High-barrier-property food packaging material and preparation process thereof

Through a three-layer structure of high-barrier food packaging materials, combined with modified polyvinyl alcohol, polypropylene and polyethylene/nylon/curcumin blend materials, the problem of poor antibacterial performance and performance degradation of BOPP films has been solved, and a higher level has been achieved. Excellent barrier and mechanical properties, suitable for food packaging.

CN118752876AActive Publication Date: 2024-10-11ANHUI SHUNTONG PACKAGING MATERIAL

Patent Information

Application Number
CN202410903509.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Existing food packaging materials such as BOPP films have poor antibacterial properties and can easily lead to food mold and microbial erosion. Their performance declines after long-term storage and cannot meet the higher barrier requirements in the field of food packaging technology.

Method used

It adopts a three-layer structure of high-barrier food packaging materials, including a barrier layer, a core layer and a secondary barrier layer. It is made through co-extrusion and biaxial stretching processes. The barrier layer material is modified polyvinyl alcohol and the core layer material is polyvinyl alcohol. Propylene, the secondary barrier layer material is a blend of polyethylene, nylon and curcumin to enhance the barrier, antibacterial and antioxidant properties of the material.

Benefits of technology

It significantly improves the barrier properties, antibacterial properties and mechanical properties of packaging materials, extends the performance stability of the materials, and is suitable for the field of food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004931260840000031
    Figure BDA0004931260840000031
  • Figure BDA0004931260840000041
    Figure BDA0004931260840000041
  • Figure BDA0004931260840000042
    Figure BDA0004931260840000042
Patent Text Reader

Abstract

The invention discloses a high-barrier-property food packaging material and a preparation process thereof, and belongs to the technical field of food packaging. Comprising a barrier layer, a core layer and a secondary barrier layer, and the core layer is located between the barrier layer and the secondary barrier layer; the barrier layer, the core layer and the secondary barrier layer are co-extruded and then biaxially stretched into a whole, one-time extrusion molding is achieved, and the method is simple. Wherein the secondary barrier layer is prepared by blending polyethylene, nylon and curcumin, and the polyethylene and the nylon have complementary advantages, so that the barrier property and the mechanical property of the packaging material are greatly enhanced; curcumin not only can improve the antibacterial property of the packaging material, but also can enhance the oxidation resistance of the packaging material. The barrier layer is made of modified polyvinyl alcohol, has excellent barrier property on gas, is modified by grafting an organic molecular chain, has better compatibility with polypropylene, can greatly enhance the antibacterial property, mechanical property and oxidation resistance of the packaging material, has long and stable performance, and has important application value in the technical field of food packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of food packaging, and in particular, relates to a high-barrier food packaging material and a preparation process thereof. Background Art

[0002] With the continuous development of science and technology, people's quality of life has been greatly improved, and people are paying more and more attention to the quality and safety of food. Therefore, the field of food packaging materials related to food safety has also received great attention. An important performance of food packaging materials is barrier property. The barrier property of a material is its ability to prevent the penetrating object from penetrating, passing through and reaching the other side from one side. The penetrating objects include common gases, liquids, water vapor and organic matter. Food packaging materials with high barrier properties can effectively prevent food from oxidation, mold and deterioration, and have important application value in the field of food packaging technology.

