Polyester and chinlon composite fabric as well as preparation method and application thereof

Through heat treatment and glue lamination on polyester and nylon fabrics, problems such as water ripples and wrinkles during the lamination process are solved, the flatness and drape of the fabrics are improved, and the integrity and elasticity effects are maintained during the washing process.

CN118752880AInactive Publication Date: 2024-10-11BOSIDENG DOWN WEAR LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411062079.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the lamination process of polyester and nylon fabrics, problems such as water ripples, wrinkles or natural fabric curls are prone to occur, resulting in poor flatness and drape of the fabric, and possible delamination during the washing process.

Method used

The polyester and nylon fabrics are heat-treated before lamination. Ensure that they are heat-treated before lamination. The surface of the polyester fabric is sanded to increase the lamination fastness and waxy feel. Polyurethane hot melt adhesive is used for lamination and sealing. and thermal insulation.

Benefits of technology

The polyester and nylon composite fabric produced has good flatness, drape and elasticity effects, does not delaminate during washing and dry cleaning, and has a soft luster.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118752880A_ABST
    Figure CN118752880A_ABST
Patent Text Reader

Abstract

The invention provides a terylene and chinlon composite fabric and a preparation method and application thereof, the preparation method comprises the following steps: (1) carrying out heat treatment on a terylene fabric to obtain a heat-treated terylene fabric; (2) carrying out heat treatment on the chinlon fabric to obtain a heat-treated chinlon fabric; (3) gluing the surface of the heat-treated polyester fabric prepared in the step (1), and compounding the heat-treated polyester fabric with the heat-treated chinlon fabric prepared in the step (2) to obtain the polyester and chinlon composite fabric, the step (1) and the step (2) are carried out step by step regardless of a sequence or are carried out at the same time. The terylene and chinlon composite fabric prepared by the preparation method provided by the invention is good in flatness, draping effect and elastic effect, free of water ripples, wrinkles or natural rolling of the fabric, free of layering in water washing and dry cleaning processes, and soft in gloss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabric processing, and specifically relates to a polyester and nylon composite fabric and a preparation method and application thereof. Background Art

[0002] In traditional clothing, women's skirts, dresses or waist skirts all have certain requirements for drape. If the above skirts are made of all-nylon stretch fabric, they are too tight or close-fitting, and cannot achieve the effect of drape and elegance, and can only be used for spring and summer clothing. If you want to make autumn and winter clothing and need good drape, close fit, moderate elasticity, and smooth feel, you need to use polyester and nylon composite fabrics.

[0003] Polyester fabric has high strength and elastic recovery ability. Polyester is the best heat-resistant fabric among synthetic fabrics. It is thermoplastic and can be made into pleated skirts with long-lasting pleats. Nylon fabric has high strength, high wear resistance, high chemical resistance, good deformation resistance and aging resistance, but its disadvantage is that it feels hard. Due to the difference in elasticity and shrinkage between polyester and nylon fabrics, water ripples, wrinkles or natural curling of fabrics are prone to occur during the compounding process.

[0004] Therefore, it is necessary to provide a method for preparing a polyester and nylon composite fabric to solve the problems of water ripples, wrinkles or natural curling of the fabric that are prone to occur during the composite process of the polyester fabric and the nylon fabric. Summary of the invention

[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a polyester and nylon composite fabric and a preparation method and application thereof. The polyester and nylon composite fabric prepared by the preparation method has good flatness, drape and elasticity, no water ripples, wrinkles or natural curling of the fabric, no stratification during washing and dry cleaning, and a soft luster.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a polyester and nylon composite fabric, the preparation method comprising the following steps:

[0008] (1) heat-treating the polyester fabric to obtain a heat-treated polyester fabric;

[0009] (2) heat-treating the nylon fabric to obtain the heat-treated nylon fabric;

[0010] (3) gluing the surface of the heat-treated polyester fabric obtained in step (1) and compounding it with the heat-treated nylon fabric obtained in step (2) to obtain the polyester and nylon composite fabric;

[0011] The steps (1) and (2) are performed in no particular order, or are performed simultaneously.

[0012] In the present invention, by performing heat treatment before gluing and compounding the polyester fabric and the nylon fabric, the prepared polyester and nylon composite fabric will not have problems such as water ripples, wrinkles or natural curling of the fabric due to differences in elasticity and shrinkage rate; the polyester and nylon composite fabric prepared by the preparation method has good flatness, drape and elasticity, does not delaminate during washing and dry cleaning, and has a soft luster.

