to obtain a functional copolymer.
[0011] Preferably, the mass ratio of the 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, initiator, and high boiling point solvent is 3:(0.8-1.2):(2-4):2:(0.3-0.5):(0.08-0.12):(25-45).
[0012] Preferably, the initiator is azobisisobutyronitrile; and the high boiling point solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone.
[0013] Preferably, the inert gas is any one of nitrogen, helium, neon and argon.
[0014] Preferably, there is no special requirement for the source of the titanium dioxide quantum dots. In one embodiment of the present invention, the titanium dioxide quantum dots are prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN114085540B.
[0015] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0016] Preferably, the preparation method of the functional fiber comprises the following steps: after uniformly mixing the components except sodium alginate, adding them into a melt-blowing device, spraying them through small holes on a spinneret to obtain spun fibers, and then soaking the spun fibers in a sodium alginate aqueous solution at 50-65°C for 20-40h, taking them out, washing them with clean water, and drying them to obtain functional fibers.
[0017] Preferably, the mass percentage concentration of the sodium alginate aqueous solution is 5-10wt%.
[0018] Another object of the present invention is to provide a method for preparing the sweat-absorbing and antibacterial sports bandage material, comprising the following steps: cleaning and combing each raw material, and then subjecting the raw materials to the steps of drawing, roving and spinning to obtain blended yarn, and then weaving and finishing to obtain the sweat-absorbing and antibacterial sports bandage material.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The method for preparing the sweat-absorbing and antibacterial sports bandage material disclosed in the present invention has a simple process, convenient operation and control, no need for special equipment, and no need to modify the existing production line. It has low capital investment, low energy consumption, high preparation efficiency and finished product qualification rate, is suitable for continuous large-scale production, and has high promotion and application value.
[0021] (2) The sweat-absorbing and antibacterial sports bandage material disclosed in the present invention is made of the following raw materials in percentage by weight: 20-30wt% of Tencel fiber, 15-20wt% of hemp fiber, and the remainder of functional fiber; through the mutual cooperation and joint action of the raw materials, the advantages of each fiber raw material can be combined to give the sports bandage material product the advantages of strong sweat absorption ability, good air permeability and wearing comfort, good antibacterial and antibacterial stability, and long service life. The functional fiber is made of the following components by weight: 70-80 parts of functional copolymer, 3-5 parts of zinc pyrithione, 3-5 parts of titanium dioxide quantum dots, 1-2 parts of coupling agent, and 1-2 parts of sodium alginate; the functional copolymer includes the following monomers introduced by free radical copolymerization: 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl] ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile. Through the mutual cooperation between the components, the above-mentioned properties of the material are further improved; the use of titanium dioxide quantum dots can not only improve the softness and antibacterial properties of the product, avoid the generation of odor after sweat absorption, and improve the wearing comfort. The copolymer structure contains imidazole salts, amphoteric organic ion salts, cyano, trifluoromethylphenyl, amide, toluenesulfonyl, indole and carbonitrile. These groups and structures, under the multiple effects of electronic effect, steric effect and conjugation effect, make the manufactured products more sweat-absorbent, more breathable and comfortable to wear, more antibacterial and antibacterial stability, and longer service life.
[0022] (3) The sweat-absorbing and antibacterial sports bandage material disclosed in the present invention is prepared by first making the components other than sodium alginate into primary fibers, which are then immersed in a sodium alginate aqueous solution. Sodium alginate can undergo ion exchange with the imidazole salt on the primary fibers to form an ion cross-linked structure, thereby effectively improving the mechanical properties, antibacterial properties and wearing comfort of the bandage material. DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.
[0024] Example 1
[0025] A sweat-absorbing and antibacterial sports bandage material is made of the following raw materials in percentage by weight: 20wt% of tencel fiber, 15wt% of hemp fiber, and the balance is functional fiber; the functional fiber is made of the following components in percentage by weight: 70 parts of functional copolymer, 3 parts of zinc pyrithione, 3 parts of titanium dioxide quantum dots, 1 part of coupling agent, and 1 part of sodium alginate; the functional copolymer includes structural units introduced by free radical copolymerization of the following monomers: 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile.