[0003] In order to improve the barrier properties of food packaging materials, packaging films are usually in the form of composite packaging films, such as biaxially oriented polypropylene films, referred to as BOPP films. The production of BOPP film is to first make the melt of high molecular weight polypropylene into sheets or thick films through a narrow and long die, and then stretch it in two vertical directions (longitudinal and transverse) at a certain temperature and set speed in a special stretching machine at the same time or in steps, and then undergo appropriate cooling or heat treatment or special processing (such as corona, coating, etc.) to make a film. This kind of film has high physical stability, high mechanical strength, good air tightness, high transparency and gloss, and is tough and wear-resistant, and enjoys the reputation of "Queen of Packaging". However, the antibacterial property of BOPP film is poor. For foods that are stored for a long time, bacteria and mold will breed in large numbers, which can easily cause the food to be eroded by mold and microorganisms. In addition, the long-term storage of BOPP film will cause a certain aging, resulting in a decrease in the performance of the film. Therefore, it is urgent to invent a food packaging material that can solve the above problems to meet the higher demands in the field of food packaging technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a high barrier food packaging material and a preparation process thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high barrier food packaging material, comprising a barrier layer, a core layer and a secondary barrier layer, wherein the core layer is located between the barrier layer and the secondary barrier layer; the barrier layer, the core layer and the secondary barrier layer are formed into one piece by co-extrusion and biaxial stretching; the mass percentages of the barrier layer material, the core layer material and the secondary barrier layer material are: 15-25% for the barrier layer, 50-70% for the core layer and 15-25% for the secondary barrier layer;

[0007] A preparation process of a high barrier food packaging material comprises the following steps:

[0008] A1. Extruding the barrier layer material, the core layer material and the secondary barrier layer material into a barrier layer sheet, a core layer sheet and a secondary barrier layer sheet respectively through three extruders;

[0009] A2. The extruded barrier layer sheet, core layer sheet and secondary barrier layer sheet are extruded into cast sheets through a die head, and the temperature at the die head is set to 245° C. The core layer sheet is located between the barrier layer sheet and the secondary barrier layer sheet; the cast sheet is shaped by a chilled roller, and then longitudinally and transversely stretched into a film. The film is corona treated, rolled, and slit to form a high-barrier food packaging material.

[0010] Furthermore, in step A1, the core layer material is polypropylene.

[0011] Furthermore, in step A1, the extrusion temperature of the extruder for extruding the barrier layer is 200-215°C, the extrusion temperature of the extruder for extruding the core layer is 200-220°C, and the extrusion temperature of the extruder for extruding the secondary barrier layer is 210-230°C.

[0012] The barrier layer, the core layer and the secondary barrier layer are co-extruded to obtain the packaging material. The core layer material is polypropylene, which has strong chemical resistance and good mechanical properties. The packaging material is formed by one-time extrusion, and the method is simple.

[0013] Furthermore, the material of the secondary barrier layer is prepared by the following steps:

[0014] The polyethylene resin, curcumin and PA6 are uniformly stirred, added into a twin-screw extruder, melt-blended and extruded to obtain a secondary barrier layer material.

[0015] Furthermore, the raw materials are calculated in parts by weight as follows: 80-100 parts of polyethylene resin, 3-5 parts of curcumin, and 10-20 parts of PA6.

[0016] Polyethylene has good impact resistance and good barrier properties to water vapor, while nylon has high strength and good barrier properties to oxygen. The two complement each other's advantages, giving the secondary barrier layer material excellent barrier properties and mechanical strength. The added curcumin has significant antibacterial activity against foodborne pathogens, which can not only improve the antibacterial properties of the secondary barrier layer material, but also enhance the material's antioxidant properties.

[0017] Furthermore, the material of the barrier layer is prepared by the following steps:

[0018] S1. Mix 3,5-di-tert-butyl-4-hydroxybenzaldehyde, piperidine (condensing agent) and toluene in a three-necked flask equipped with a stirring device, heat to 40°C, stir until the solid is completely dissolved, add 3,4-diaminopyridine, keep warm for 4 hours, and after the reaction is completed, cool naturally and distill under reduced pressure to obtain intermediate 1; the ratio of 3,5-di-tert-butyl-4-hydroxybenzaldehyde, piperidine, toluene and 3,4-diaminopyridine is 23.4 g:15 mL:100 mL:11.4 g;

