Preparation method and application of sodium metaaluminate

By using sodium hydroxide, ethanol and aluminum hydroxide to perform an alkalization reaction at 55-65°C, the problem of difficult storage and transportation of sodium metaaluminate solution is solved, and low energy consumption and efficient preparation of sodium metaaluminate are achieved. The process flow is simplified and product stability is improved.

CN118754173APending Publication Date: 2024-10-11HUNAN FORTUNE ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410641168.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing production method of sodium metaaluminate, the storage and transportation of sodium metaaluminate solution as an intermediate product is difficult, and the product quality is difficult to guarantee, and it is easily affected by water and carbon dioxide, leading to deterioration.

Method used

Sodium hydroxide is mixed with ethanol and alkalized with aluminum hydroxide at a temperature of 55 to 65°C to obtain sodium metaaluminate through solid-liquid separation, which avoids high-temperature evaporation and crushing and simplifies the process.

Benefits of technology

It reduces the energy consumption and cost of sodium metaaluminate production, improves the stability and implementability of the product, avoids product deterioration problems caused by hydrolysis and carbon dioxide reaction, and simplifies the storage and transportation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a preparation method and application of sodium metaaluminate, and the preparation method comprises the following steps: mixing sodium hydroxide and ethanol to obtain a mixed material; adding aluminum hydroxide into the mixed material for alkalization reaction to obtain sodium metaaluminate; wherein the temperature of the alkalization reaction is 55-65 DEG C, the time of the alkalization reaction is 2-3 hours, and the mass ratio of the aluminum hydroxide to the sodium hydroxide to the ethanol is 100: (56-72): (300-500). The preparation process of the sodium metaaluminate is low in reaction temperature, does not need to set a subsequent evaporation link and a crushing link, simplifies the process, and reduces the cost and the energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium metaaluminate synthesis, and particularly relates to a preparation method of sodium metaaluminate and application thereof. Background Art

[0002] Sodium aluminate, with the chemical formula NaAlO2, is a white crystalline powder. It is hygroscopic, highly soluble in water, and insoluble in ethanol. Its aqueous solution is alkaline. When placed in the air, it can gradually absorb moisture and carbon dioxide in the air to form aluminum hydroxide.

[0003] Sodium aluminate is mainly used in the following industries: (1) Water treatment agent: Sodium aluminate is often used as a flocculant in water treatment to help particles suspended in water aggregate into large particles for easy precipitation or filtration. (2) Textile industry: As an auxiliary agent for dyes and textile fixing agents, it can improve the uniform dispersion and adhesion of dyes. (3) Leather industry: Sodium aluminate can be used as an acid regulator and tanning agent in leather dyeing and tanning. (4) Cosmetics: As a regulator and stabilizer for cosmetics.

[0004] The production methods of sodium aluminate mainly include: (1) Bayer process: crush and grind bauxite, then mix it with caustic soda solution, send it into an autoclave and use high temperature and high pressure to convert the aluminum oxide in the bauxite into sodium aluminate and transfer it into the solution. After separation, the sodium aluminate solution is obtained, and the product is obtained after evaporation. In recent years, the high-pressure dissolution process of alkali solution has developed from intermittent to continuous, and pipeline dissolution has begun to be used in Bayer process production.

[0005] (2) Sintering method: bauxite, soda ash and limestone are ground and mixed, and sintered at a high temperature above 1200℃. The clinker is leached with water, and the sodium aluminate solution after leaching is desiliconized to obtain a refined sodium aluminate solution, which is evaporated to dryness to obtain the product. The sintering method is divided into dry material sintering method and wet material sintering method. At present, the wet material sintering method has basically replaced the dry material sintering method.

[0006] (3) Combined method: The so-called combined method refers to a production method in which the Bayer process and the sintering process are used simultaneously. If the Bayer process is used as the main method and the sintering process is used as the auxiliary method in production, the high-silicon bauxite is treated by the Bayer process, and then the resulting red mud is treated by the sintering process. This is called a series combined method. If the low-silicon bauxite ore is treated by the Bayer process and the high-silicon bauxite is treated by the sintering process, the two methods are carried out simultaneously during the production process, and then the crude liquids obtained by the two methods are combined. This is called a parallel combined method, and the obtained sodium aluminate solution is evaporated to obtain the product.

[0007] (4) Alkaline hydrolysis of aluminum hydroxide: Add crude aluminum hydroxide to a sodium hydroxide solution at 50-80°C and heat to 110°C. Keep warm for 3 hours to obtain a sodium aluminate solution. Evaporate to dryness to obtain the product.

