Low-temperature grinding wheel abrasive particle finishing method, system and device based on hydroxyl modification

Through the hydroxyl-modified low-temperature grinding wheel abrasive dressing method, hydroxyl dehydration and condensation reaction is used for atomic-level removal, which solves the problem of resin-based sintered grinding wheel dressing and achieves higher surface smoothness and lower roughness.

CN118752415AActive Publication Date: 2024-10-11SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY

Patent Information

Application Number
CN202410953165.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-11
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing grinding wheel dressing technology is difficult to effectively dress resin-based sintered grinding wheels, especially when maintaining surface quality and removing diamond abrasive grains.

Method used

A low-temperature grinding wheel abrasive dressing method based on hydroxyl modification is adopted. By controlling the hydroxyl radical injection on the polishing disc and the relative movement of the grinding wheel, the hydroxyl dehydration condensation reaction is used to remove material layer by layer at the atomic level to realize the dressing of the resin-based sintered grinding wheel. .

Benefits of technology

It achieves lower roughness and higher smoothness on the surface of the resin-based sintered grinding wheel, and improves the processing quality of the diamond surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118752415A_ABST
    Figure CN118752415A_ABST
Patent Text Reader

Abstract

The invention provides a low-temperature grinding wheel abrasive particle finishing method, system and device based on hydroxyl modification, and the method comprises the steps that a polishing disc is controlled to rotate, and hydroxyl free radicals are sprayed on the polishing disc, so that a modified layer is formed on the polishing disc; and the grinding wheel to be trimmed is controlled to rotate and abut against the modified layer on the polishing disc, so that the abutting face is subjected to a hydroxyl dehydration condensation reaction, and the part, subjected to the hydroxyl dehydration condensation reaction, on the grinding wheel is trimmed in an atomic-scale layer-by-layer material removal mode under the mechanical shearing action generated by relative movement of the grinding wheel and the polishing disc. According to the method, mixed gas of argon and water vapor is used, microwave plasmas are excited in a low-temperature mode, micro-removal of diamond is achieved through small mechanical force, then finishing of the resin-based sintered grinding wheel is achieved, the diamond is removed in an atomic-scale layer-by-layer removal mode, and the quality of the resin-based sintered grinding wheel is improved. The surface of the resin-based sintered grinding wheel can achieve lower roughness, and higher smoothness of the diamond surface is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grinding wheel dressing, and in particular to a hydroxyl-modified low-temperature grinding wheel abrasive dressing method, system and device. Background Art

[0002] In the process of precision grinding, stable surface processing quality depends on the cutting edge state of the diamond abrasive grains on the grinding wheel. Therefore, the key to achieving high surface processing quality grinding lies in controlling the cutting edge morphology of the diamond abrasive grains. The existing steps for controlling the cutting edge morphology of diamond abrasive grains include sharpening and dressing. Sharpening can make the diamond abrasive grains cut, and dressing can change the cutting edge morphology of the diamond abrasive grains. Existing grinding wheel dressing technologies include mechanical grinding and dressing, laser dressing and discharge-assisted dressing. Mechanical grinding and dressing is a mechanical dressing technology that uses a high-speed rotating dressing wheel to perform thermochemical grinding and removal of the cutting edge of the diamond abrasive grains; laser dressing is to inject the laser beam along the tangent direction of the grinding wheel surface and use continuous high-temperature thermochemical removal of diamond abrasive grains; discharge-assisted dressing is to use the chips and the binder to form a discharge gap to generate pulse discharge. The discharge heat is transferred to the cutting edge of the abrasive grain and coupled with the cutting heat to cause the surface temperature to rise, forming a graphitized layer that is removed under the action of the cutting force.

[0003] Compared with electroplated grinding wheels and metal-based sintered grinding wheels, resin-based sintered grinding wheels have a softer bond and higher elasticity, and are usually used in the last process of grinding to obtain better surface quality. However, the melting point of the bond of resin-based sintered grinding wheels is low and the abrasive particles are easy to fall off. There is currently no method for dressing resin-based sintered grinding wheels. Summary of the invention

[0004] In view of this, the present invention proposes a method, system and device for dressing low-temperature grinding wheels based on hydroxyl modification, and the specific scheme is as follows:

[0005] In the first part, the present application proposes a low-temperature grinding wheel abrasive dressing method based on hydroxyl modification, comprising:

[0006] Controlling the rotation of the polishing disc and controlling the spraying of hydroxyl radicals on the polishing disc so that a low-temperature modified layer is formed in the sprayed area on the polishing disc;

[0007] The grinding wheel to be dressed is controlled to rotate, and the grinding wheel is made to abut against the modified layer on the polishing disk, so that a hydroxyl dehydration condensation reaction occurs on the contact surface of the grinding wheel abutting against the modified layer, and under the mechanical shearing action generated by the relative movement of the grinding wheel and the polishing disk, the part of the grinding wheel where the hydroxyl dehydration condensation reaction occurs is dressed by removing material layer by layer at the atomic level.

