Method for reducing hot rolling roll sticking defect of ferritic stainless steel
By controlling the equiaxed grain ratio, hot rolling finishing temperature and roll conditions, combined with emulsion lubrication and cooling management, the problem of roll sticking defects in hot rolling of ferritic stainless steel is solved, linear roughness is significantly reduced, and product quality is improved. and yield.
Patent Information
- Application Number
- CN202410976774.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Ferritic stainless steel often suffers from roll sticking defects during the hot rolling process, resulting in linear roughness on the surface and affecting product quality and output.
By controlling the equiaxed crystal ratio, hot rolling finishing temperature, roll material, emulsion lubrication and roll temperature, adjusting the rolling speed and deformation rate, combined with electromagnetic stirring and cooling water management, the occurrence of roll sticking defects can be reduced.
It effectively reduces the defective rate of linear roughness on the surface of ferritic stainless steel from 3.2% to 0.8%, improving product quality and output.
Smart Images

Figure CN118751684A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of metallurgy and stainless steel production, and in particular to a method for reducing the hot-rolling sticking defect of ferrite stainless steel. Background Art
[0002] Ferritic stainless steel is a stainless steel material with excellent corrosion resistance and mechanical properties, and is widely used in the fields of petroleum, chemical industry, electric power, shipbuilding, etc. However, during the hot rolling process, due to the influence of factors such as rolling temperature, rolling speed and rolling pressure, the sticking defect often occurs, forming linear roughness on the surface of the strip. In severe cases, the iron oxide scales in the linear roughness are not easy to be cleaned by hot wire pickling, resulting in iron scales remaining after hot wire washing, and iron scales pressed into the surface after cold rolling. Therefore, how to reduce the sticking defect of ferritic stainless steel hot rolling has become an urgent problem to be solved.
[0003] The invention discloses a method for reducing the hot rolling sticking defect of ferritic stainless steel. The method effectively reduces the occurrence of the sticking defect and improves the quality and output of the product by adjusting the hot rolling temperature, rolling speed and rolling pressure, and controlling the cooling speed and time. Summary of the invention
[0004] The purpose of the present invention is to provide a method for reducing the sticking roller defect of ferritic stainless steel hot rolling in view of the above problems.
[0005] The object of the present invention is achieved as follows: A method for reducing the sticking defects of ferritic stainless steel hot rolling, comprising the following aspects: (1) controlling the equiaxed crystal ratio: the equiaxed crystal ratio is controlled between 45-55%. On the one hand, electromagnetic stirring is used during the continuous casting process, and on the other hand, the hot rolling finishing temperature is controlled as follows: the finishing inlet temperature is 1050-1080°C, and the final rolling temperature is 900-940°C, so that the finishing process is located in the austenite-ferrite two-phase region; (2) roller material selection: ensure that the working rollers of the last two to three racks of the continuous rolling unit use M2 high-speed steel rollers; (3) use emulsion for roller gap lubrication: the emulsion needs to be evenly covered on the roller surface, the emulsion concentration is 5-8%, the water pressure is 3-5 bar, and the total flow rate is 50-100m 3 / h; (4) Strictly control the roll temperature: the roll temperature of the first three stands F1-F3: 300-400℃, the middle two stands: F4-F5: 250-300℃, the last two stands F6-F7: 200-280℃, the inlet and outlet cooling water flow rate is controlled at 5000-8000m 3 / h, water pressure: 1-2bar; (5) Control the rolling speed and deformation rate of each pass: the rolling speed is 1.2-2.0m / s, the deformation rate of the first stand of finishing rolling is 40-50%, the deformation rate of the second and third stands is 30-40%, the deformation rate of the fourth and fifth stands is 20-30%, the deformation rate of the sixth stand is 20-25%, and the deformation rate of the seventh stand is 15-20%.
[0006] (1) The current of medium electromagnetic stirring is 1650-1800A, the stirring frequency is 4.5-6.0HZ, and the electromagnetic stirring switching time is 50-60 seconds.