[0013] Preferably, the polyester fabric comprises the following components by mass percentage: 92%-98% (92.5%, 93%, 93.5%, 94%, 94.5%, 95%, 95.5%, 96%, 96.5%, 97% or 97.5%, etc.) of polyester and 3%-8% (for example, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7% or 7.5%, etc.) of spandex.

[0014] Preferably, the polyester fabric has a gram weight of 130-150 g / m 2 , for example 132g / m 2 , 134g / m 2 , 136g / m 2 , 138g / m 2 , 140g / m 2 , 142g / m 2 , 144g / m 2 , 146g / m 2 or 148g / m 2 wait.

[0015] Preferably, the nylon fabric comprises the following components by mass percentage: 80%-85% nylon (for example, 80.5%, 81%, 81.5%, 82%, 82.5%, 83%, 83.5%, 84% or 84.5%, etc.) and 15%-20% spandex (for example, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19% or 19.5%, etc.).

[0016] Preferably, the nylon fabric has a gram weight of 150-170 g / m 2 , for example 152g / m 2 , 154g / m 2 , 156g / m 2 , 158g / m 2 , 160g / m 2 , 162g / m 2 , 164g / m 2 , 166g / m 2 or 168g / m2 wait.

[0017] In the present invention, the mass percentage of spandex in the nylon fabric is ≥15%, so the nylon fabric has great elasticity and a large shrinkage rate. If the existing technology is adopted, after the hot melt adhesive laminating machine is heated up, the base fabric (polyester fabric) is directly glued, and then the hot melt adhesive laminating machine is introduced into the surface fabric (nylon fabric) to bond the two fabrics, and after the rotating wheel, the pressure of the conduit is bonded, and finally the fabric bonding process is cooled, the polyester and nylon composite fabric prepared will have water ripples or wrinkles at the lightest due to excessive shrinkage rate, and the hand feel will be stiff and the product will be scrapped.

[0018] In the present invention, the wrinkles refer to a very obvious and regular texture, which is specifically manifested in the appearance of folds (wrinkles) in the warp or weft direction. The reason for this is that the shrinkage rate of the surface fabric or the base fabric is too large on one side, and it cannot shrink due to the glue compound, thereby affecting the flatness of the entire fabric. The marks appear in a vertical or horizontal manner. If the fabric is cut, it will roll up immediately. It is different from wrinkles, which are irregular textures.

[0019] Preferably, the heat treatment in step (1) and step (2) specifically includes heating the surface of the substrate in a non-gluing state by means of a hot melt adhesive laminating machine.

[0020] Preferably, the heat treatment temperatures in step (1) and step (2) are each independently 80-100°C, for example, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C or 98°C, etc.

[0021] In the present invention, the heat treatment in step (1) and step (2) can be performed during the heating process of the hot melt adhesive laminating machine or during the cooling process of the hot melt adhesive laminating machine.

[0022] Preferably, the heat treatment speeds in step (1) and step (2) are each independently 1.5-2.5 m / s, for example, 1.6 m / s, 1.7 m / s, 1.8 m / s, 1.9 m / s, 2.0 m / s, 2.1 m / s, 2.2 m / s, 2.3 m / s or 2.4 m / s, etc.

[0023] Preferably, the heat treatment in step (1) and step (2) further includes a cooling step.

[0024] Preferably, the step (3) of gluing the surface of the heat-treated polyester fabric obtained in step (1) specifically includes gluing the side of the sanded (raised) surface of the heat-treated polyester fabric obtained in step (1).

[0025] In the present invention, by applying glue on the side of the polyester fabric surface that has been sanded after heat treatment, the composite fastness of the polyester fabric and the nylon fabric is increased, and the hand feeling is also increased, and light transmission does not occur. This is because there is a space difference between the top and the root of the wool particles on the side of the polyester fabric surface that has been sanded, and there are gaps between the wool particles, so that after the polyester fabric and the nylon fabric are composited, there is an effect similar to an air interlayer, making the fit of the polyester fabric and the nylon fabric more plastic, the drape and elasticity are not deteriorated due to the composite, the hand feeling becomes more glutinous, and light transmission is not easy to occur.

[0026] Preferably, the gluing and compounding in step (3) are performed on a hot melt adhesive compounding machine, the temperature of the hot melt adhesive compounding machine is 100-120°C, for example, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C or 118°C, and the amount of glue applied is 10-20g / m 2 , for example 11g / m 2 , 12g / m 2 , 13g / m 2 , 14g / m 2 , 15g / m 2 , 16g / m 2 , 17g / m 2 , 18g / m 2 or 19g / m 2 wait.