[0008] In a specific embodiment, the polishing disk comprises: a flat polishing disk; and the “controlling the spraying of hydroxyl radicals on the polishing disk” comprises:

[0009] The hydroxyl radicals are controlled to be sprayed on the plane polishing surface of the polishing disk; the distance between the spraying position of the substance on the plane polishing surface and the rotation center of the polishing disk is equal to the distance from the grinding wheel to the rotation center.

[0010] In a specific embodiment, the shape of the polishing disc includes a truncated cone shape, and the rotation center axis of the polishing disc is the center axis of the truncated cone;

[0011] The “controlling the spraying of hydroxyl radicals on the polishing disc” includes: controlling the spraying of hydroxyl radicals on the side of the truncated cone-shaped polishing disc;

[0012] The step of "making the grinding wheel abut against the modified layer on the polishing disk" includes: making the surface to be trimmed on one side of the grinding wheel abut against the modified layer on one side of the truncated cone-shaped polishing disk; if the surface to be trimmed on one side of the grinding wheel is trimmed, making the surface to be trimmed on the other side of the grinding wheel abut against the modified layer on the other side of the truncated cone-shaped polishing disk.

[0013] In a specific embodiment, the rotation direction of the polishing disc is the same as the rotation direction of the grinding wheel.

[0014] In one specific embodiment, the polishing disk comprises a rigid polishing disk;

[0015] The modified layer has a hardness lower than a hardness of a remaining portion of the polishing pad excluding the modified layer.

[0016] In a specific embodiment, "making the grinding wheel abut against the modified layer on the polishing disk" includes: applying a preset load force to the grinding wheel so that the grinding wheel abuts against the modified layer on the polishing disk; the preset load force ranges from 1N to 4N.

[0017] In a specific embodiment, the method for generating the hydroxyl radicals includes microwave plasma, and the generation of the hydroxyl radicals is obtained by exciting a mixed gas of water vapor and argon through the microwave plasma.

[0018] In a specific embodiment, the method further includes: exciting the microwave plasma by preset microwave power so that the temperature acting on the grinding wheel is lower than the melting point of a bonding agent used for bonding abrasive grains in the grinding wheel;

[0019] The preset microwave power ranges from 150w to 225w.

[0020] In the second part, the present application proposes a hydroxyl-modified low-temperature grinding wheel abrasive dressing system, comprising:

[0021] A control module, used for controlling the rotation of the polishing disc and controlling the spraying of hydroxyl radicals on the polishing disc, so that a low-temperature modified layer is formed in the sprayed area on the polishing disc;

[0022] The dressing module is used to control the rotation of the grinding wheel to be dressed and make the grinding wheel abut against the modified layer on the polishing disk, so that the contact surface of the grinding wheel abutting against the modified layer undergoes hydroxyl dehydration condensation reaction, and under the mechanical shearing action generated by the relative movement of the grinding wheel and the polishing disk, the part of the grinding wheel undergoing hydroxyl dehydration condensation reaction is dressed by removing material layer by layer at the atomic level.

[0023] In the third part, the present application proposes a low-temperature grinding wheel abrasive dressing device based on hydroxyl modification, which is used to perform the above-mentioned low-temperature grinding wheel abrasive dressing method based on hydroxyl modification, and the device includes: a polishing disc, a movable clamp, a plasma torch tube for spraying microwave plasma and a driving unit; the plasma torch tube is provided with a nozzle facing the polishing disc, and the driving unit drives and connects the polishing disc and the movable clamp respectively, and is used to control the relative movement of the polishing disc and the movable clamp; the movable clamp is used to control the grinding wheel to be dressed to abut against the polishing disc.

[0024] Beneficial effects:

[0025] The present invention uses a mixed gas of argon and water vapor to excite microwave plasma at low temperature, so as to achieve micro-removal of diamond with a small mechanical force, thereby achieving the dressing of the resin-based sintered grinding wheel. In addition, the diamond is removed layer by layer at the atomic level, so that the surface of the resin-based sintered grinding wheel can achieve a lower roughness and a higher smoothness of the diamond surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a flow chart of a method for dressing low-temperature grinding wheels based on hydroxyl modification according to an embodiment of the present invention;

[0027] Figure 2 is a structural diagram of a low-temperature grinding wheel abrasive dressing system based on hydroxyl modification according to an embodiment of the present invention;

[0028] Figure 3 is a schematic diagram of a grinding wheel abrasive dressing device according to an embodiment of the present invention;

[0029] Figure 4 is a cross-sectional view of a truncated cone-shaped polishing disc according to an embodiment of the present invention;