[0008] In the above methods, sodium aluminate solution is used as an intermediate product and then evaporated to dryness or spray dried to obtain sodium aluminate product. This method of preparing sodium aluminate product from sodium aluminate solution is complex and energy-intensive. As a strong base and weak acid salt, sodium aluminate is easily hydrolyzed, and its solution product has poor stability. In addition, it is easy to deteriorate when exposed to carbon dioxide and water in the air, which brings challenges to subsequent storage, transportation and product quality. Summary of the invention

[0009] The invention aims to solve the technical problems that the sodium aluminate solution is used as an intermediate product in the above-mentioned common technology, the storage and transportation are difficult, and the quality of the sodium aluminate product is difficult to ensure. The present invention provides a method for preparing sodium aluminate, comprising the steps of:

[0010] Sodium hydroxide is mixed with ethanol to obtain a mixed material;

[0011] Aluminum hydroxide is added to the mixed material for alkalization reaction to obtain sodium aluminate; wherein the temperature of the alkalization reaction is 55-65°C, the time of the alkalization reaction is 2-3h, and the mass ratio of the aluminum hydroxide, the sodium hydroxide and the ethanol is 100:56-72:300-500.

[0012] Furthermore, the sodium hydroxide is mixed with ethanol to obtain a mixed material comprising: the sodium hydroxide and the ethanol are mixed under stirring conditions, the stirring is in the form of turbine stirring or centrifugal stirring, and the stirring speed is 300-500 r / min.

[0013] Furthermore, before adding aluminum hydroxide to the mixture, the mixture is heated to 55-65°C.

[0014] Furthermore, the sodium hydroxide is in the form of flakes and / or powder.

[0015] Furthermore, the step of adding aluminum hydroxide to the mixture for alkalization reaction also includes adding a catalyst, and the catalyst includes tetraethylammonium hydroxide and / or triethylamine.

[0016] Furthermore, the ratio of the aluminum hydroxide, the sodium hydroxide, the ethanol, and the catalyst is 100:(56-72):(300-500):(0.1-0.5).

[0017] Furthermore, adding aluminum hydroxide to the mixed material for alkalization reaction to obtain sodium aluminate also includes, after the alkalization reaction is completed, reducing the liquid temperature after the alkalization reaction to 20-30° C., separating the solid and the liquid, and collecting the solid to obtain the sodium aluminate.

[0018] Furthermore, the sodium aluminate is dried at a temperature of 50 to 70° C. and for a time of 1 to 2 hours.

[0019] Furthermore, the ethanol includes the first ethanol obtained by condensing and recovering the ethanol evaporated during the alkalization reaction, and the second ethanol obtained by separating the solid and the liquid after the liquid temperature drops to 20-30° C. after the alkalization reaction and collecting the liquid.

[0020] The present invention also provides an application of the preparation method of sodium metaaluminate as described in any one of the above in the industrial production of sodium metaaluminate.

[0021] Compared with the prior art, the present invention has at least the following advantages:

[0022] The present invention provides a method for preparing sodium metaaluminate. The raw materials include aluminum hydroxide, sodium hydroxide and ethanol in a mass ratio of 100:(56-72):(300-500). The main reaction formula and reaction mechanism are as follows:

[0023] Reaction formula: CH3CH2OH+NaOH→CH3CH2ONa+H2O Formula ①

[0024] Al(OH)3+CH3CH2ONa+H2O→NaAl(OH)4+CH3CH2OH Formula ②

[0025] Reaction mechanism: Sodium ethoxide is a white to slightly yellow hygroscopic powder, which is rapidly hydrolyzed into sodium hydroxide and ethanol when in contact with water. Therefore, formula ① is a reversible reaction, and the reaction direction is difficult to maintain in a positive direction. After aluminum hydroxide is added, the water generated by formula ① is continuously consumed during the reaction of aluminum hydroxide, and formula ① is continuously carried out in a positive direction. The temperature control of 55 to 65° C. and the design of the raw material ratio (the mass ratio of aluminum hydroxide, the sodium hydroxide and the ethanol is 100:(56-72):(300 to 500)) ensure the production efficiency of the sodium aluminate product, and overcome the technical prejudice that ethanol cannot be involved in the preparation of sodium aluminate in the commonly used technology.