[0019] Under the action of the condensing agent, the amino group on 3,4-diaminopyridine condenses with the aldehyde group on 3,5-di-tert-butyl-4-hydroxybenzaldehyde to form an imine group (C=N Schiff base structure), and by controlling the molar ratio of the two to be close to 1:1 and a slight excess of 3,4-diaminopyridine, only one amino group on 3,4-diaminopyridine participates in the reaction to obtain intermediate 1; the specific reaction process is as follows:

[0020]

[0021] S2. Add intermediate 1, stearic acid, dicyclohexylcarbodiimide (DCC, dehydrating agent) and toluene to a three-necked flask equipped with a stirring device, stir and mix well, place in a water bath at 55°C, and heat in a water bath for 6 hours. After the reaction is completed, filter, remove the solvent by vacuum distillation, and then purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two is 4:3), and remove the eluent by rotary evaporation to obtain intermediate 2; the ratio of the amount of intermediate 1, stearic acid, dicyclohexylcarbodiimide and toluene is 32.5g:28.4g:20.6g:150mL;

[0022] Under the action of dicyclohexylcarbodiimide, intermediate 1 undergoes amidation reaction with stearic acid to obtain intermediate 2. The specific reaction process is as follows:

[0023]

[0024] S3, in a three-necked flask equipped with a stirring device, add intermediate 2 and toluene, stir and mix evenly, add epibromopropane, control the reaction temperature to 75 ° C, react for 12 hours, the reaction is completed, remove part of the solvent under vacuum, and then purify by column chromatography (eluent using a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 4:3), rotary evaporation to remove the eluent, to obtain a modifier; the ratio of intermediate 2, toluene, and epibromopropane is 59.1g:150mL:14.1g;

[0025] Intermediate 2 undergoes quaternization reaction with epibromopropane to obtain a modifier; the specific reaction process is as follows:

[0026]

[0027] S4. Add dimethyl sulfoxide and polyvinyl alcohol to a three-necked flask equipped with a stirring device. Under magnetic stirring, heat the oil bath to 95°C until the polyvinyl alcohol is completely dissolved, cool to 65°C, keep the temperature constant, add a modifier, stir for 10 minutes, then drop sodium hydroxide solution (mass fraction 12%), adjust the pH of the reaction system to 9-10, react at 65°C for 6 hours, cool to room temperature, add acetone, stir at room temperature until a colloidal precipitate is precipitated, filter, and vacuum dry to obtain a barrier layer material; the ratio of dimethyl sulfoxide, polyvinyl alcohol, and modifier is 50mL:10g:8g;

[0028] The hydroxyl groups on the polyvinyl alcohol molecules react with the epoxy groups on the modifiers, and the modifiers are grafted onto the macromolecular chains of the polyvinyl alcohol to obtain the barrier layer material;

[0029] The barrier layer material prepared is modified polyvinyl alcohol, which has excellent barrier properties to oxygen, nitrogen, hydrogen and carbon dioxide, and can improve the barrier properties of packaging materials; by modifying polyvinyl alcohol and grafting organic molecular chains, the polarity of polyvinyl alcohol can be reduced and the compatibility of polyvinyl alcohol with polypropylene can be improved; in addition, the grafted organic molecular chains contain pyridinium quaternary ammonium salt, Schiff base, long carbon chain, benzene ring and hindered phenol structure; among them, pyridinium quaternary ammonium salt is a new type of quaternary ammonium salt, whose positive charge is more concentrated and has stronger bactericidal ability, avoiding the problem of bacterial resistance caused by the long-term use of quaternary ammonium salt antibacterial agents, and can greatly enhance the antibacterial properties of the material; in addition, C=N Schiff base The structure can interact with bacterial proteins and enzymes, hindering the synthesis of bacterial nucleotides and amino acids, and acting synergistically with pyridinium quaternary ammonium salts to further improve the antibacterial properties of the material; the introduced long carbon chain belongs to the methylene chain segment as a flexible segment, which can not only enhance the mechanical properties of the material to a certain extent, but also belongs to the hydrophobic group with the benzene ring, thereby improving the waterproofness of the material; the hindered phenol structure has excellent antioxidant properties, which can not only improve the antioxidant properties of the material, but also act as an antioxidant in the production process, avoiding the addition of additional antioxidants and affecting the homogeneity of the material; finally, the polyvinyl alcohol grafted modifier can prevent the migration and shedding of small molecule modifiers, thereby ensuring the long-term stability of the material performance.