[0030] Figure 5 1 is a schematic diagram of a process of a low-temperature grinding wheel abrasive dressing method based on hydroxyl modification according to an embodiment of the present invention;

[0031] Figure 6Schematic diagram of characteristic spectrum excited by plasma before and after water vapor is introduced into the plasma according to an embodiment of the present invention;

[0032] Figure 7 is a graph showing the relationship between microwave plasma power and temperature according to an embodiment of the present invention;

[0033] Figure 8 is a schematic diagram of the morphology of a resin-based sintered grinding wheel before microwave plasma dressing according to an embodiment of the present invention;

[0034] Fig. 9 is a schematic diagram of the morphology of a resin-based sintered grinding wheel after microwave plasma dressing according to an embodiment of the present invention;

[0035] Fig.10 is a 3D schematic diagram of a resin-based sintered grinding wheel according to an embodiment of the present invention before being dressed by microwave plasma;

[0036] Fig.11 is a 3D schematic diagram of a resin-based sintered grinding wheel after microwave plasma dressing according to an embodiment of the present invention;

[0037] Fig.12 Schematic diagram of the contours of a plurality of abrasive grains after the resin-based sintered grinding wheel is dressed in an embodiment of the present invention;

[0038] Fig.13 is a schematic diagram of diamond shedding analysis of a resin-based sintered grinding wheel before dressing under maximum load according to an embodiment of the present invention;

[0039] Fig.14 It is a schematic diagram of diamond shedding analysis of the resin-based sintered grinding wheel according to an embodiment of the present invention after dressing under maximum load.

[0040] Figure numerals: 1-polishing disc; 2-grinding wheel; 3-modified layer; 4-movable fixture; 5-plasma torch; 6-driving unit; 7-control module; 8-dressing module. DETAILED DESCRIPTION

[0041] In the following, various embodiments of the present disclosure will be described more fully. The present disclosure may have various embodiments, and adjustments and changes may be made therein. However, it should be understood that there is no intention to limit the various embodiments of the present disclosure to the specific embodiments disclosed herein, but the present disclosure should be understood to cover all adjustments, equivalents and / or alternatives that fall within the spirit and scope of the various embodiments of the present disclosure.

[0042] The terms used in the various embodiments disclosed in the present invention are only used for the purpose of describing specific embodiments and are not intended to limit the various embodiments disclosed in the present invention. As used herein, the singular form is intended to also include the plural form, unless the context clearly indicates otherwise. Unless otherwise specified, all terms used herein (including technical terms and scientific terms) have the same meaning as the meanings commonly understood by ordinary technicians in the field of the various embodiments disclosed in the present invention. The terms (such as the terms defined in the generally used dictionary) will be interpreted as having the same meaning as the contextual meaning in the relevant technical field and will not be interpreted as having an idealized meaning or an overly formal meaning, unless clearly defined in the various embodiments disclosed in the present invention.

[0043] Example 1

[0044] The present invention uses a mixed gas of argon and water vapor to excite microwave plasma at low temperature, so as to achieve micro-removal of diamonds with a small mechanical force, thereby achieving the dressing of the resin-based sintered grinding wheel. In addition, the diamonds are removed layer by layer at the atomic level, so that the surface of the resin-based sintered grinding wheel can achieve a lower roughness and a higher smoothness of the diamond surface. The specific scheme is as follows:

[0045] The method mentioned in this embodiment is a method for dressing abrasive grains of a grinding wheel 2 based on hydroxyl modification, as shown in the attached Figure 1 -Attached Figure 3 As shown, including:

[0046] 101. Control the rotation of the polishing disc 1 and control the spraying of hydroxyl radicals on the polishing disc 1, so that the sprayed area on the polishing disc 1 forms a low-temperature modified layer 3. This embodiment adopts an advanced grinding wheel dressing technology, in which the key steps include controlling the rotation of the polishing disc 1 and spraying hydroxyl radicals thereon.

[0047] Specifically, as attached Figure 3 As shown, the grinding wheel 2 sample is pressed against the polishing disc under the action of the load force F, and the microwave plasma source rich in hydroxyl radicals (OH) is ejected from the plasma torch 5 at a preset flow rate, irradiated on the surface of the polishing disc 1 and chemically reacted, forming a modified layer with low hardness and low temperature on the surface of the polishing disc 1. In this embodiment, the grinding wheel is a resin-based sintered grinding wheel, and the low temperature range is room temperature (20°-25°)-the melting point of the resin binder (250°). The temperature during the dressing process is lower than the melting point of the resin binder, which can achieve effective dressing of the resin-based sintered grinding wheel. In practical applications, the rotation speed and direction of the polishing disc 1 can be accurately controlled to ensure that the ejected microwave plasma can evenly cover its surface, so as to form a uniform and high-quality modified layer 3.