[0027] In the present invention, the gluing and compounding of step (3) are performed on a hot melt adhesive compounding machine, and can be performed according to the compounding process of compounding on a hot melt adhesive compounding machine well known in the art, and at the same time, the roller tension needs to be kept to a minimum, and the left and right pulling force of the whole equipment on both sides should not be too large, so that the fabric can be kept flat. The present invention does not have any special restrictions on the hot melt adhesive used for gluing, and hot melt adhesives that can be used for bonding between fabrics that are well known to those skilled in the art can be used, such as polyurethane hot melt adhesive.

[0028] Preferably, the compounding speed in step (3) is 1-2 m / s, for example, 1.1 m / s, 1.2 m / s, 1.3 m / s, 1.4 m / s, 1.5 m / s, 1.6 m / s, 1.7 m / s, 1.8 m / s or 1.9 m / s, etc.

[0029] Preferably, step (3) further includes the steps of sealing and heat preservation after the compounding.

[0030] Preferably, the sealing includes sealing with a thermal insulation film.

[0031] Preferably, the temperature of the heat preservation treatment is 50-100°C, for example, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C.

[0032] Preferably, the insulation treatment time is 4-5 h, for example, 4.1 h, 4.2 h, 4.3 h, 4.4 h, 4.5 h, 4.6 h, 4.7 h, 4.8 h or 4.9 h.

[0033] In the present invention, the polyester and nylon composite fabric has good elasticity through sealing and heat preservation treatment after composite. If the polyester and nylon composite fabric is not subjected to heat preservation treatment, the elasticity effect will be greatly reduced and the fabric will become soft.

[0034] In a second aspect, the present invention provides a polyester and nylon composite fabric, which is prepared by the preparation method described in the first aspect.

[0035] In a third aspect, the present invention provides an application of the polyester and nylon composite fabric as described in the second aspect in clothing.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] In the present invention, by performing heat treatment before gluing and compounding the polyester fabric and the nylon fabric, the prepared polyester and nylon composite fabric will not have problems such as water ripples, wrinkles or natural curling of the fabric due to differences in elasticity and shrinkage rate; the polyester and nylon composite fabric prepared by the preparation method has good flatness, drape and elasticity, does not delaminate during washing and dry cleaning, and has a soft luster. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 A schematic diagram of the structure of the polyester and nylon composite fabric provided in Example 1;

[0039] Among them, 1-polyester fabric layer; 2-viscose layer; 3-nylon fabric layer. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0041] Some of the raw materials in the embodiments and comparative examples are as follows:

[0042] Polyurethane hot melt adhesive is commercially available, and the same commercial product was used in parallel experiments.

[0043] Example 1

[0044] This embodiment provides a polyester and nylon composite fabric and a preparation method thereof, such as Figure 1 As shown, the polyester and nylon composite fabric comprises a polyester fabric layer 1, a viscose layer 2 and a nylon fabric layer 3 which are stacked in sequence;

[0045] The polyester fabric layer 1 comprises polyester fabric, which is a knitted fabric of 95wt% polyester and 5wt% spandex, with a gram weight of 140g / m 2 , Width: 170cm, one side is sanded;

[0046] The adhesive layer 2 includes polyurethane hot melt adhesive;

[0047] The nylon fabric layer 3 comprises nylon fabric, which is a knitted fabric of 85wt% nylon and 15wt% spandex, with a gram weight of 160g / m 2 , width: 160cm.

[0048] The preparation method comprises the following steps:

[0049] (1) heating the hot melt adhesive laminating machine, and passing the polyester fabric through the hot melt adhesive laminating machine for heat treatment without gluing during the heating process, at a speed of 2 m / s, wherein the temperature of the hot melt adhesive laminating machine is raised from 80° C. to 100° C., and after the heat treatment, the fabric is cooled at room temperature for 10 minutes to obtain a heat-treated polyester fabric;

[0050] (2) raising the temperature of the hot melt adhesive laminating machine, and passing the nylon fabric through the hot melt adhesive laminating machine for heat treatment without gluing during the heating process, at a speed of 2 m / s, wherein the temperature of the hot melt adhesive laminating machine is raised from 80° C. to 100° C., and after the heat treatment, the nylon fabric is cooled at room temperature for 10 min to obtain the heat-treated nylon fabric;

[0051] (3) The temperature of the hot melt adhesive laminating machine was raised to 120° C. The side of the polyester fabric surface subjected to heat treatment obtained in step (1) was coated with polyurethane hot melt adhesive for gluing, and the amount of adhesive was 20 g / m 2 Then, the heat-treated nylon fabric obtained in step (2) is introduced into the hot melt adhesive laminating machine for lamination. The laminating speed is 1 m / s, the roller tension is minimized, and the left and right pulling force of the whole equipment on both sides should not be too large, so that the fabric can be kept flat. After lamination, the tube is quickly drawn out, and the polyethylene insulation film is wrapped to seal it, and it is placed in a 60°C insulation room for insulation treatment for 4 hours to obtain the polyester and nylon composite fabric.