[0030] Beneficial effects of the present invention:

[0031] 1. The packaging material prepared by the present invention comprises a barrier layer, a core layer and a secondary barrier layer which are co-extruded. The core layer material is polypropylene which has strong chemical resistance and good mechanical properties. The packaging material is extruded once and the method is simple.

[0032] 2. The secondary barrier layer material is made of a blend of polyethylene, nylon and curcumin. The advantages of polyethylene and nylon complement each other, greatly enhancing the barrier and mechanical properties of the packaging material. Curcumin can not only improve the antibacterial properties of the packaging material, but also enhance the antioxidant properties of the packaging material.

[0033] 3. The barrier layer material is modified polyvinyl alcohol, which has excellent barrier properties to gases. It is modified by grafting organic molecular chains. Compared with ordinary polyvinyl alcohol, it has better compatibility with polypropylene. It can also greatly enhance the antibacterial, mechanical and antioxidant properties of the packaging material, and the performance is long-lasting and stable.

[0034] Therefore, the packaging material prepared by the present invention has stable and efficient barrier, antibacterial, mechanical and antioxidant properties, and has important application value in the field of food packaging technology. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] Preparation of barrier layer materials:

[0038] S1. In a three-necked flask equipped with a stirring device, 23.4 g of 3,5-di-tert-butyl-4-hydroxybenzaldehyde, 15 mL of piperidine and 100 mL of toluene were mixed, the temperature was raised to 40°C, and the mixture was stirred until the solid was completely dissolved. 11.4 g of 3,4-diaminopyridine was added, and the mixture was kept warm for 4 h. After the reaction was completed, the mixture was naturally cooled and distilled under reduced pressure to obtain intermediate 1.

[0039] S2, in a three-necked flask equipped with a stirring device, add 32.5g of intermediate 1, 28.4g of stearic acid, 20.6g of dicyclohexylcarbodiimide and 150mL of toluene, stir and mix well, place in a 55°C water bath, heat in a water bath for 6h, filter after the reaction, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 4:3), and remove the eluent by rotary evaporation to obtain intermediate 2;

[0040] S3, in a three-necked flask equipped with a stirring device, 59.1g of intermediate 2 and 150mL of toluene were added and stirred and mixed uniformly, then 14.1g of epibromopropane was added, and the reaction temperature was controlled to be 75°C, and the reaction was reacted for 12h. After the reaction was completed, part of the solvent was removed under vacuum, and then purified by column chromatography (eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:3), and the eluent was removed by rotary evaporation to obtain a modifier;

[0041] S4. Add 50 mL of dimethyl sulfoxide and 10 g of polyvinyl alcohol to a three-necked flask equipped with a stirring device. Under magnetic stirring, heat the oil bath to 95°C until the polyvinyl alcohol is completely dissolved, cool to 65°C, keep the temperature constant, add 8 g of modifier, stir for 10 minutes, then add sodium hydroxide solution (mass fraction 12%) dropwise, adjust the pH of the reaction system to 9, react at 65°C for 6 hours, cool to room temperature, add acetone, stir at room temperature until a colloidal precipitate is precipitated, filter, and vacuum dry to obtain a barrier layer material.

[0042] Example 2

[0043] Preparation of barrier layer materials:

[0044] S1. In a three-necked flask equipped with a stirring device, 46.8 g of 3,5-di-tert-butyl-4-hydroxybenzaldehyde, 30 mL of piperidine and 200 mL of toluene were mixed, the temperature was raised to 40°C, and the mixture was stirred until the solid was completely dissolved. 22.8 g of 3,4-diaminopyridine was added, and the mixture was kept warm for 4 h. After the reaction was completed, the mixture was naturally cooled and distilled under reduced pressure to obtain intermediate 1.