[0026] On the one hand, sodium aluminate is insoluble in ethanol. In the present invention, ethanol provides a liquid environment for sodium aluminate to react. Sodium aluminate is precipitated in solid form after synthesis. At this time, solid-liquid separation can complete the extraction of solid sodium aluminate. This effectively avoids the negative impact of using sodium aluminate solution as an intermediate product on storage, transportation and even product quality in the common technology.

[0027] In the commonly used technology, the liquid environment of the sodium aluminate synthesis reaction is water. Based on the above, sodium aluminate is prone to hydrolysis, resulting in fluctuations in the solute composition. At the same time, when the sodium aluminate aqueous solution is exposed to the air, it is easy to capture carbon dioxide in the air, causing a reaction that causes the product to deteriorate. Therefore, the sodium aluminate solution has high requirements for the storage conditions of the storage container and needs to be sealed in a plastic barrel resistant to strong alkali. At the same time, the transportation cost of the sodium aluminate solution is high and it is not suitable for long-distance transportation, which brings inconvenience to the application and production of sodium aluminate.

[0028] On the other hand, due to the change in the types of raw materials (including only sodium hydroxide, ethanol and aluminum hydroxide), the activation energy required for the synthesis reaction of sodium aluminate is reduced, and sodium aluminate can be rapidly synthesized within a temperature range of 55 to 65° C. while ensuring the synthesis efficiency.

[0029] In the commonly used technology, the process of combining sodium hydroxide and aluminum hydroxide to form sodium aluminate requires a reaction at a high temperature of 110°C. After the reaction is completed, the sodium aluminate solution is evaporated to a high temperature of 130-150°C. Since sodium aluminate cannot be concentrated, crystallized, or filtered to obtain sodium aluminate crystals, it is necessary to evaporate the sodium aluminate solution to a high temperature of 130-150°C, evaporate the water, and obtain solid sodium aluminate. Since the evaporated solid sodium aluminate will form large lumps, the obtained sodium aluminate solid needs to be crushed later.

[0030] The sodium aluminate preparation process of the present application has a low reaction temperature and does not require subsequent evaporation and crushing steps. It simplifies the process, reduces costs and energy consumption, and avoids workshop pollution and product loss caused by the crushing of sodium aluminate blocks, greatly improving the feasibility and industrial value of the technical solution of the present application. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0033] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention.

[0034] The present invention provides a method for preparing sodium metaaluminate, which is characterized by comprising the steps of:

[0035] S1. Sodium hydroxide and ethanol are mixed to obtain a mixed material.

[0036] In some embodiments, the concentration of ethanol can be greater than 95%. The reduction of water content in ethanol is conducive to the positive progress of formula ① (CH3CH2OH+NaOH→CH3CH2ONa+H2O).

[0037] Exemplarily, the ethanol may be anhydrous ethanol.

[0038] Exemplarily, aluminum hydroxide and sodium hydroxide are in solid state, the purity of aluminum hydroxide may be 98%, and the purity of sodium hydroxide may be 96%.

[0039] In some embodiments, sodium hydroxide can be added into ethanol to improve the uniformity of sodium hydroxide in ethanol.

[0040] Since sodium hydroxide is insoluble in ethanol, stirring can be started before sodium hydroxide is added to ethanol, and then ethanol is added to sodium hydroxide. Exemplarily, the stirring speed can be 300-500 r / min, and the stirring form can be turbine stirring or centrifugal stirring.

[0041] As another example, a reaction kettle can be used to hold ethanol and sodium hydroxide, and the stirring function of a stirrer can be used to optimize the homogenization effect.

[0042] In some embodiments, the sodium hydroxide may be in a solid state, and may be in the form of flakes and / or powder.

[0043] Sodium hydroxide can be slowly added to ethanol to increase the reaction rate of sodium hydroxide and ethanol as much as possible.

[0044] In other embodiments, sodium hydroxide is mixed with ethanol to obtain a mixed material, which further includes: the mixed material includes a catalyst, and the catalyst includes an organic base such as tetraethylammonium hydroxide or triethylamine. The addition of the catalyst can further reduce the activation energy of the reaction, increase the reaction rate, and thus improve the production efficiency of sodium aluminate.

[0045] Exemplarily, the catalyst can be added before the sodium hydroxide is added, can be added after the sodium hydroxide is added, or can be added into the ethanol together with the sodium hydroxide.

[0046] As another example, the ratio of the aluminum hydroxide, the sodium hydroxide, the ethanol, and the catalyst is 100:(56-72):(300-500):(0.1-0.5).