[0052] The above-mentioned hot melt adhesive laminating machine is a 2019 model hot melt adhesive laminating machine of Jiangsu Hongye Machinery Co., Ltd.

[0053] Example 2

[0054] This embodiment provides a polyester and nylon composite fabric and a preparation method thereof, wherein the polyester and nylon composite fabric comprises a polyester fabric layer, a viscose layer and a nylon fabric layer stacked in sequence;

[0055] The polyester fabric layer includes polyester fabric, which is a knitted fabric with 92wt% polyester and 8wt% spandex, and a gram weight of 140g / m 2 , Width: 170cm, one side is sanded;

[0056] The adhesive layer includes polyurethane hot melt adhesive;

[0057] The nylon fabric layer comprises nylon fabric, which is a knitted fabric of 80wt% nylon and 20wt% spandex, with a gram weight of 160g / m 2 , width: 160cm.

[0058] The preparation method comprises the following steps:

[0059] (1) cooling the hot melt adhesive laminating machine, and during the cooling process, passing the polyester fabric through the hot melt adhesive laminating machine for heat treatment without gluing, at a speed of 2 m / s, wherein the temperature of the hot melt adhesive laminating machine is cooled from 100° C. to 80° C., and after the heat treatment, the polyester fabric is cooled at room temperature for 10 minutes to obtain the heat-treated polyester fabric;

[0060] (2) cooling the hot melt adhesive laminating machine, and during the cooling process, passing the nylon fabric through the hot melt adhesive laminating machine for heat treatment without gluing, at a speed of 2 m / s, wherein the temperature of the hot melt adhesive laminating machine is cooled from 100° C. to 80° C., and after the heat treatment, cooled at room temperature for 10 min to obtain the heat-treated nylon fabric;

[0061] (3) The temperature of the hot melt adhesive laminating machine was raised to 100° C., and a polyurethane hot melt adhesive was applied to the brushed side of the heat-treated polyester fabric obtained in step (1) for gluing, with the gluing amount being 10 g / m 2 Then, the heat-treated nylon fabric obtained in step (2) is introduced into the hot melt adhesive laminating machine for lamination. The laminating speed is 2 m / s, the roller tension is minimized, and the left and right pulling force of the whole equipment on both sides should not be too large, so that the fabric can be kept flat. After lamination, the tube is quickly drawn out, and the polyethylene insulation film is wrapped to seal it, and it is placed in an 80°C insulation room for insulation treatment for 5 hours to obtain the polyester and nylon composite fabric.

[0062] The above-mentioned hot melt adhesive laminating machine is a 2019 model hot melt adhesive laminating machine of Jiangsu Hongye Machinery Co., Ltd.

[0063] Example 3

[0064] This embodiment provides a polyester and nylon composite fabric and a preparation method thereof. The only difference between this embodiment and embodiment 1 is that the polyester fabric is a knitted fabric of 95wt% polyester and 5wt% spandex, with a gram weight of 140g / m 2 , width: 170cm, not sanded.

[0065] In step (3), the step of coating one side of the heat-treated polyester fabric obtained in step (1) with polyurethane hot-melt adhesive for gluing is adjusted to coating one side of the heat-treated polyester fabric obtained in step (1) with polyurethane hot-melt adhesive for gluing.

[0066] Other conditions are the same as in Example 1.

[0067] Example 4

[0068] This embodiment provides a polyester and nylon composite fabric and a preparation method thereof, which differs from Embodiment 1 only in that it does not include the steps of wrapping with a polyethylene insulation film for sealing and placing in a 60° C. insulation room for 4 hours, and other conditions are the same as those in Embodiment 1.

[0069] Comparative Example 1

[0070] The present comparative example provides a polyester and nylon composite fabric and a preparation method thereof, which differs from Example 1 only in that it does not include step (1) and step (2), and step (3) is adjusted to raise the temperature of the hot melt adhesive laminating machine to 120°C, apply polyurethane hot melt adhesive on one side of the polyester fabric for gluing, and then introduce the nylon fabric into the hot melt adhesive laminating machine for laminating, the laminating speed is 2m / s, the roller tension is minimized, the left and right pulling force of the whole equipment on both sides should not be too large, so that the fabric can be kept flat, and after laminating, the tube is quickly drawn out, and wrapped with polyethylene insulation film to seal, and placed in a 60°C insulation room for insulation treatment for 4 hours to obtain the polyester and nylon composite fabric.