[0007] The beneficial effect of the present invention is that the linear roughness on the surface of ferritic stainless steel caused by hot rolling roller sticking is significantly reduced by the above method, and the linear roughness non-conformity rate is reduced from 3.2% to 0.8%, with a reduction of 75%. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] The present invention will be further described below in conjunction with the accompanying drawings.
[0009] Figure 1 It is the equilibrium phase diagram of ferrite and austenite of the present invention.
[0010] Figure 2 This is a diagram showing the sticking of rollers made of different materials during hot rolling. DETAILED DESCRIPTION
[0011] The present invention proposes a method for reducing the sticking defect of ferritic stainless steel during hot rolling. The method mainly includes the following schemes: 1. Controlling the equiaxed crystal ratio: To ensure that the ferritic stainless steel does not stick to the roller during hot rolling, the equiaxed crystal ratio is generally controlled between 45-55%. On the one hand, electronic stirring must be used during the continuous casting process, the electromagnetic stirring current: 1650-1800A, the stirring frequency: 4.5-6.0HZ, the electromagnetic stirring reversing time: 50-60 seconds, on the other hand, in order to obtain more equiaxed crystal structure, it is also necessary to control a reasonable hot rolling finishing temperature.
[0012] According to the equilibrium phase diagram, the hot rolling finishing mill process is formulated as follows: the finishing rolling inlet temperature is 1050-1080℃, and the final rolling temperature is 900-940℃. The finishing rolling process is located in the austenite-ferrite two-phase region, with high elongation and easy rolling.
[0013] 2. Roller material selection: Tests show that the material of the hot rolling work roll has a significant impact on hot rolling roll sticking. Figure 2 It can be seen that after the rolling time exceeds 10 minutes, the sticking degree of M2 high-speed steel roll is the lightest. Therefore, in order to ensure the surface quality of the strip, at least the working rolls of the last two to three stands of the continuous rolling mill should be made of M2 high-speed steel rolls.
[0014] 3. Use emulsion to lubricate the roll gap. The emulsion evenly covers the roll surface, which can reduce friction and heat during rolling, and reduce the adhesion between the material and the roll, effectively preventing the roll from sticking. The emulsion concentration is generally controlled at 5-8%, the water pressure is 3-5 bar, and the total flow rate is 50-100m 3 / h.
[0015] 4. Strictly control the temperature of the rolls. If the temperature of the rolls is too high, the oxide film on the surface of the rolls will melt, accelerate the wear of the rolls, affect the plate shape control during the rolling process, and even cause problems such as sticking steel and breaking the steel strip. If the temperature of the rolls is too low, the friction coefficient will increase during the rolling process, which will increase the rolling torque, easily cause mill vibration, and affect the stability of the rolling process. To ensure a good strip surface, the roll temperature of the first three stands F1-F3: 300-400℃, the middle two stands: F4-F5: 250-300℃, the last two stands F6-F7: 200-280℃, and the inlet and outlet cooling water flow rate is controlled at 5000-8000m 3 / h, water pressure: 1-2bar.
[0016] 5. Control the rolling speed and deformation rate of each pass: Control the rolling speed within the range of 1.2m / S to 2.0m / S to ensure uniform temperature distribution of steel during rolling and reduce the sticking phenomenon caused by local overheating. The deformation rate of the first stand of finishing rolling is 40-50%, the deformation rate of the second and third stands is 30-40%, the deformation rate of the fourth and fifth stands is 20-30%, the deformation rate of the sixth stand is 20-25%, and the deformation rate of the seventh stand is 15-20%. This deformation rate design can ensure uniform deformation of steel during rolling and reduce the sticking phenomenon caused by stress concentration. Embodiment 1
[0017] Steel type: SUS430, continuous casting billet thickness: 200mm, hot rolling thickness: 3.0mm.
[0018] 1. Electromagnetic stirring is used in continuous casting, with electromagnetic stirring current of 1700A, stirring frequency of 5.0HZ, electromagnetic stirring reversing time of 50 seconds, hot rolling finishing inlet temperature of 1075℃, final rolling temperature of 930℃, and equiaxed grain ratio of more than 48%.
[0019] The working rolls of the last three stands F5, F6 and F7 of the 2.7-stand finishing mill are made of M2 high-speed steel rolls.