[0048] In this embodiment, the method of generating hydroxyl radicals includes microwave plasma. Hydroxyl radicals are highly active chemical substances that can react chemically with the material on the surface of the polishing disc 1, thereby changing the chemical properties of the surface. During the spraying process, the spraying intensity, temperature, concentration and other parameters of the microwave plasma can also be closely monitored to ensure that it can form a uniform modified layer 3 on the surface of the polishing disc 1.

[0049] 102. The grinding wheel 2 to be dressed is controlled to rotate, and the grinding wheel 2 is made to abut against the modified layer 3 on the polishing disc 1, so that the contact surface of the grinding wheel 2 abutting against the modified layer 3 undergoes a hydroxyl dehydration condensation reaction, and the portion of the grinding wheel 2 undergoing the hydroxyl dehydration condensation reaction is dressed by removing material layer by layer at the atomic level under the mechanical shearing action generated by the relative movement of the grinding wheel 2 and the polishing disc 1. In order to achieve the dressing of the grinding wheel 2, this embodiment also includes precise control and interaction between the grinding wheel 2 and the polishing disc 1.

[0050] Specifically, the grinding wheel 2 to be dressed is controlled to rotate stably and accurately while the polishing disc 1 is controlled to rotate. The polishing disc 1 and the grinding wheel 2 rotate in the same direction at speeds Vp and Vd respectively, and the modified layer 3 rotates to the grinding wheel dressing area through the polishing disc 1. The plasma irradiation area and the grinding wheel dressing area are at the same distance from the center of the rotating disc, that is, the distance between the plasma irradiation area and the grinding wheel dressing area is the same. Figure 3 In the figure, r1=r2, thus ensuring that the grinding wheel dressing area is exactly the modified layer area. Highly active hydroxyl radicals attach to polishing disc 1 and grinding wheel 2, and form bonds with specific atoms of the two to produce a modification effect, and then a hydroxyl dehydration condensation reaction CD-OH+M-OH→CD-O-M+H2O (CD refers to the carbon atoms on the surface of grinding wheel 2 modified by hydroxyl groups, and M refers to the atoms on the surface of polishing disc 1 modified by hydroxyl groups) can occur at the interface between the two, forming a new bond CD-OM on the interface. Under the mechanical shearing action, CD-CD on the surface of grinding wheel 2 breaks. Under the mechanical shearing action generated by the relative movement of grinding wheel 2 and polishing disc 1, the part where hydroxyl dehydration condensation reaction occurs will be dressed in a layer-by-layer material removal manner at the atomic level. Since the raised part of the surface of grinding wheel 2 is easier to capture hydroxyl radicals and has a higher material removal rate, its surface flatness will eventually approach that of polishing disc 1, thereby achieving global flattening of grinding wheel 2.

[0051] It should be noted that the microwave plasma here acts on the polishing disc 1, and the hydroxyl radicals on the grinding wheel 2 are brought to the grinding wheel dressing area by the rotation of the polishing disc 1, rather than the microwave plasma directly acting on the grinding wheel abrasive, thereby ensuring that the surface grinding performance of the grinding wheel 2 will not change.

[0052] Specifically, a 100# resin-based sintered grinding wheel was used, and a microwave power of 200W was used with a 1N load, and a hydroxyl-containing plasma (8slm argon, 140sccm water vapor) was introduced, and the grinding wheel 2 rotated at 60rpm and the polishing disk 1 rotated at 200rpm for 30 minutes. The experimental results are shown in the attached figure. Figure 8 -Attached Fig.12 As shown in the figure, diamond on the surface of grinding wheel 2 can be significantly removed after microwave plasma processing, and the 3D image also shows that the morphology before and after dressing changes greatly. Fig.12 As shown, by drawing a line through multiple diamond grains in the 3D image, it can be seen that the top surfaces of different diamonds are flush, and high performance between multiple grains is guaranteed.

[0053] In a specific embodiment, the polishing disc 1 comprises: a flat polishing disc 1; and “controlling the spraying of hydroxyl radicals on the polishing disc 1” comprises:

[0054] The hydroxyl radicals are controlled to be sprayed on the plane polishing surface of the polishing disc 1; the distance between the spraying position of the sprayed material on the plane polishing surface and the rotation center of the polishing disc 1 is equal to the distance between the grinding wheel 2 and the rotation center.

[0055] As attached Figure 3 As shown, the polishing disc 1 of this embodiment can adopt a planar polishing disc structure. This design ensures the flatness and uniformity of the polishing disc surface and provides a stable foundation for the subsequent grinding wheel dressing process.

[0056] When the step of "controlling the spraying of hydroxyl radicals on the polishing disc 1" is performed, the material is precisely controlled to be sprayed on the planar polishing surface of the polishing disc 1 to ensure that the sprayed plasma can evenly cover the entire polishing surface.