[0047] S2. Add aluminum hydroxide to the mixed material for alkalization reaction to obtain sodium aluminate; wherein the temperature of the alkalization reaction is 55-65°C, the time of the alkalization reaction is 2-3h, and the mass ratio of the aluminum hydroxide, the sodium hydroxide and the ethanol is 100:(56-72):(300-500).

[0048] In some embodiments, before adding aluminum hydroxide to the mixture, the mixture is heated to 55-65° C. to provide an excellent reaction environment for the subsequent alkalization reaction.

[0049] Since the temperature of the mixed material is 55-65°C, which is close to the boiling point of ethanol (78.3°C), ethanol gas will appear in the reaction space. In order to improve the cleanliness of the process, the condenser cooling water can be started when the temperature starts to rise to condense and reflux the ethanol, and continue to participate in a new round of sodium aluminate synthesis reaction as the first ethanol.

[0050] In some embodiments, the measured solid aluminum hydroxide can be slowly added into the reactor, and the adding time lasts for 30 to 50 minutes.

[0051] In some embodiments, adding aluminum hydroxide to the mixed material for alkalization reaction to obtain sodium aluminate also includes, after the alkalization reaction is completed, reducing the liquid temperature after the alkalization reaction to 20-30°C, separating the solid and the liquid, collecting the solid to obtain the sodium aluminate, and collecting the liquid as a second ethanol.

[0052] Exemplarily, solid-liquid separation can be achieved by suction filtration.

[0053] The ethanol comprises the first ethanol obtained by condensing and recovering the evaporated ethanol and the second ethanol obtained by separating the solid and the liquid and collecting the liquid after the liquid temperature drops to 20-30° C. after the alkalization reaction.

[0054] The second ethanol can be used for no more than 3 to 5 times. When the second ethanol reaches the maximum number of times, it can be distilled and recovered to reduce the water content in the ethanol and then put into use as ethanol.

[0055] In some embodiments, the sodium aluminate may be dried to remove the residual ethanol in the sodium aluminate solid. Since the boiling point of ethanol is relatively low, the drying temperature may be 50 to 70° C. and the drying time may be 1 to 2 hours.

[0056] It should be noted that, since the hydrophilicity of sodium aluminate is stronger than that of sodium ethoxide, formula ① can proceed forward continuously, and the reaction rate of the reaction in formula ① is increased only after aluminum hydroxide is added. Therefore, the alkalization reaction includes both the reaction in formula ① and the reaction in formula ②.

[0057] Reaction formula: CH3CH2OH+NaOH→CH3CH2ONa+H2O Formula ①

[0058] Al(OH)3+CH3CH2ONa+H2O→NaAl(OH)4+CH3CH2OH formula ②

[0059] Compared with the prior art, the present invention has at least the following advantages:

[0060] The present invention provides a method for preparing sodium metaaluminate. The raw materials include aluminum hydroxide, sodium hydroxide and ethanol in a mass ratio of 100:(56-72):(300-500). The main reaction formula and reaction mechanism are as follows:

[0061] Reaction formula: CH3CH2OH+NaOH→CH3CH2ONa+H2O Formula ①

[0062] Al(OH)3+CH3CH2ONa+H2O→NaAl(OH)4+CH3CH2OH formula ②

[0063] Reaction mechanism: Sodium ethoxide is a white to slightly yellow hygroscopic powder, which is rapidly hydrolyzed into sodium hydroxide and ethanol when in contact with water. Therefore, formula ① is a reversible reaction, and the reaction direction is difficult to maintain in a positive direction. After aluminum hydroxide is added, the water generated by formula ① is continuously consumed during the aluminum hydroxide reaction, and formula ① is continuously carried out in a positive direction. The temperature control of 55 to 65° C. and the design of the raw material ratio (the mass ratio of aluminum hydroxide, the sodium hydroxide and the ethanol is 100:56-72:300 to 500) ensure the production efficiency of the sodium aluminate product, and overcome the technical prejudice that ethanol cannot participate in the preparation of sodium aluminate in the commonly used technology.

[0064] On the one hand, sodium aluminate is insoluble in ethanol. In the present invention, ethanol provides a liquid environment for the sodium aluminate to react. After the sodium aluminate is synthesized, it precipitates in a solid form. At this time, the solid-liquid separation can complete the extraction of solid sodium aluminate.