[0045] S2, in a three-necked flask equipped with a stirring device, add 65g of intermediate 1, 56.8g of stearic acid, 41.2g of dicyclohexylcarbodiimide and 300mL of toluene, stir and mix well, place in a 55°C water bath, heat in a water bath for 6h, filter after the reaction, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 4:3), and remove the eluent by rotary evaporation to obtain intermediate 2;

[0046] S3, in a three-necked flask equipped with a stirring device, 118.2g of intermediate 2 and 300mL of toluene were added and stirred and mixed uniformly, then 28.2g of epibromopropane was added, the reaction temperature was controlled to 75°C, the reaction was allowed to proceed for 12h, the reaction was completed, part of the solvent was removed under vacuum, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:3), the eluent was removed by rotary evaporation to obtain a modifier;

[0047] S4. Add 100 mL of dimethyl sulfoxide and 20 g of polyvinyl alcohol to a three-necked flask equipped with a stirring device. Under magnetic stirring, heat the oil bath to 95°C until the polyvinyl alcohol is completely dissolved, cool to 65°C, keep the temperature constant, add 16 g of modifier, stir for 10 minutes, then add sodium hydroxide solution (mass fraction 12%) dropwise, adjust the pH of the reaction system to 10, react at 65°C for 6 hours, cool to room temperature, add acetone, stir at room temperature until a colloidal precipitate is precipitated, filter, and vacuum dry to obtain a barrier layer material.

[0048] Example 3

[0049] Preparation of secondary barrier layer materials:

[0050] 80 g of polyethylene resin, 3 g of curcumin and 10 g of PA6 were uniformly stirred, added into a twin-screw extruder, melt-blended and extruded to obtain a secondary barrier layer material.

[0051] Example 4

[0052] Preparation of secondary barrier layer materials:

[0053] 100 g of polyethylene resin, 5 g of curcumin and 20 g of PA6 were uniformly stirred, added into a twin-screw extruder, melt-blended and extruded to obtain a secondary barrier layer material.

[0054] Example 5

[0055] A1. 15 g of the barrier layer material prepared in Example 1, 50 g of the core layer material (polypropylene) and 15 g of the secondary barrier layer material prepared in Example 3 were respectively extruded into a barrier layer sheet, a core layer sheet and a secondary barrier layer sheet with the same cross-sectional area by three extruders; wherein the extrusion temperature of the extruder for extruding the barrier layer sheet was 200° C., the extrusion temperature of the extruder for extruding the core layer sheet was 200° C., and the extrusion temperature of the extruder for extruding the secondary barrier layer sheet was 210° C.;

[0056] A2. Extruding the barrier layer sheet, core layer sheet and secondary barrier layer sheet through a die head to form a cast sheet, setting the temperature at the die head to 245° C. The core layer sheet is located between the barrier layer sheet and the secondary barrier layer sheet; the cast sheet is shaped by a chilled roller, and then longitudinally and transversely stretched into a film with a thickness of 80 μm. The film is corona treated, rolled, and slit to form a high-barrier food packaging material;

[0057] Example 6

[0058] A1. 20 g of the barrier layer material prepared in Example 1, 60 g of the core layer material (polypropylene) and 20 g of the secondary barrier layer material prepared in Example 3 are respectively extruded into a barrier layer sheet, a core layer sheet and a secondary barrier layer sheet with the same cross-sectional area by three extruders; wherein the extrusion temperature of the extruder for extruding the barrier layer sheet is 210° C., the extrusion temperature of the extruder for extruding the core layer sheet is 210° C., and the extrusion temperature of the extruder for extruding the secondary barrier layer sheet is 220° C.;

