Preparation method of fireproof and wear-resistant cork floor

By adding modified kaolin and graphite powder to cork flooring, and using high temperature, high pressure and EDM processing, the problem of poor fire resistance of traditional cork flooring is solved, its fire resistance and wear resistance are significantly improved, and the product quality is improved.

CN118752575APending Publication Date: 2024-10-11常州艾美环保科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410828602.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing cork floor preparation method mainly uses oak bark raw materials, which results in unsatisfactory fire protection level. When a fire occurs, the fire will expand and produce a large amount of smoke, affecting product quality.

Method used

Using the ratio of cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer, through high temperature and high pressure processing and EDM surface processing, a cork floor with excellent fire resistance and wear resistance is prepared .

Benefits of technology

The fire resistance and wear resistance of the cork floor are improved, the floor surface is fine and beautiful, the use quality is improved, and the problem of traditional cork flooring expanding the fire intensity and smoke generation in a fire is solved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a fireproof and wear-resistant cork floor, and belongs to the technical field of building material processing, and the preparation method comprises the following steps: S1, raw material preparation: selecting cork particles, modified kaolin, graphite powder, a flame retardant, a softening agent, an adhesive and a stabilizer, the soft wood composite material is prepared from the following raw materials in parts by weight: 200-300 parts of soft wood particles, 100-140 parts of modified kaolin, 100-130 parts of graphite powder, 7-8 parts of a flame retardant, 6-10 parts of a softening agent, 7-8 parts of an adhesive and 10-13 parts of a stabilizer. According to the preparation method of the fireproof and wear-resistant cork floor, the fireproof and wear-resistant cork floor has excellent fire resistance, wear resistance and performance, EDM machining precision treatment is adopted, the floor surface is fine and attractive, the use quality of the cork floor is improved, and the problems that the cork floor prepared through an existing method is mainly made of oak bark raw materials, the fireproof grade is not ideal, and when a fire happens, the cork floor cannot be damaged are solved. The fire behavior can be expanded, and a large amount of smoke can be generated in the combustion process, so that the product quality is influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building material processing, in particular to a method for preparing a fireproof and wear-resistant cork floor. Background Art

[0002] Cork flooring is a type of flooring material made from cork. Cork is a natural material extracted from the bark of the Portuguese cypress tree and has become a popular flooring choice due to its unique structure and characteristics. Cork flooring has many advantages, including wear resistance, anti-slip, sound insulation and comfortable feel. Its soft characteristics make it soundless when people walk on it, just like walking on the beach, so cork flooring is particularly popular in recording studios, conference rooms, libraries, reading rooms, elderly homes, electronic classrooms and high-rise buildings. At the same time, cork flooring has good thermal insulation properties. In summer, it can reduce the intrusion of hot air from the outside, and in winter, it can prevent indoor heat from escaping through the ground, ensuring the constant surface temperature of the floor. Structurally, cork itself is a polyhedral (similar to honeycomb) structure filled with air, which is also the reason for its strong sound absorption ability. In addition, the anti-slip coefficient of cork flooring is high, and it will not be very slippery even if there is oil on it, which is very safe for the elderly and children. Its moisture resistance also determines that the stability of the floor is very strong, and it can even be used in humid environments such as bathrooms.

[0003] After searching, the patent number CN101602220B in the prior art discloses a method for preparing cork flooring, which includes the following steps: a. crushing oak bark into cork particles with a diameter of 0.2-0.8 mm; b. selecting oak bark of a certain length, boiling it in water, drying it in the sun, cutting it into small pieces of patterned fabrics, mixing it with polyurethane glue, pressing it into blanks, heating it, cooling it, and cutting it into sheet-like patterned fabrics; c. mixing the cork particles with the polyurethane glue, pressing it into blanks, heating it, cooling it, and slicing it to obtain a base material; d. pressurizing and compounding the patterned fabric and the base material coating liquid, heating it, cooling it, and sanding it to obtain a finished product; the cork flooring prepared by the method described in the invention has a high-pressure density of 600 kg / m 3 Above, the surface wear resistance revolutions reach more than 8000 revolutions.