[0065] In the conventional technology, the liquid environment of the sodium aluminate synthesis reaction is water. Based on the above, sodium aluminate is prone to hydrolysis reaction, resulting in fluctuations in solute composition. At the same time, when the sodium aluminate solution (since sodium aluminate is insoluble in ethanol but soluble in water, the sodium aluminate solution is assumed to be a sodium aluminate aqueous solution with water as the solvent, the same below) is exposed to the air, it is easy to capture carbon and water in the air, and the reaction causes the product to deteriorate. Therefore, the sodium aluminate solution has high requirements for the storage conditions of the storage container and needs to be sealed in a plastic barrel resistant to strong alkali. At the same time, the transportation cost of the sodium aluminate solution is high and it is not suitable for long-distance transportation, which brings inconvenience to the application and production of sodium aluminate.

[0066] On the other hand, due to the change in the types of raw materials (including only sodium hydroxide, ethanol and aluminum hydroxide), the activation energy required for the synthesis reaction of sodium aluminate is reduced, and sodium aluminate can be rapidly synthesized within a temperature range of 55 to 65° C. while ensuring the synthesis efficiency.

[0067] In the commonly used technology, the process of combining sodium hydroxide and aluminum hydroxide to form sodium aluminate requires a reaction at a high temperature of 110°C. After the reaction is completed, the sodium aluminate solution is evaporated to a high temperature of 130-150°C. Since sodium aluminate is easy to form sodium tetrahydroxyaluminate when combined with water, which in turn affects the purity of the product, sodium aluminate cannot be concentrated, crystallized, or filtered to obtain sodium aluminate crystals. It is necessary to evaporate the sodium aluminate solution to a high temperature of 130-150°C and evaporate it to dryness to obtain solid sodium aluminate. Since the solid sodium aluminate after evaporation will form large lumps, the obtained sodium aluminate solid needs to be crushed later.

[0068] The sodium aluminate preparation process of the present application has a low reaction temperature and does not require subsequent evaporation and crushing steps. It simplifies the process, reduces costs and energy consumption, and avoids workshop pollution and product loss caused by the crushing of sodium aluminate blocks, greatly improving the feasibility and industrial value of the technical solution of the present application.

[0069] In order to facilitate those skilled in the art to further understand the present invention, examples are given below:

[0070] Example 1

[0071] A stainless steel reactor with a volume of 1000 L was selected, and aluminum hydroxide, sodium hydroxide, ethanol, and tetraethylhydroxylamine catalyst were prepared in a mass ratio of 100:56:300:0.1.

[0072] Add the measured ethanol into the reactor and start the stirrer at a speed of 300 r / min;

[0073] Adding measured sodium hydroxide solid into the reaction kettle to obtain a mixed material;

[0074] Start the heating system of the reactor to raise the temperature of the mixed material to 55°C; while starting to heat up, start the cooling water of the condenser to condense and reflux the ethanol.

[0075] Slowly add the measured solid aluminum hydroxide into the reactor for alkalization reaction, and the addition time lasts for 30 minutes;

[0076] After the addition of aluminum hydroxide was completed, the temperature was maintained at 55°C and the reaction was continued for 2 hours;

[0077] After the alkalization reaction is completed, the mixture is cooled to 30° C. and filtered to obtain solid sodium aluminate. The filtered solid sodium aluminate is dried at 50° C. for 2 h to obtain dry solid sodium aluminate.

[0078] Table 1. Product performance test data

[0079]

[0080] Example 2

[0081] A stainless steel reactor with a volume of 1000 L was selected, and aluminum hydroxide, sodium hydroxide, ethanol, and tetraethylhydroxylamine catalyst were prepared in a mass ratio of 100:65:300:0.3.

[0082] Add the measured ethanol into the reactor and start the stirrer at a speed of 300 r / min;

[0083] Adding measured sodium hydroxide solid into the reaction kettle to obtain a mixed material;

[0084] Start the heating system of the reactor to raise the temperature of the mixed material to 60°C; while starting to heat up, start the cooling water of the condenser to condense and reflux the ethanol.

[0085] Slowly add the measured solid aluminum hydroxide into the reactor for alkalization reaction, and the addition time lasts for 30 minutes;

[0086] After the addition of aluminum hydroxide is completed, the temperature is maintained at 60°C and the reaction is continued for 2 hours;

[0087] After the alkalization reaction is completed, the mixture is cooled to 30° C. and filtered to obtain solid sodium aluminate. The filtered solid sodium aluminate is dried at 60° C. for 2 h to obtain dry solid sodium aluminate.

[0088] Table 2. Product performance test data

[0089]

[0090] Comparative Example 1

[0091] Select a stainless steel reactor with a volume of 1000L, and prepare aluminum hydroxide, sodium hydroxide, and ethanol in a mass ratio of 100:56:300.