[0020] 3. All finishing mills use emulsion for roll gap lubrication, with an emulsion concentration of 6.5%, a water pressure of 5 bar, and a total flow rate of 90m 3 / h.
[0021] 4. The working roll temperature, cooling water flow rate and cooling water pressure of each stand of the finishing mill are controlled as shown in the following table.
[0022]
[0023] Effect: Through the above method, the linear roughness on the surface of ferritic stainless steel caused by hot rolling roller sticking is significantly reduced, and the linear roughness non-conformity rate is reduced from 3.2% to 0.6%. Embodiment 2
[0024] Steel type: SUS430, continuous casting billet thickness: 200mm, hot rolling thickness: 5.0mm.
[0025] 1. Electromagnetic stirring is used in continuous casting, with electromagnetic stirring current of 1650A, stirring frequency of 6.0HZ, electromagnetic stirring reversing time of 55 seconds, hot rolling finishing inlet temperature of 1070℃, final rolling temperature of 935℃, and equiaxed grain ratio of more than 50%.
[0026] The working rolls of the last three stands F5, F6 and F7 of the 2.7-stand finishing mill are made of M2 high-speed steel rolls.
[0027] 3. All finishing mills use emulsion for roll gap lubrication, with an emulsion concentration of 6.0%, a water pressure of 4.0 bar, and a total flow of 82m 3 / h.
[0028] 4. The working roll temperature, cooling water flow rate and cooling water pressure of each stand of the finishing mill are controlled as shown in the following table.
[0029]
[0030] Effect: Through the above method, the linear roughness on the surface of ferritic stainless steel caused by hot rolling roller sticking is significantly reduced, and the linear roughness non-conformity rate is reduced from 3.2% to 0.2%.
[0031] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.
Claims
1. A method for reducing the sticking defect of ferritic stainless steel hot rolling, Features: These include: (1) Controlling the equiaxed crystal ratio: The equiaxed crystal ratio is controlled between 45-55%. On the one hand, electromagnetic stirring is used during the continuous casting process, and on the other hand, the hot rolling and finishing temperatures are controlled as follows: the finishing rolling inlet temperature is 1050-1080°C, and the final rolling temperature is 900-940°C, so that the finishing rolling process is in the austenite-ferrite two-phase region; (2) Roller material selection: Ensure that the working rolls of the last two to three stands of the continuous rolling mill are made of M2 high-speed steel rolls; (3) Use emulsion for roll gap lubrication: The emulsion needs to be evenly covered on the roll surface, the emulsion concentration is 5-8%, the water pressure is 3-5 bar, and the total flow rate is 50-100m 3 / h; (4) Strictly control the roller temperature: the roller temperature of the first three stands F1-F3: 300-400℃, the middle two stands: F4-F5: 250-300℃, the last two stands F6-F7: 200-280℃, the inlet and outlet cooling water flow rate is controlled at 5000-8000m 3 / h, water pressure: 1-2bar; (5) Control the rolling speed and deformation rate of each pass: the rolling speed is 1.2-2.0 m / s, the deformation rate of the first stand of finishing rolling is 40-50%, the deformation rate of the second and third stands is 30-40%, the deformation rate of the fourth and fifth stands is 20-30%, the deformation rate of the sixth stand is 20-25%, and the deformation rate of the seventh stand is 15-20%.
2. A method for reducing the sticking defect of ferritic stainless steel hot rolling according to claim 1, Features: (1) The current of medium electromagnetic stirring is 1650-1800A, the stirring frequency is 4.5-6.0HZ, and the electromagnetic stirring switching time is 50-60 seconds.
Citation Information
Patent Citations
Method for preventing surface oxide film of nichrome roller from being peeling-off
CN101003053A
Anti-wrinkle ferritic stainless steel with low cost and production method thereof
CN102534409A
Ferrite stainless steel with good polishing performance and manufacturing method thereof
CN103741053A
Method for reducing defect of being attached to roller of medium-high-chromium ultra-pure ferrite stainless steel during hot rolling
CN109550793A
430 ferritic stainless steel and production process thereof
CN113462967A