[0059] A2. Extruding the barrier layer sheet, core layer sheet and secondary barrier layer sheet through a die head to form a cast sheet, setting the temperature at the die head to 245° C. The core layer sheet is located between the barrier layer sheet and the secondary barrier layer sheet; the cast sheet is shaped by a chilled roller, and then longitudinally and transversely stretched into a film with a thickness of 80 μm. The film is corona treated, rolled, and slit to form a high-barrier food packaging material;

[0060] Example 7

[0061] A1. 25 g of the barrier layer material prepared in Example 1, 50 g of the core layer material (polypropylene) and 25 g of the secondary barrier layer material prepared in Example 3 were respectively extruded into a barrier layer sheet, a core layer sheet and a secondary barrier layer sheet with the same cross-sectional area by three extruders; wherein the extrusion temperature of the extruder for extruding the barrier layer sheet was 215° C., the extrusion temperature of the extruder for extruding the core layer sheet was 220° C., and the extrusion temperature of the extruder for extruding the secondary barrier layer sheet was 230° C.;

[0062] A2. Extruding the barrier layer sheet, core layer sheet and secondary barrier layer sheet through a die head to form a cast sheet, setting the temperature at the die head to 245° C. The core layer sheet is located between the barrier layer sheet and the secondary barrier layer sheet; the cast sheet is shaped by a chilled roller, and then longitudinally and transversely stretched into a film with a thickness of 80 μm. The film is corona treated, rolled, and slit to form a high-barrier food packaging material;

[0063] Comparative Example 1

[0064] Different from Example 7, the barrier layer material uses ordinary polyvinyl alcohol with the same mass fraction to prepare the food packaging material.

[0065] Comparative Example 2

[0066] Different from Example 7, the barrier layer material uses ordinary polyvinyl alcohol with the same mass fraction, and the secondary barrier layer material uses ordinary polyethylene with the same mass fraction to prepare the food packaging material.

[0067] Comparative Example 3

[0068] A commercially available high barrier BOPP film with a thickness of 80 μm was used.

[0069] Examples 5-7 and comparative examples 1-3 were made into corresponding shapes according to different test standards and subjected to the following performance tests:

[0070] The tensile strength was determined using the national standard GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets";

[0071] The oxygen permeability is measured using the national standard GB / T 1038-2022 "Plastic film and sheeting gas permeability test method pressure difference method";

[0072] The water vapor permeability is measured using the national standard GB / T 1037-2010 "Plastic film and sheeting water vapor permeability determination cup weight gain and weight loss method";

[0073] The national standard GB / T 31402-2015 "Test method for antibacterial performance of plastic surfaces" was adopted, and the film method was used to detect the inhibitory effect on Escherichia coli and Staphylococcus aureus; the method is as follows: Escherichia coli or Staphylococcus aureus bacteria were inoculated on the plate culture medium, covered with a film and preserved for 24 hours, and then live bacteria were cultured; the parallel experimental results of the blank samples were compared to obtain the antibacterial rate of the sample;

[0074] After the samples were placed at room temperature for 180 days, the tensile strength, oxygen permeability and moisture permeability of the samples were measured using the same standard;

[0075] The measured results are shown in the following table:

[0076]

[0077]

[0078] It can be seen from the above table that the barrier properties, antibacterial properties and mechanical properties of the packaging material prepared in the embodiment of the present invention are higher than those of the comparative example, and the performance is long-lasting and stable, which has important application value in the field of food packaging technology.