[0071] Other conditions are the same as in Example 1.

[0072] Performance Testing

[0073] The polyester and nylon composite fabrics provided in the above embodiments and comparative examples were tested, and the specific testing method is as follows:

[0074] Appearance: Visually observe that if the polyester and nylon composite fabric is smooth, without water ripples, wrinkles, or natural curls, it is marked as "qualified". If the polyester and nylon composite fabric is not smooth, without water ripples, wrinkles, or natural curls, it is marked as "unqualified".

[0075] Hand feel: The polyester and nylon composite fabrics provided in the embodiments and comparative examples were subjected to hand feel tests by professional testers to test the waxiness, drape and elasticity of the fabrics.

[0076] The test results are shown in Table 1 below:

[0077] Table 1

[0078]

[0079] It can be seen from the contents of Table 1 that the polyester and nylon composite fabrics prepared by the preparation methods provided in Examples 1-4 have good flatness, and no water ripples, wrinkles or natural curling of the fabrics occur.

[0080] Compared with Example 1, the composite fastness, glutinous hand feeling and light-proof effect of the polyester and nylon composite fabric prepared in Example 1 are far superior to those of the polyester and nylon composite fabric provided in Example 3. It can be seen that in the present invention, by applying glue on the side of the heat-treated polyester fabric with velvet and sanding, the prepared polyester and nylon composite fabric has a better effect.

[0081] Compared with Example 1, if the step of wrapping with a polyethylene insulation film for sealing and placing in a 60°C insulation room for insulation treatment for 4 hours is not included (Example 4), the elastic effect of the obtained polyester and nylon composite fabric is poor and the fabric becomes soft. It can be seen that in the present invention, the polyester and nylon composite fabric prepared by sealing after compounding and insulation treatment is better.

[0082] Compared with Example 1, if step (1) and step (2) are not included (Comparative Example 1), the prepared polyester and nylon composite fabric will have water ripples, and a smooth polyester and nylon composite fabric cannot be obtained.

[0083] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a polyester and nylon composite fabric, characterized in that: The preparation method comprises the following steps: (1) heat-treating the polyester fabric to obtain a heat-treated polyester fabric; (2) heat-treating the nylon fabric to obtain the heat-treated nylon fabric; (3) gluing the surface of the heat-treated polyester fabric obtained in step (1) and compounding it with the heat-treated nylon fabric obtained in step (2) to obtain the polyester and nylon composite fabric; The steps (1) and (2) are performed in no particular order, or are performed simultaneously.

2. The preparation method according to claim 1, characterized in that: The polyester fabric comprises the following components by mass percentage: 92%-98% polyester and 3%-8% spandex.

3. The preparation method according to claim 1 or 2, characterized in that: The nylon fabric comprises the following components by mass percentage: 80%-85% nylon and 15%-20% spandex.

4. The preparation method according to any one of claims 1 to 3, characterized in that The heat treatment in step (1) and step (2) specifically includes heat treatment in a hot melt adhesive laminating machine without gluing.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The heat treatment temperatures in step (1) and step (2) are each independently 80-100° C.; Preferably, the speed of the heat treatment in step (1) and step (2) is independently 1.5-2.5 m / s; Preferably, the heat treatment in step (1) and step (2) further includes a cooling step.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The step (3) of gluing the surface of the heat-treated polyester fabric obtained in step (1) specifically includes gluing the side of the brushed surface of the heat-treated polyester fabric obtained in step (1).

7. The preparation method according to any one of claims 1 to 6, characterized in that: The gluing and compounding steps in step (3) are carried out on a hot melt adhesive compounding machine, the gluing temperature is 100-120°C, and the gluing amount is 10-20g / m 2 ; Preferably, the compounding speed in step (3) is 1-2 m / s.

8. The preparation method according to any one of claims 1 to 7, characterized in that: Step (3) further comprises the steps of sealing and heat preservation after compounding; Preferably, the sealing comprises sealing with a thermal insulation film; Preferably, the temperature of the heat preservation treatment is 50-100°C; Preferably, the heat preservation treatment time is 4-5h.

9. A polyester and nylon composite fabric, characterized in that: The polyester and nylon composite fabric is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the polyester and nylon composite fabric as claimed in claim 9 in clothing.

Citation Information

Patent Citations

  • 3D shell fabric realizing no penetration of down feather and preparation method of 3D shell fabric

    CN107048545A

  • Nylon-polyester composite fabric and dyeing and finishing method thereof

    CN117841485A

  • Polyester composite fabric heating device

    CN213861209U