[0026] The tencel fiber is tencel A100; the hemp fiber is hemp fiber.
[0027] The preparation method of the functional copolymer comprises the following steps: adding 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile and an initiator into a high boiling point solvent, stirring and reacting at 60° C. for 4 hours in an inert gas atmosphere, then precipitating in water, washing the precipitated polymer with ethanol for 3 times, and finally placing in a vacuum drying oven at 85° C. The functional copolymer is dried to constant weight to obtain the functional copolymer; the mass ratio of 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl] ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, initiator, and high boiling point solvent is 3:0.8:2:2:0.3:0.08:25; the initiator is azobisisobutyronitrile; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen. The M of the functional copolymer is measured by GPC test. n =15830 g / mol, M W / M n=1.319; calculated by elemental analysis and weight change, the mass ratio of the structural units introduced by 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile in the functional copolymer is 2.99:0.78:1.97:2:0.29.
[0028] The titanium dioxide quantum dots are prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN114085540B; the coupling agent is silane coupling agent KH550.
[0029] The preparation method of the functional fiber comprises the following steps: uniformly mixing the components except sodium alginate, adding the components into a melt-blowing device, spraying the components through small holes on a spinneret to obtain nascent fibers, and then immersing the nascent fibers in a sodium alginate aqueous solution at 50° C. for 20 hours, taking the components out, washing them with clean water, and drying them to obtain the functional fibers; the mass percentage concentration of the sodium alginate aqueous solution is 5wt%.
[0030] A method for preparing the sweat-absorbing and antibacterial sports bandage material comprises the following steps: cleaning and combing each raw material, and then subjecting the raw materials to drawing, roving and spinning processes to obtain blended yarn, and then weaving and finishing to obtain the sweat-absorbing and antibacterial sports bandage material.
[0031] Example 2
[0032] A sweat-absorbing and antibacterial sports bandage material is made of the following raw materials in percentage by weight: 23wt% of tencel fiber, 16wt% of hemp fiber, and the balance is functional fiber; the functional fiber is made of the following components in percentage by weight: 73 parts of functional copolymer, 3.5 parts of zinc pyrithione, 3.5 parts of titanium dioxide quantum dots, 1.2 parts of coupling agent, and 1.2 parts of sodium alginate; the functional copolymer includes structural units introduced by free radical copolymerization of the following monomers: 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile.
[0033] The tencel fiber is tencel A100; the hemp fiber is ramie fiber.
[0034] The preparation method of the functional copolymer comprises the following steps: adding 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile and an initiator into a high boiling point solvent, stirring and reacting at 62° C. for 4.5 hours in an inert gas atmosphere, then precipitating in water, washing the precipitated polymer with ethanol for 4 times, and finally drying in a vacuum drying oven at 87° C. to obtain a functional copolymer. Constant weight to obtain a functional copolymer; the mass ratio of 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, initiator, and high boiling point solvent is 3:0.9:2.5:2:0.35:0.09:30; the initiator is azobisisobutyronitrile; the high boiling point solvent is N,N-dimethylformamide; and the inert gas is helium.
[0035] The titanium dioxide quantum dots are prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN114085540B; the coupling agent is silane coupling agent KH560.
[0036] The preparation method of the functional fiber comprises the following steps: uniformly mixing the components except sodium alginate, adding the components into a melt-blowing device, spraying the components through small holes on a spinneret to obtain nascent fibers, and then immersing the nascent fibers in a sodium alginate aqueous solution at 55° C. for 25 hours, taking the components out, washing them with clean water, and drying them to obtain the functional fibers; the mass percentage concentration of the sodium alginate aqueous solution is 6wt%.
[0037] A method for preparing the sweat-absorbing and antibacterial sports bandage material comprises the following steps: cleaning and combing each raw material, and then subjecting the raw materials to drawing, roving and spinning processes to obtain blended yarn, and then weaving and finishing to obtain the sweat-absorbing and antibacterial sports bandage material.