[0004] The cork floor prepared by the above method is mainly made of oak bark raw material, and the fire resistance level is not ideal. When a fire occurs, the fire will spread and a large amount of smoke will be generated during the combustion process, affecting the quality of the product. Based on this, a method for preparing fire-resistant and wear-resistant cork floor is proposed to solve the above problems. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a fire-resistant and wear-resistant cork floor, which has the advantages of excellent fire resistance and the like, and solves the problem that the cork floor prepared by the prior method is mainly made of oak bark raw material, has an unsatisfactory fire resistance level, and when a fire occurs, will spread the fire and generate a large amount of smoke during the combustion process, thus affecting the product quality.

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a fireproof and wear-resistant cork floor, comprising the following steps:

[0007] S1. Raw material preparation: select cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer, and the weight proportion of the raw materials is 200-300 parts of cork particles, 100-140 parts of modified kaolin, 100-130 parts of graphite powder, 7-8 parts of flame retardant, 6-10 parts of softener, 7-8 parts of adhesive and 10-13 parts of stabilizer;

[0008] S2, mixing raw materials: adding the cork particles, modified kaolin and graphite powder selected in S1 into a mixer through a batching machine and stirring for 10-15 minutes, adding flame retardant, softener, adhesive and stabilizer in sequence during stirring, and finally obtaining a mixture;

[0009] S3, sheet forming: putting the mixed material in S2 into a mold, processing it under high temperature and high pressure, pressing it and cooling it to obtain a blank sheet;

[0010] S4, cutting and trimming: cutting the blank plate in S3 into the required size, and trimming the edges to remove impurities such as surface burrs;

[0011] S5. Surface EDM processing: Use the principle of electric spark discharge to process the surface of the blank plate after trimming in S4, remove the bad areas on the surface of the blank plate, and carve out fine lines and edges. After the processing is completed, the cork floor is obtained.

[0012] Furthermore, the cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in the following weight proportions: 200 parts of cork particles, 100 parts of modified kaolin, 100 parts of graphite powder, 7 parts of flame retardant, 6 parts of softener, 7 parts of adhesive and 10 parts of stabilizer.

[0013] Furthermore, the cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in the following weight proportions: 300 parts of cork particles, 140 parts of modified kaolin, 130 parts of graphite powder, 8 parts of flame retardant, 10 parts of softener, 8 parts of adhesive and 13 parts of stabilizer.

[0014] Furthermore, the cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in the following weight proportions: 250 parts of cork particles, 120 parts of modified kaolin, 120 parts of graphite powder, 7 parts of flame retardant, 8 parts of softener, 7 parts of adhesive and 11 parts of stabilizer.

[0015] Furthermore, the cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in the following weight proportions: 200 parts of cork particles, 140 parts of modified kaolin, 100 parts of graphite powder, 8 parts of flame retardant, 6 parts of softener, 8 parts of adhesive and 12 parts of stabilizer.

[0016] Furthermore, the cork particles are made of cork oak or cork paper mulberry bark, and the modified kaolin is made of kaolinite, fine sand, hydromica, silane coupling agent, calcium stearate and ethyl fiber.

[0017] Furthermore, the softener includes but is not limited to ammonia water, phenol, ethylene glycol and sulfuric acid, and the flame retardant includes but is not limited to chlorinated paraffin, tetrabromobisphenol A, tricresyl phosphate, triethoxysilane phosphate, antimony trioxide, magnesium hydroxide and aluminum hydroxide.

[0018] Furthermore, the adhesive includes but is not limited to acrylic adhesive, cellulose acetate adhesive, silicone adhesive, cement adhesive and hot melt adhesive, and the stabilizer includes an antioxidant, an anti-moisture agent, a filler and a moisture-proof agent.

[0019] Furthermore, in S2, the flame retardant, the softener and the stabilizer are added after stirring in the mixer for 5 minutes, and the adhesive is added after stirring for 8 minutes.