[0057] In order to ensure the best interaction between the grinding wheel 2 and the polishing disc 1, the injection position of the substance is further adjusted. Specifically, the distance between the injection position of the substance on the flat polishing surface and the rotation center of the polishing disc 1 is equal to the distance between the grinding wheel 2 and the rotation center. This design ensures that during the rotation of the grinding wheel 2, its surface and the modified layer 3 on the polishing disc 1 can always maintain a constant distance and contact area, thereby achieving more uniform and efficient grinding wheel dressing.

[0058] Through this precise control and adjustment, not only can the grinding wheel 2 be accurately dressed, but also the dressing efficiency and quality can be maximized. This grinding wheel dressing technology is not only applicable to resin-based sintered grinding wheels, but can also be applied to other types of grinding wheel dressing processes.

[0059] In a specific embodiment, the shape of the polishing disc 1 includes a truncated cone shape, and the rotation center axis of the polishing disc 1 is the center axis of the truncated cone;

[0060] “Controlling the spraying of hydroxyl radicals on the polishing disc 1” includes: controlling the spraying of hydroxyl radicals on the side of the truncated cone-shaped polishing disc 1;

[0061] “Making the grinding wheel 2 abut against the modified layer 3 on the polishing disk 1” includes: making the surface to be dressed on one side of the grinding wheel 2 abut against the modified layer 3 on one side of the truncated cone-shaped polishing disk 1; if the surface to be dressed on one side of the grinding wheel 2 is dressed, making the surface to be dressed on the other side of the grinding wheel 2 abut against the modified layer 3 on the other side of the truncated cone-shaped polishing disk 1.

[0062] As attached Figure 4 As shown, the shape of the polishing disc 1 of this embodiment can also be a truncated cone. This truncated cone design not only enhances the structural stability of the polishing disc 1, but also brings unique advantages to its functional characteristics. The rotation center axis of the polishing disc 1 is set as the center axis of the truncated cone, which ensures that the polishing disc 1 can maintain a uniform rotation speed and a stable rotation trajectory when rotating.

[0063] In the step of "controlling the spraying of hydroxyl radicals on the polishing disc 1", the spraying is controlled on the side of the truncated cone-shaped polishing disc 1 so that the substance can evenly cover the side of the polishing disc, thereby forming a uniform modified layer 3. Further, the surface to be dressed on one side of the grinding wheel 2 is made to abut against the modified layer 3 on one side of the truncated cone-shaped polishing disc 1. In this way, during the rotation and feeding process of the grinding wheel 2, its surface to be dressed can fully contact and rub with the modified layer, thereby achieving the dressing of the grinding wheel 2.

[0064] When the dressing surface of one side of the grinding wheel 2 is finished, the other side of the grinding wheel 2 can be rotated to abut against the modified layer 3 on the other side of the frustum-shaped polishing disc 1. This design not only improves the dressing efficiency, but also avoids errors and damages that may occur during the removal and reinstallation of the grinding wheel 2.

[0065] In this way, the grinding wheel 2 can be fully dressed, greatly improving the dressing efficiency and quality. At the same time, due to the frustum-shaped design of the polishing disc 1 and the method of side-spraying microwave plasma, the entire dressing process is more stable and reliable.

[0066] In a specific embodiment, the polishing disc 1 rotates in the same direction as the grinding wheel 2. The polishing disc 1 and the grinding wheel 2 rotate in the same direction, which can significantly reduce the friction and resistance generated when the two are in contact. This helps to achieve a smoother and more stable dressing process, avoiding the problem of grinding wheel surface damage or excessive wear of the polishing disc due to excessive friction.

[0067] Secondly, the rotation in the same direction also helps to improve the uniformity and consistency of dressing. When the grinding wheel 2 and the polishing disc 1 rotate in the same direction, every point on the surface of the grinding wheel 2 can fully contact and rub with the modified layer on the polishing disc 1, thereby ensuring the uniform distribution of the dressing effect. This uniform dressing effect can improve the machining accuracy and efficiency of the grinding wheel. In addition, the rotation in the same direction also helps to reduce noise and vibration during operation. Since the two rotate in the same direction, the vibration and noise caused by relative motion can be significantly reduced.

[0068] In one specific embodiment, the polishing disc 1 comprises a rigid polishing disc 1;

[0069] The hardness of the modified layer 3 is lower than the hardness of the remaining portion of the polishing pad 1 except the modified layer 3 .

[0070] In this embodiment, the polishing disc 1 adopts a rigid polishing disc structure. Such a rigid polishing disc not only has excellent structural strength and stability, but also can maintain shape stability during high-speed rotation and contact with the grinding wheel, ensuring the accuracy and reliability of the dressing process.