[0038] Example 3
[0039] A sweat-absorbing and antibacterial sports bandage material is made of the following raw materials in percentage by weight: 25wt% of tencel fiber, 18wt% of hemp fiber, and the balance is functional fiber; the functional fiber is made of the following components in percentage by weight: 75 parts of functional copolymer, 4 parts of zinc pyrithione, 4 parts of titanium dioxide quantum dots, 1.5 parts of coupling agent, and 1.5 parts of sodium alginate; the functional copolymer includes structural units introduced by free radical copolymerization of the following monomers: 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile.
[0040] The tencel fiber is tencel A100; the hemp fiber is crown flax fiber.
[0041] The preparation method of the functional copolymer comprises the following steps: adding 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile and an initiator into a high boiling point solvent, stirring and reacting at 65° C. for 5 hours in an inert gas atmosphere, then precipitating in water, washing the precipitated polymer with ethanol for 5 times, and finally placing the polymer in a vacuum drying oven at 90° C. Dry to constant weight to obtain a functional copolymer; the mass ratio of the 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, initiator, and high boiling point solvent is 3:1:3:2:0.4:0.1:35; the initiator is azobisisobutyronitrile; the high boiling point solvent is N-methylpyrrolidone; and the inert gas is neon.
[0042] The titanium dioxide quantum dots are prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN114085540B; the coupling agent is silane coupling agent KH570.
[0043] The preparation method of the functional fiber comprises the following steps: uniformly mixing the components except sodium alginate, adding the components into a melt-blowing device, spraying the components through small holes on a spinneret to obtain nascent fibers, and then immersing the nascent fibers in a sodium alginate aqueous solution at 58° C. for 30 hours, taking the components out, washing them with clean water, and drying them to obtain the functional fibers; the mass percentage concentration of the sodium alginate aqueous solution is 8wt%.
[0044] A method for preparing the sweat-absorbing and antibacterial sports bandage material comprises the following steps: cleaning and combing each raw material, and then subjecting the raw materials to drawing, roving and spinning processes to obtain blended yarn, and then weaving and finishing to obtain the sweat-absorbing and antibacterial sports bandage material.
[0045] Example 4
[0046] A sweat-absorbing and antibacterial sports bandage material is made of the following raw materials in percentage by weight: 28wt% of tencel fiber, 19wt% of hemp fiber, and the balance is functional fiber; the functional fiber is made of the following components in percentage by weight: 78 parts of functional copolymer, 4.5 parts of zinc pyrithione, 4.5 parts of titanium dioxide quantum dots, 1.8 parts of coupling agent, and 1.8 parts of sodium alginate; the functional copolymer includes structural units introduced by free radical copolymerization of the following monomers: 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile.
[0047] The tencel fiber is tencel A100; the hemp fiber is abaca fiber.
[0048] The preparation method of the functional copolymer comprises the following steps: adding 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile and an initiator into a high boiling point solvent, stirring and reacting at 68° C. for 5.5 hours in an inert gas atmosphere, then precipitating in water, washing the precipitated polymer with ethanol for 5 times, and finally drying in a vacuum drying oven at 93° C. to constant weight to obtain the functional copolymer. The mass ratio of the 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, initiator, and high boiling point solvent is 3:1.1:3.5:2:0.45:0.11:43; the initiator is azobisisobutyronitrile; the high boiling point solvent is a mixture of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone in a mass ratio of 1:3:2; and the inert gas is argon.
[0049] The titanium dioxide quantum dots are made according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN114085540B; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570 in a mass ratio of 1:3:5.
[0050] The preparation method of the functional fiber comprises the following steps: uniformly mixing the components except sodium alginate, adding the components into a melt-blowing device, spraying the components through small holes on a spinneret to obtain nascent fibers, and then immersing the nascent fibers in a sodium alginate aqueous solution at 63° C. for 35 hours, taking the components out, washing them with clean water, and drying them to obtain the functional fibers; the mass percentage concentration of the sodium alginate aqueous solution is 9wt%.