[0020] Compared with the prior art, the present invention provides a method for preparing a fire-resistant and wear-resistant cork floor, which has the following beneficial effects:

[0021] The method for preparing the fireproof and wear-resistant cork flooring ensures the softness of the cork flooring by adding modified kaolin and graphite powder on the basis of cork particle raw materials, and at the same time has excellent fire resistance and wear resistance, excellent performance, and fine processing by EDM processing, so that the surface of the flooring is fine and beautiful, and the use quality of the cork flooring is improved, and the problem that the cork flooring prepared by the existing method is mainly made of oak bark raw materials, the fire resistance level is not ideal, when a fire occurs, the fire will be expanded, and a large amount of smoke will be generated during the combustion process, affecting the product quality. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] A method for preparing a fireproof and wear-resistant cork floor comprises the following steps:

[0025] S1. Raw material preparation: select cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer. The weight proportion of the raw materials is 200 parts of cork particles, 100 parts of modified kaolin, 100 parts of graphite powder, 7 parts of flame retardant, 6 parts of softener, 7 parts of adhesive and 10 parts of stabilizer.

[0026] The cork particles are made of cork oak or cork paper bark, and the modified kaolin is made of kaolinite, fine sand, hydromica, silane coupling agent, calcium stearate and ethyl cellulose. Softeners include but are not limited to ammonia water, phenol, ethylene glycol and sulfuric acid, and flame retardants include but are not limited to chlorinated paraffin, tetrabromobisphenol A, tricresol phosphate, triethoxysilane phosphate, antimony trioxide, magnesium hydroxide and aluminum hydroxide. Adhesives include but are not limited to acrylic glue, cellulose acetate glue, silicone glue, cement glue and hot melt glue, and stabilizers include antioxidants, anti-moisture agents, fillers and moisture-proof agents.

[0027] S2. Mixing raw materials: adding the cork particles, modified kaolin and graphite powder selected in S1 into a mixer through a batching machine and stirring for 10-15 minutes. During the stirring period, flame retardants, softeners, adhesives and stabilizers are added in sequence to finally obtain a mixture.

[0028] Among them, the flame retardant, softener and stabilizer are added after stirring in the mixer for 5 minutes, and the adhesive is added after stirring for 8 minutes.

[0029] S3, sheet forming: the mixed material in S2 is placed in a mold, processed at high temperature and high pressure, pressed and cooled to obtain a blank sheet.

[0030] S4, cutting and trimming: cutting the blank plate in S3 into the required size, and trimming the edges to remove surface burrs and other impurities.

[0031] S5. Surface EDM processing: Use the principle of electric spark discharge to process the surface of the blank plate after trimming in S4, remove the bad areas on the surface of the blank plate, and carve out fine lines and edges. After the processing is completed, the cork floor is obtained.

[0032] Embodiment 2:

[0033] A method for preparing a fireproof and wear-resistant cork floor comprises the following steps:

[0034] S1. Raw material preparation: select cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer. The weight proportion of the raw materials is 300 parts of cork particles, 140 parts of modified kaolin, 130 parts of graphite powder, 8 parts of flame retardant, 10 parts of softener, 8 parts of adhesive and 13 parts of stabilizer.

[0035] The cork particles are made of cork oak or cork paper bark, and the modified kaolin is made of kaolinite, fine sand, hydromica, silane coupling agent, calcium stearate and ethyl cellulose. Softeners include but are not limited to ammonia water, phenol, ethylene glycol and sulfuric acid, and flame retardants include but are not limited to chlorinated paraffin, tetrabromobisphenol A, tricresol phosphate, triethoxysilane phosphate, antimony trioxide, magnesium hydroxide and aluminum hydroxide. Adhesives include but are not limited to acrylic glue, cellulose acetate glue, silicone glue, cement glue and hot melt glue, and stabilizers include antioxidants, anti-moisture agents, fillers and moisture-proof agents.

[0036] S2. Mixing raw materials: adding the cork particles, modified kaolin and graphite powder selected in S1 into a mixer through a batching machine and stirring for 10-15 minutes. During the stirring period, flame retardants, softeners, adhesives and stabilizers are added in sequence to finally obtain a mixture.

[0037] Among them, the flame retardant, softener and stabilizer are added after stirring in the mixer for 5 minutes, and the adhesive is added after stirring for 8 minutes.

[0038] S3, sheet forming: the mixed material in S2 is placed in a mold, processed at high temperature and high pressure, pressed and cooled to obtain a blank sheet.

[0039] S4, cutting and trimming: cutting the blank plate in S3 into the required size, and trimming the edges to remove surface burrs and other impurities.