[0092] Add the measured ethanol into the reactor and start the stirrer at a speed of 300 r / min;

[0093] Adding measured sodium hydroxide solid into the reaction kettle to obtain a mixed material;

[0094] Start the heating system of the reactor to raise the temperature of the material to 55°C; while the temperature starts to rise, start the cooling water of the condenser to condense and reflux the ethanol.

[0095] Slowly add the measured solid aluminum hydroxide into the reactor for alkalization reaction, and the addition time lasts for 30 minutes;

[0096] After the addition of aluminum hydroxide was completed, the temperature was maintained at 55°C and the reaction was continued for 2 hours;

[0097] After the reaction is completed, the mixture is cooled to 30° C. and filtered to obtain solid sodium aluminate. The filtered solid sodium aluminate is dried at 50° C. for 2 h to obtain dry solid sodium aluminate.

[0098] Table 3. Product performance test data

[0099]

[0100]

[0101] Comparative Example 2

[0102] A stainless steel reactor with a volume of 1000 L was selected, and aluminum hydroxide, sodium hydroxide, ethanol, and tetraethylhydroxylamine catalyst were prepared in a mass ratio of 100:65:300:0.3.

[0103] Add the measured ethanol into the reactor and start the stirrer at a speed of 300 r / min;

[0104] Adding measured sodium hydroxide solid into the reaction kettle to obtain a mixed material;

[0105] Start the heating system of the reactor to raise the temperature of the mixed material to 40°C; while starting to heat up, start the cooling water of the condenser to condense and reflux the ethanol.

[0106] Slowly add the measured solid aluminum hydroxide into the reactor for 30 minutes;

[0107] After the addition of aluminum hydroxide was completed, the temperature was maintained at 40°C and the reaction was continued for 2 hours;

[0108] After the reaction is completed, the mixture is cooled to 30° C. and filtered to obtain solid sodium aluminate. The filtered solid sodium aluminate is dried at 60° C. for 2 h to obtain dry solid sodium aluminate.

[0109] Table 4. Product performance test data

[0110]

[0111] Comparative Examples 1 and 2 show that adding a catalyst and increasing the reaction temperature can effectively accelerate the reaction rate.

[0112] The above technical solutions of the present invention are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention specification under the technical concept of the present invention, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for preparing sodium metaaluminate, characterized in that: Includes steps: Sodium hydroxide is mixed with ethanol to obtain a mixed material; Aluminum hydroxide is added to the mixed material for alkalization reaction to obtain sodium aluminate; wherein the temperature of the alkalization reaction is 55-65°C, the time of the alkalization reaction is 2-3h, and the mass ratio of the aluminum hydroxide, the sodium hydroxide and the ethanol is 100:56-72:300-500.

2. The preparation method according to claim 1, characterized in that: The sodium hydroxide and ethanol are mixed to obtain a mixed material comprising: the sodium hydroxide and the ethanol are mixed under stirring conditions, the stirring is in the form of turbine stirring or centrifugal stirring, and the stirring speed is 300-500 r / min.

3. The preparation method according to claim 1, characterized in that: Before adding the aluminum hydroxide to the mixed material, the mixed material is heated to 55-65°C.

4. The preparation method according to claim 1, characterized in that: The sodium hydroxide is in the form of flakes and / or powder.

5. The preparation method according to claim 1, characterized in that: The step of adding aluminum hydroxide to the mixed material for alkalization reaction also includes adding a catalyst, and the catalyst includes tetraethylammonium hydroxide and / or triethylamine.

6. The preparation method according to claim 5, characterized in that: The ratio of the aluminum hydroxide, the sodium hydroxide, the ethanol and the catalyst is 100:56-72:300-500:0.1-0.

5.

7. The preparation method according to claim 1, characterized in that: The step of adding aluminum hydroxide to the mixed material for alkalization reaction to obtain sodium aluminate further comprises: after the alkalization reaction is completed, lowering the liquid temperature after the alkalization reaction to 20-30° C., separating the solid from the liquid, and collecting the solid to obtain the sodium aluminate.

8. The preparation method according to claim 7, characterized in that: The sodium aluminate is dried at a temperature of 50 to 70° C. and a drying time of 1 to 2 hours.

9. The preparation method according to claim 7, characterized in that: The ethanol includes the first ethanol obtained by condensing and recovering the ethanol evaporated during the alkalization reaction, and the second ethanol obtained by collecting the liquid after the liquid temperature drops to 20-30° C. after the alkalization reaction and separating the solid and the liquid.