[0051] A method for preparing the sweat-absorbing and antibacterial sports bandage material comprises the following steps: cleaning and combing each raw material, and then subjecting the raw materials to drawing, roving and spinning processes to obtain blended yarn, and then weaving and finishing to obtain the sweat-absorbing and antibacterial sports bandage material.
[0052] Example 5
[0053] A sweat-absorbing and antibacterial sports bandage material is made of the following raw materials in percentage by weight: 30wt% of tencel fiber, 20wt% of hemp fiber, and the balance is functional fiber; the functional fiber is made of the following components in percentage by weight: 80 parts of functional copolymer, 5 parts of zinc pyrithione, 5 parts of titanium dioxide quantum dots, 2 parts of coupling agent, and 2 parts of sodium alginate; the functional copolymer includes structural units introduced by free radical copolymerization of the following monomers: 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile.
[0054] The tencel fiber is tencel A100; the hemp fiber is hemp fiber.
[0055] The preparation method of the functional copolymer comprises the following steps: adding 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile and an initiator into a high boiling point solvent, stirring and reacting at 70° C. for 6 hours in an inert gas atmosphere, then precipitating in water, washing the precipitated polymer with ethanol for 6 times, and finally placing in a vacuum drying oven at 95° C. and dried to constant weight to obtain a functional copolymer; the mass ratio of 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, initiator, and high boiling point solvent is 3:1.2:4:2:0.5:0.12:45; the initiator is azobisisobutyronitrile; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen.
[0056] The titanium dioxide quantum dots are prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN114085540B; the coupling agent is silane coupling agent KH550.
[0057] The preparation method of the functional fiber comprises the following steps: uniformly mixing the components except sodium alginate, adding the components into a melt-blowing device, spraying the components through small holes on a spinneret to obtain nascent fibers, and then immersing the nascent fibers in a sodium alginate aqueous solution at 65° C. for 40 hours, taking the components out, washing them with clean water, and drying them to obtain the functional fibers; the mass percentage concentration of the sodium alginate aqueous solution is 10wt%.
[0058] A method for preparing the sweat-absorbing and antibacterial sports bandage material comprises the following steps: cleaning and combing each raw material, and then subjecting the raw materials to drawing, roving and spinning processes to obtain blended yarn, and then weaving and finishing to obtain the sweat-absorbing and antibacterial sports bandage material.
[0059] Comparative Example 1
[0060] A sweat-absorbing and antibacterial sports bandage material and a preparation method thereof, which are substantially the same as those in Example 1, except that functional fibers are used instead of hemp fibers, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile is not added.
[0061] Comparative Example 2
[0062] A sweat-absorbing and antibacterial sports bandage material and a preparation method thereof, which is basically the same as Example 1, except that titanium dioxide quantum dots, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt and N-vinyl caprolactam are not added.
[0063] In order to further illustrate the unexpected positive technical effects achieved by the products of each embodiment of the present invention, the sweat-absorbing and antibacterial sports bandage materials prepared in each example were subjected to relevant performance tests. The test results are shown in Table 1. The test method is as follows: 3 bandages of each of Examples 1-5 and Comparative Examples 1-2 were selected, each with a size of 5 cm×10 cm. The water absorption was measured with reference to the standard of GB / T22799-2009, and the sedimentation time (s) was recorded. The national standard GB / T20944.3-2008 "Evaluation of Antibacterial Properties of Textiles Part 3: Oscillation Method" was used to conduct quantitative antibacterial test, and the antibacterial rate of Escherichia coli of the bandages of the examples and comparative examples was tested before washing and after washing 50 times. The samples of the bandage materials to be tested (area of 2000mm 2 ) Tested by YG461H automatic air permeability instrument, the pressure difference is 100Pa, the test conditions are: temperature 20±2℃, humidity 65±2% constant temperature and humidity laboratory, the test reference standard is: GB / T5453-1997 "Determination of air permeability of fabrics".