[0040] S5. Surface EDM processing: Use the principle of electric spark discharge to process the surface of the blank plate after trimming in S4, remove the bad areas on the surface of the blank plate, and carve out fine lines and edges. After the processing is completed, the cork floor is obtained.

[0041] Embodiment three:

[0042] A method for preparing a fireproof and wear-resistant cork floor comprises the following steps:

[0043] S1. Raw material preparation: select cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer. The weight proportion of the raw materials is 250 parts of cork particles, 120 parts of modified kaolin, 120 parts of graphite powder, 7 parts of flame retardant, 8 parts of softener, 7 parts of adhesive and 11 parts of stabilizer.

[0044] The cork particles are made of cork oak or cork paper bark, and the modified kaolin is made of kaolinite, fine sand, hydromica, silane coupling agent, calcium stearate and ethyl cellulose. Softeners include but are not limited to ammonia water, phenol, ethylene glycol and sulfuric acid, and flame retardants include but are not limited to chlorinated paraffin, tetrabromobisphenol A, tricresol phosphate, triethoxysilane phosphate, antimony trioxide, magnesium hydroxide and aluminum hydroxide. Adhesives include but are not limited to acrylic glue, cellulose acetate glue, silicone glue, cement glue and hot melt glue, and stabilizers include antioxidants, anti-moisture agents, fillers and moisture-proof agents.

[0045] S2. Mixing raw materials: adding the cork particles, modified kaolin and graphite powder selected in S1 into a mixer through a batching machine and stirring for 10-15 minutes. During the stirring period, flame retardants, softeners, adhesives and stabilizers are added in sequence to finally obtain a mixture.

[0046] Among them, the flame retardant, softener and stabilizer are added after stirring in the mixer for 5 minutes, and the adhesive is added after stirring for 8 minutes.

[0047] S3, sheet forming: the mixed material in S2 is placed in a mold, processed at high temperature and high pressure, pressed and cooled to obtain a blank sheet.

[0048] S4, cutting and trimming: cutting the blank plate in S3 into the required size, and trimming the edges to remove surface burrs and other impurities.

[0049] S5. Surface EDM processing: Use the principle of electric spark discharge to process the surface of the blank plate after trimming in S4, remove the bad areas on the surface of the blank plate, and carve out fine lines and edges. After the processing is completed, the cork floor is obtained.

[0050] Embodiment 4:

[0051] A method for preparing a fireproof and wear-resistant cork floor comprises the following steps:

[0052] S1. Raw material preparation: select cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer. The weight proportion of the raw materials is 200 parts of cork particles, 140 parts of modified kaolin, 100 parts of graphite powder, 8 parts of flame retardant, 6 parts of softener, 8 parts of adhesive and 12 parts of stabilizer.

[0053] The cork particles are made of cork oak or cork paper bark, and the modified kaolin is made of kaolinite, fine sand, hydromica, silane coupling agent, calcium stearate and ethyl cellulose. Softeners include but are not limited to ammonia water, phenol, ethylene glycol and sulfuric acid, and flame retardants include but are not limited to chlorinated paraffin, tetrabromobisphenol A, tricresol phosphate, triethoxysilane phosphate, antimony trioxide, magnesium hydroxide and aluminum hydroxide. Adhesives include but are not limited to acrylic glue, cellulose acetate glue, silicone glue, cement glue and hot melt glue, and stabilizers include antioxidants, anti-moisture agents, fillers and moisture-proof agents.

[0054] S2. Mixing raw materials: adding the cork particles, modified kaolin and graphite powder selected in S1 into a mixer through a batching machine and stirring for 10-15 minutes. During the stirring period, flame retardants, softeners, adhesives and stabilizers are added in sequence to finally obtain a mixture.

[0055] Among them, the flame retardant, softener and stabilizer are added after stirring in the mixer for 5 minutes, and the adhesive is added after stirring for 8 minutes.

[0056] S3, sheet forming: the mixed material in S2 is placed in a mold, processed at high temperature and high pressure, pressed and cooled to obtain a blank sheet.

[0057] S4, cutting and trimming: cutting the blank plate in S3 into the required size, and trimming the edges to remove surface burrs and other impurities.