[0071] Furthermore, the hardness of the modified layer 3 is less than the hardness of the rest of the polishing disc 1 except the modified layer 3, which can better adapt to the characteristics of the resin-based sintered grinding wheel binder being soft and having a high elasticity, thereby providing a more uniform and detailed dressing effect. In addition, the hardness of the modified layer 3 enables it to deform to a certain extent when in contact with the grinding wheel, filling the tiny depressions and protrusions on the surface of the grinding wheel 2. This deformation effect makes the contact between the grinding wheel 2 and the polishing disc 1 closer, thereby improving the efficiency and accuracy of dressing.

[0072] In a specific embodiment, "making the grinding wheel 2 abut against the modified layer 3 on the polishing disk 1" includes: acting on the grinding wheel 2 with a preset load force, so that the grinding wheel 2 abuts against the modified layer 3 on the polishing disk 1. In this embodiment, the method of generating hydroxyl radicals is microwave plasma, and the preset load force ranges from 1N to 4N. Within the range of this load force, when the grinding wheel 2 is being dressed, the diamond abrasive grains on the grinding wheel 2 will not fall off. Hydroxyl-containing plasma (8slm argon, 140sccm water vapor) was introduced at a microwave power of 200W, and the processing was carried out for 30 minutes at a grinding wheel 2 speed of 60rpm and a polishing disk 1 speed of 200rpm. The maximum processing load of 4N was used for processing, and the morphology of the diamond on the surface after dressing and whether it fell off were observed. The results are shown in the attached figure. Fig.13 and attached Fig.14As shown in the figure, it can be seen that the flat surface of the diamond surface becomes larger after microwave plasma dressing, and the diamond on the grinding wheel 2 does not fall off. The 5 sharp abrasive grains before processing are still 5 sharp abrasive grains after dressing, and the top surfaces of the 2nd and 3rd abrasive grains become larger after dressing. The load used in the microwave plasma processing process is lower than the force in general grinding, so the diamond will not fall off during the dressing process.

[0073] By applying a preset load force to the grinding wheel 2, the grinding wheel 2 and the modified layer 3 on the polishing disc 1 are in stable and uniform contact. This contact state can not only ensure that the microscopic unevenness on the surface of the grinding wheel 2 is effectively removed, but also enable the surface of the grinding wheel 2 to be evenly worn and trimmed. At the same time, due to the reasonable control of the preset load force, the performance degradation or damage of the surface of the grinding wheel 2 caused by excessive wear can also be avoided.

[0074] In a specific embodiment, the method for generating hydroxyl radicals includes microwave plasma, and the generation of hydroxyl radicals is obtained by exciting a mixed gas of water vapor and argon through microwave plasma. Figure 6 As shown in Figure 2, optical emission spectrometry (OES) was used to compare the activity of free radicals in the two plasmas when water vapor was introduced into the reaction gas and when water vapor was not introduced into the reaction gas. Other experimental conditions were load 1N, microwave power 200W, grinding wheel speed 60rpm, silicon disk speed 200rpm for 30min processing. The results are shown in the attached figure. Figure 6 As shown, at a wavelength of λ=309nm, it can be observed that the activity of hydroxyl groups when water vapor is introduced is higher than that when water vapor is not introduced, which can make more active hydroxyl groups adhere to the polishing disk and diamond surface. Therefore, water vapor is selected as the reaction gas in microwave plasma dressing of grinding wheels.

[0075] In a specific embodiment, the method further includes: exciting microwave plasma by preset microwave power so that the temperature acting on the grinding wheel 2 is lower than the melting point of a binder for bonding abrasive grains in the grinding wheel 2;

[0076] The preset microwave power range is 150w-225w. Figure 7 As shown, this embodiment uses an infrared thermal imager to measure the temperature of a resin-based sintered grinding wheel during microwave plasma processing. The load used is 1N, and a hydroxyl-containing plasma (8slm argon, 140sccm water vapor) is introduced at a microwave power of 200W, and the processing is carried out for 30 minutes at a grinding wheel speed of 60rpm and a polishing disk speed of 200rpm. The temperature measurement points are the contact points between the plasma torch tube 5 and the polishing disk 1 and the contact points between the resin grinding wheel 2 and the polishing disk 1. The microwave power is selected at equal intervals between 150W and 225W. The results are shown in the attached figure. Figure 7As shown in the figure, the temperature of the two measuring points increases with the increase of microwave power, reaching the maximum at 225 W, with the highest temperature of 133.3 ° C, which is lower than the melting temperature of the resin binder of 250 ° C. Therefore, in the dressing process, if the power is between 150 W and 225 W, the resin binder will not be melted, and the resin-based sintered grinding wheel can be effectively dressed.