[0079] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0080] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A high barrier food packaging material, comprising a barrier layer, a core layer and a secondary barrier layer, characterized in that: The material of the barrier layer is prepared by the following steps: S1. Mix 3,5-di-tert-butyl-4-hydroxybenzaldehyde, piperidine and toluene, heat to 40°C, stir until the solid is completely dissolved, add 3,4-diaminopyridine, keep warm for 4 hours, and after the reaction is complete, cool naturally and distill under reduced pressure to obtain intermediate 1; S2. Add intermediate 1, stearic acid, dicyclohexylcarbodiimide and toluene into a three-necked flask, stir and mix well, heat at 55° C. for 6 h, and when the reaction is complete, filter, distill under reduced pressure, purify by column chromatography, and rotary evaporate to obtain intermediate 2; S3, adding intermediate 2 and toluene into a three-necked flask, stirring and mixing, adding epibromopropane, reacting at 75° C. for 12 h, and after the reaction is completed, removing part of the solvent under vacuum conditions, purifying by column chromatography, and rotary evaporation to obtain a modifier; S4. Add dimethyl sulfoxide and polyvinyl alcohol into a three-necked flask, raise the temperature to 95°C under magnetic stirring until the polyvinyl alcohol is completely dissolved, cool to 65°C, keep the temperature constant, add a modifier, stir for 10 minutes, then drop sodium hydroxide solution, adjust the pH of the reaction system to 9-10, react at 65°C for 6 hours, cool the reaction, add acetone, stir at room temperature until a precipitate is precipitated, filter, and vacuum dry to obtain a barrier layer material.

2. A high barrier food packaging material according to claim 1, characterized in that: In step S1, the ratio of the amount of 3,5-di-tert-butyl-4-hydroxybenzaldehyde, piperidine, toluene and 3,4-diaminopyridine is 23.4 g: 15 mL: 100 mL: 11.4 g.

3. A high barrier food packaging material according to claim 1, characterized in that: In step S2, the ratio of the amount of intermediate 1, stearic acid, dicyclohexylcarbodiimide and toluene is 32.5 g: 28.4 g: 20.6 g: 150 mL.

4. The high barrier food packaging material according to claim 1, characterized in that: In step S3, the ratio of the amount of intermediate 2, toluene and epibromopropane used is 59.1 g:150 mL:14.1 g.

5. The high barrier food packaging material according to claim 1, characterized in that: In step S4, the ratio of dimethyl sulfoxide, polyvinyl alcohol and modifier is 50 mL: 10 g: 8 g.

6. The high barrier food packaging material according to claim 1, characterized in that: The material of the secondary barrier layer is prepared by the following steps: The polyethylene resin, curcumin and PA6 are uniformly stirred, added into a twin-screw extruder, melt-blended and extruded to obtain a secondary barrier layer material.

7. A high barrier food packaging material according to claim 6, characterized in that: The raw materials are calculated in parts by weight as follows: 80-100 parts of polyethylene resin, 3-5 parts of curcumin, and 10-20 parts of PA6.

8. The method for processing an antibacterial food packaging material according to claim 1, characterized in that: The following steps are involved: A1. Extruding the barrier layer material, the core layer material and the secondary barrier layer material into a barrier layer sheet, a core layer sheet and a secondary barrier layer sheet respectively through three extruders; A2. The extruded barrier layer sheet, core layer sheet and secondary barrier layer sheet are extruded into cast sheets through a die head, and the temperature at the die head is set to 245° C. The core layer sheet is located between the barrier layer sheet and the secondary barrier layer sheet; the cast sheet is shaped by a chilled roller, and then longitudinally and transversely stretched into a film. The film is corona treated, rolled, and slit to form a high-barrier food packaging material.

Citation Information

Patent Citations

  • High-barrier material for red wine BIB packaging

    CN104723639A

  • Preparation method of high-strength acrylate rubber material

    CN112898711A

  • Environment-friendly coating with high corrosion resistance and oxidation resistance and preparation method

    CN114891415A

  • Plastic resin modifier compositions and methods of making thermoplastic materials and articles using same

    CN116419948A

  • Cationic modified soft PVC membrane material and preparation method thereof

    CN119241976A

Cited By

  • High-barrier recyclable eleven-layer co-extrusion film for food packaging and preparation process

    CN119217699A

  • Polyethylene environment-friendly packaging material as well as preparation method and application thereof

    CN119749021A