[0058] S5. Surface EDM processing: Use the principle of electric spark discharge to process the surface of the blank plate after trimming in S4, remove the bad areas on the surface of the blank plate, and carve out fine lines and edges. After the processing is completed, the cork floor is obtained.

[0059] The cork flooring produced by the above method is better in fire resistance and wear resistance than the current cork flooring.

[0060] The cork floors prepared in Examples 1-4 were subjected to performance tests. Through rigorous experiments, the experimental results are as follows: the cork floors prepared in the present invention are superior to traditional cork floors in terms of fire resistance and wear resistance.

[0061] The beneficial effects of the present invention are:

[0062] The preparation method of the fireproof and wear-resistant cork flooring ensures the softness of the cork flooring by adding modified kaolin and graphite powder on the basis of cork particle raw materials, and at the same time has excellent fire resistance and wear resistance, excellent performance, and adopts EDM processing to finely treat the flooring surface, which improves the use quality of the cork flooring and has good application prospects.

[0063] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a fireproof and wear-resistant cork floor, characterized in that: The following steps are involved: S1. Raw material preparation: select cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer, and the weight proportion of the raw materials is 200-300 parts of cork particles, 100-140 parts of modified kaolin, 100-130 parts of graphite powder, 7-8 parts of flame retardant, 6-10 parts of softener, 7-8 parts of adhesive and 10-13 parts of stabilizer; S2, mixing raw materials: adding the cork particles, modified kaolin and graphite powder selected in S1 into a mixer through a batching machine and stirring for 10-15 minutes, adding flame retardant, softener, adhesive and stabilizer in sequence during stirring, and finally obtaining a mixture; S3, sheet forming: putting the mixed material in S2 into a mold, processing it under high temperature and high pressure, pressing it and cooling it to obtain a blank sheet; S4, cutting and trimming: cutting the blank plate in S3 into the required size, and trimming the edges to remove impurities such as surface burrs; S5. Surface EDM processing: Use the principle of electric spark discharge to process the surface of the blank plate after trimming in S4, remove the bad areas on the surface of the blank plate, and carve out fine lines and edges. After the processing is completed, the cork floor is obtained.

2. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: The cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in proportion by weight: 200 parts of cork particles, 100 parts of modified kaolin, 100 parts of graphite powder, 7 parts of flame retardant, 6 parts of softener, 7 parts of adhesive and 10 parts of stabilizer.

3. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: The cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in proportion by weight: 300 parts of cork particles, 140 parts of modified kaolin, 130 parts of graphite powder, 8 parts of flame retardant, 10 parts of softener, 8 parts of adhesive and 13 parts of stabilizer.

4. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: The cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in proportion by weight: 250 parts of cork particles, 120 parts of modified kaolin, 120 parts of graphite powder, 7 parts of flame retardant, 8 parts of softener, 7 parts of adhesive and 11 parts of stabilizer.

5. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: The cork particles, modified kaolin, graphite powder, flame retardant, softener, adhesive and stabilizer also include the following raw materials in the following weight proportions: 200 parts of cork particles, 140 parts of modified kaolin, 100 parts of graphite powder, 8 parts of flame retardant, 6 parts of softener, 8 parts of adhesive and 12 parts of stabilizer.

6. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: The cork particles are made from cork oak or cork paper mulberry bark, and the modified kaolin is made from kaolinite, fine sand, hydromica, silane coupling agent, calcium stearate and ethyl fiber.

7. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: The softener includes but is not limited to ammonia water, phenol, ethylene glycol and sulfuric acid, and the flame retardant includes but is not limited to chlorinated paraffin, tetrabromobisphenol A, tricresyl phosphate, triethoxysilane phosphate, antimony trioxide, magnesium hydroxide and aluminum hydroxide.

8. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: The adhesive includes but is not limited to acrylic adhesive, cellulose acetate adhesive, silicone adhesive, cement adhesive and hot melt adhesive, and the stabilizer includes antioxidant, anti-moisture agent, filler and moisture-proof agent.

9. The method for preparing a fireproof and wear-resistant cork floor according to claim 1, characterized in that: In S2, the flame retardant, softener and stabilizer are added after stirring in the mixer for 5 minutes, and the adhesive is added after stirring for 8 minutes.