[0077] Embodiment 2

[0078] This embodiment provides a hydroxyl-modified grinding wheel 2 abrasive dressing system, which systematizes the hydroxyl-modified grinding wheel 2 abrasive dressing method of embodiment 1 to make it more practical. The specific scheme is as follows:

[0079] A hydroxyl-modified grinding wheel 2 abrasive dressing system, as shown in the attached Figure 2 As shown, including:

[0080] A control module 7, used for controlling the rotation of the polishing disc 1, and controlling the spraying of hydroxyl radicals on the polishing disc 1, so that a low-temperature modified layer 3 is formed in the sprayed area on the polishing disc 1;

[0081] The dressing module 8 is used to control the rotation of the grinding wheel 2 to be dressed, and to make the grinding wheel 2 abut against the modified layer 3 on the polishing disc 1, so that the contact surface of the grinding wheel 2 abutting against the modified layer 3 undergoes a hydroxyl dehydration condensation reaction, and under the mechanical shearing action generated by the relative movement of the grinding wheel 2 and the polishing disc 1, the part of the grinding wheel 2 undergoing the hydroxyl dehydration condensation reaction is dressed in a manner of removing material layer by layer at the atomic level.

[0082] In a specific embodiment, the polishing disk comprises: a flat polishing disk; and “controlling the spraying of hydroxyl radicals on the polishing disk” comprises:

[0083] The hydroxyl radicals are sprayed on the plane polishing surface of the polishing disc in a controlled manner; the distance between the spray position of the sprayed material on the plane polishing surface and the rotation center of the polishing disc is equal to the distance between the grinding wheel and the rotation center.

[0084] In a specific embodiment, the shape of the polishing disc includes a truncated cone shape, and the central axis of rotation of the polishing disc is the central axis of the truncated cone;

[0085] “Controlling the spraying of hydroxyl radicals on the polishing disc”, comprising: controlling the spraying of hydroxyl radicals on the side of the truncated cone-shaped polishing disc;

[0086] "Making the grinding wheel abut against the modified layer on the polishing disk" includes: making one side of the grinding wheel to be dressed abut against the modified layer on one side of the truncated cone-shaped polishing disk; if one side of the grinding wheel to be dressed is dressed, making the other side of the grinding wheel to be dressed abut against the modified layer on the other side of the truncated cone-shaped polishing disk.

[0087] In a specific embodiment, the rotation direction of the polishing disk is the same as the rotation direction of the grinding wheel.

[0088] In one specific embodiment, the polishing disk comprises a rigid polishing disk;

[0089] The modified layer has a hardness lower than the hardness of the remaining portion of the polishing pad excluding the modified layer.

[0090] In a specific embodiment, "making the grinding wheel abut against the modified layer on the polishing disc" includes: applying a preset load force to the grinding wheel to make the grinding wheel abut against the modified layer on the polishing disc and prevent abrasive grains from falling off during dressing.

[0091] In a specific embodiment, the method for generating hydroxyl radicals includes microwave plasma, and the generation of hydroxyl radicals is obtained by exciting a mixed gas of water vapor and argon gas through microwave plasma.

[0092] In a specific embodiment, the method further includes: exciting microwave plasma by presetting microwave power so that the temperature acting on the grinding wheel is lower than the melting point of a bonding agent used for bonding abrasive grains in the grinding wheel;

[0093] The preset microwave power range is 150w-225w.

[0094] Embodiment 3

[0095] This embodiment provides an abrasive dressing device for a grinding wheel 2 based on hydroxyl modification, which implements the abrasive dressing method for a grinding wheel 2 based on hydroxyl modification in embodiment 1 to make it more practical. The specific scheme is as follows:

[0096] A hydroxyl-modified grinding wheel 2 abrasive dressing device comprises: a polishing disc 1, a movable fixture 4, a plasma torch 5 for spraying microwave plasma, and a driving unit 6; the plasma torch 5 is provided with a nozzle facing the polishing disc 1, the driving unit 6 drives the polishing disc 1 and the movable fixture 4 to control the relative movement between the polishing disc 1 and the movable fixture 4; the movable fixture 4 is used to control the grinding wheel 2 to be dressed to abut against the polishing disc 1.

[0097] The present invention uses a mixed gas of argon and water vapor to excite microwave plasma at low temperature, so as to achieve micro-removal of diamonds with a small mechanical force, thereby achieving the dressing of the resin-based sintered grinding wheel. Diamonds are removed layer by layer at the atomic level, so that the surface of the resin-based sintered grinding wheel can achieve lower roughness and higher smoothness of the diamond surface.

[0098] Those skilled in the art will appreciate that the accompanying drawings are only schematic diagrams of a preferred implementation scenario, and the modules or processes in the accompanying drawings are not necessarily required for implementing the present invention. Those skilled in the art will appreciate that the modules in the devices in the implementation scenario may be distributed in the devices in the implementation scenario according to the description of the implementation scenario, or may be changed accordingly and located in one or more devices different from the present implementation scenario.