[0064] Table 1
[0065] project Settling time(s) Antibacterial rate before washing (%) Antibacterial rate after 50 washes (%) Air permeability (mm / s) Example 1 16.4 98.9 98.5 1330 Example 2 16.0 99.2 98.9 1336 Example 3 15.8 99.4 99.2 1340 Example 4 15.5 99.5 99.4 1348 Example 5 15.0 99.9 99.8 1353 Comparative Example 1 17.2 97.5 96.7 1215 Comparative Example 2 18.0 98.0 97.0 1307
[0066] As can be seen from Table 1, the sweat-absorbing and antibacterial sports bandage material disclosed in the embodiment of the present invention has better water absorption performance, better antibacterial property and antibacterial stability, and better air permeability than the comparative example product. The combined use of hemp fiber, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, titanium dioxide quantum dots, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt and N-vinyl caprolactam is beneficial to improving the above properties.
[0067] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as described above. However, any technician familiar with the profession can make some changes, modifications and evolutions of the technical content disclosed above without departing from the scope of the technical solution of the present invention, which are all equivalent embodiments of the present invention. At the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A sweat-absorbing and antibacterial sports bandage material, characterized in that: The invention is made of the following raw materials in percentage by weight: 20-30wt% of tencel fiber, 15-20wt% of hemp fiber, and the balance is functional fiber; the functional fiber is made of the following components in percentage by weight: 70-80 parts of functional copolymer, 3-5 parts of zinc pyrithione, 3-5 parts of titanium dioxide quantum dots, 1-2 parts of coupling agent, and 1-2 parts of sodium alginate; the functional copolymer includes structural units introduced by free radical copolymerization of the following monomers: 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, and 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile.
2. The sweat-absorbing and antibacterial sports bandage material according to claim 1, characterized in that: The tencel fiber is tencel A100.
3. The sweat-absorbing and antibacterial sports bandage material according to claim 1, characterized in that: The hemp fiber is any one of hemp fiber, ramie fiber, crown fiber and abaca fiber.
4. The sweat-absorbing and antibacterial sports bandage material according to claim 1, characterized in that: The preparation method of the functional copolymer comprises the following steps: adding 1-allyl-3-methyl imidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium] propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile and an initiator into a high boiling point solvent, stirring and reacting for 4-6 hours at 60-70° C. in an inert gas atmosphere, then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying in a vacuum drying oven at 85-95° C. to constant weight to obtain the functional copolymer.
5. The sweat-absorbing and antibacterial sports bandage material according to claim 4, characterized in that: The mass ratio of the 1-allyl-3-methylimidazole chloride, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, N-vinyl caprolactam, 1-toluenesulfonyl-3-vinyl-1H-indole-5-carbonitrile, initiator, and high boiling point solvent is 3:(0.8-1.2):(2-4):2:(0.3-0.5):(0.08-0.12):(25-45).
6. The sweat-absorbing and antibacterial sports bandage material according to claim 4, characterized in that: The initiator is azobisisobutyronitrile; the high boiling point solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone; and the inert gas is any one of nitrogen, helium, neon, and argon.
7. The sweat-absorbing and antibacterial sports bandage material according to claim 1, characterized in that: The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.
8. The sweat-absorbing and antibacterial sports bandage material according to claim 1, characterized in that: The preparation method of the functional fiber comprises the following steps: uniformly mixing the components except sodium alginate, adding the components into a melt-blowing device, spraying the components through small holes on a spinneret to obtain nascent fibers, and then soaking the nascent fibers in a sodium alginate aqueous solution at 50-65° C. for 20-40 hours, taking the components out, washing them with clean water, and drying them to obtain the functional fibers.
9. The sweat-absorbing and antibacterial sports bandage material according to claim 8, characterized in that: The mass percentage concentration of the sodium alginate aqueous solution is 5-10wt%.
10. A method for preparing the sweat-absorbing and antibacterial sports bandage material according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: cleaning and combing the raw materials respectively, and then preparing the blended yarn through drawing, roving and spun spinning processes; and then obtaining the sweat-absorbing and antibacterial sports bandage material through weaving and finishing.
Citation Information
Cited By
Soft hydrophilic contact lens and material, preparation method and application thereof
CN121022013A