Claims

1. A method for dressing low-temperature grinding wheels based on hydroxyl modification, characterized in that: include: Controlling the rotation of the polishing disc and controlling the spraying of hydroxyl radicals on the polishing disc so that a low-temperature modified layer is formed in the sprayed area on the polishing disc; The grinding wheel to be dressed is controlled to rotate, and the grinding wheel is made to abut against the modified layer on the polishing disk, so that a hydroxyl dehydration condensation reaction occurs on the contact surface of the grinding wheel abutting against the modified layer, and under the mechanical shearing action generated by the relative movement of the grinding wheel and the polishing disk, the part of the grinding wheel where the hydroxyl dehydration condensation reaction occurs is dressed by removing material layer by layer at the atomic level.

2. The method according to claim 1, characterized in that The polishing disc comprises: a flat polishing disc; and the “controlling the spraying of hydroxyl radicals on the polishing disc” comprises: The hydroxyl radicals are controlled to be sprayed on the plane polishing surface of the polishing disk; the distance between the spraying position of the hydroxyl radicals on the plane polishing surface and the rotation center of the polishing disk is equal to the distance from the grinding wheel to the rotation center.

3. The method according to claim 1, characterized in that The shape of the polishing disc includes a truncated cone shape, and the rotation center axis of the polishing disc is the center axis of the truncated cone; The “controlling the spraying of hydroxyl radicals on the polishing disc” comprises: controlling the spraying of hydroxyl radicals on the side of the frustum-shaped polishing disc; The "making the grinding wheel abut against the modified layer on the polishing disk" includes: making one side of the grinding wheel to be dressed abut against the modified layer on one side of the truncated cone-shaped polishing disk; if one side of the grinding wheel to be dressed is dressed, making the other side of the grinding wheel to be dressed abut against the modified layer on the other side of the truncated cone-shaped polishing disk.

4. The method according to claim 1 or 2, characterized in that: The rotation direction of the polishing disc is the same as the rotation direction of the grinding wheel.

5. The method according to claim 1, characterized in that The polishing disc comprises a rigid polishing disc; The modified layer has a hardness lower than a hardness of a remaining portion of the polishing pad excluding the modified layer.

6. The method according to any one of claims 1 to 3, characterized in that: The “making the grinding wheel abut against the modified layer on the polishing disc” includes: applying a preset load force to the grinding wheel so that the grinding wheel abuts against the modified layer on the polishing disc; The preset load force ranges from 1N to 4N.

7. The method according to claim 1, characterized in that The method for generating the hydroxyl radicals includes microwave plasma, and the generation of the hydroxyl radicals is obtained by exciting a mixed gas of water vapor and argon through the microwave plasma.

8. The method according to claim 7, characterized in that Also includes: The microwave plasma is excited by preset microwave power so that the temperature acting on the grinding wheel is lower than the melting point of the bonding agent used for bonding abrasive grains in the grinding wheel; The preset microwave power ranges from 150w to 225w.

9. A low-temperature grinding wheel abrasive dressing system based on hydroxyl modification, characterized in that: include: A control module, used for controlling the rotation of the polishing disc and controlling the spraying of hydroxyl radicals on the polishing disc, so that a low-temperature modified layer is formed in the sprayed area on the polishing disc; The dressing module is used to control the rotation of the grinding wheel to be dressed and make the grinding wheel abut against the modified layer on the polishing disk, so that the contact surface of the grinding wheel abutting against the modified layer undergoes hydroxyl dehydration condensation reaction, and under the mechanical shearing action generated by the relative movement of the grinding wheel and the polishing disk, the part of the grinding wheel undergoing hydroxyl dehydration condensation reaction is dressed by removing material layer by layer at the atomic level.

10. A low-temperature grinding wheel abrasive dressing device based on hydroxyl modification, characterized in that: The device is used to execute the method described in any one of claims 1 to 8, comprising: a polishing disc, a movable clamp, a plasma torch for spraying microwave plasma and a driving unit; the plasma torch is provided with a nozzle facing the polishing disc, the driving unit drives and connects the polishing disc and the movable clamp respectively, and is used to control the relative movement between the polishing disc and the movable clamp; the movable clamp is used to control the grinding wheel to be dressed to abut against the polishing disc.

Citation Information

Patent Citations

  • Grinding wheel finishing method and device based on fluid dynamic pressure driving

    CN107756252A

  • Diamond polishing method based on plasma etching and modification effect

    CN117733662A

  • Slurries containing abrasive grains having a unique morphology

    US20100064593A1

Cited By

  • Device and method for chemically and mechanically polishing diamond substrate with assistance of double-modified multi-energy field

    CN119188584A