Preparation method of alumina powder and alumina powder

By controlling the heating and heat preservation of aluminum hydroxide powder in the constant temperature zone of the tube furnace, alumina powders of different phases are prepared, which solves the problems of complexity and low efficiency of the existing alumina powder preparation methods, and achieves high efficiency and high efficiency. Low cost alumina powder production.

CN118754178APending Publication Date: 2024-10-11XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411075908.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing alumina powder preparation methods have complex processes and low efficiency. It is difficult to control the synthesis temperature and morphology, resulting in low yield and high cost. Impurities are easily introduced, affecting particle size distribution and stability.

Method used

The constant temperature zone of the tube furnace is used to heat the aluminum hydroxide powder to the target temperature for decomposition reaction, and the alumina powder of different phases is determined according to the holding time. Pure phase alumina powder is prepared by controlling the heating rate and holding time. Reduce production costs and impurity introduction.

Benefits of technology

The process is simplified, the operating efficiency and output are improved, the production cost is reduced, and the particle size distribution of the alumina powder is ensured to be small and stable, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754178A_ABST
    Figure CN118754178A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a preparation method of aluminum oxide powder and the aluminum oxide powder. The preparation method comprises the following steps: placing aluminum hydroxide powder in a constant-temperature area of a tubular furnace; the heating rate, the target temperature, the heat preservation time and the cooling time of the tubular furnace are determined, the tubular furnace is heated to the target temperature according to the heating rate, so that the aluminum hydroxide powder is subjected to a decomposition reaction at the target temperature, heat preservation treatment is conducted according to the heat preservation time, and a sample is obtained; and determining the phase of the sample, and generating alumina powder with different phases. The preparation efficiency of the aluminum oxide powder can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present disclosure relate to the field of material technology, and in particular, to a method for preparing aluminum oxide powder and aluminum oxide powder. Background Art

[0002] In practical applications, the thermal conductivity of alumina ceramics is often lower than the theoretical value, because the presence of a large amount of oxygen and other impurities and crystal defects will reduce the thermal conductivity. The main method for large-scale preparation of high-quality alumina powder in industry is carbon thermal reduction. However, this method has a high process temperature and a long time, resulting in higher temperatures for subsequent sintering into porcelain, high energy consumption, and high costs. After the reaction, it is also necessary to decarbonize at high temperature in the air, which can easily cause an increase in oxygen impurities. In addition, it also faces the problem of a sharp increase in oxygen content as the particle size decreases and the specific surface area increases.

[0003] In the related art, aluminum nitrate nonahydrate is used as an aluminum source and an oxidant, urea is used as a fuel, and water-soluble organic matter is used as a carbon source to prepare alumina. Aluminum nitrate nonahydrate and melamine can also be used as raw materials, and a precursor with a uniform raw material mixture is prepared by a solution reaction process, and then the precursor is subjected to a carbon thermal reduction reaction in an ammonia atmosphere to prepare nano-alumina. In addition, water-soluble inorganic aluminum salts can be used as aluminum sources, water-soluble organic matter as a carbon source, and one of ammonium nitrate, glycine, alanine, lysine, and citric acid as an auxiliary agent to prepare alumina powder.

[0004] However, in the above method, since urea is used as fuel, the combustion process is fast and the temperature is difficult to control, resulting in the morphology of the synthesized alumina powder being difficult to control. In addition, the precursor preparation process is relatively complicated, the operation process is complicated, the experimental cycle is long, and the time is long, so the preparation efficiency is low. Summary of the invention

[0005] The purpose of the present disclosure is to provide a method for preparing aluminum oxide powder and aluminum oxide powder, thereby overcoming the problem of low efficiency in preparing aluminum oxide powder due to limitations and defects of related technologies, at least to a certain extent.

[0006] According to one aspect of the present disclosure, there is provided a method for preparing alumina powder, comprising: placing aluminum hydroxide powder in a constant temperature zone of a tubular furnace; determining a heating rate, a target temperature, a holding time, and a cooling time of the tubular furnace, heating the tubular furnace to a target temperature by a heating rate so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and performing a holding treatment according to a holding time to obtain a sample; determining a physical phase of the sample to generate alumina powders of different physical phases.

[0007] In some embodiments of the present disclosure, the alumina powder is any one of χ-Al2O3, δ-Al2O3, γ-Al2O3, κ-Al2O3 and α-Al2O3.

[0008] In some embodiments of the present disclosure, the heating rate of the tubular furnace below 1000° C. is a first rate, and the heating rate of the tubular furnace above 1000° C. is a second rate; wherein the first rate is greater than the second rate.

[0009] In some embodiments of the present disclosure, the heating rate is used to heat the tube furnace to a target temperature so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and the sample is obtained by heat preservation treatment according to the heat preservation time, including: heating the temperature of the tube furnace to 650-750°C at a first rate, so that the aluminum hydroxide powder undergoes a decomposition reaction and the heat preservation treatment is performed according to the heat preservation time to prepare a pure phase χ-Al2O3 powder; heating the temperature of the tube furnace to 750-800°C at a first rate so that the aluminum hydroxide powder undergoes a decomposition reaction and the heat preservation treatment is performed according to the heat preservation time to prepare a δ-Al2O3 powder; The temperature of the tubular furnace is increased to 800-840°C at a first rate to decompose the aluminum hydroxide powder and perform heat preservation treatment according to the heat preservation time to prepare pure phase γ-Al2O3 powder; the temperature of the tubular furnace is increased to 900-1050°C at a first rate to decompose the aluminum hydroxide powder and perform heat preservation treatment according to the heat preservation time to prepare pure phase κ-Al2O3 powder; the temperature of the tubular furnace is increased to 1000°C at a first rate, and then increased to 1150-1300°C at a second rate to decompose the aluminum hydroxide powder and perform heat preservation treatment according to the heat preservation time to prepare pure phase α-Al2O3 powder.

[0010] In some embodiments of the present disclosure, the insulation time is: the insulation time of pure phase χ-Al2O3 powder is 2 to 4 hours, the insulation time of pure phase δ-Al2O3 powder is 3 to 5 hours, the insulation time of pure phase γ-Al2O3 powder is 3 to 5 hours, the insulation time of pure phase θ-Al2O3 powder is 2 to 4 hours, and the insulation time of pure phase α-Al2O3 powder is 2 to 4 hours.

[0011] In some embodiments of the present disclosure, the method further includes: after the heat preservation treatment is performed according to the heat preservation time, the tube furnace is subjected to a temperature reduction treatment.

[0012] In some embodiments of the present disclosure, the step of cooling the tube furnace comprises:

[0013] When the target temperature is above 1000°C, the temperature is lowered to the preset temperature at a third rate, and after reaching the preset temperature, the furnace is cooled to room temperature; the third rate is greater than the second rate and less than the first rate; when the target temperature is below 1000°C, the furnace is cooled to room temperature.

[0014] In some embodiments of the present disclosure, determining the physical phase of the sample includes: performing X-ray diffraction on the sample to determine the physical phase of the sample.

[0015] In some embodiments of the present disclosure, the X-ray diffraction angle ranges from 5 to 95°.

[0016] According to one aspect of the present disclosure, there is provided an alumina powder, wherein the alumina powder is prepared according to any one of the above-mentioned methods for preparing alumina powder.

[0017] In the technical solution provided in the embodiments of the present disclosure, on the one hand, it is only necessary to place the aluminum hydroxide powder in the constant temperature zone of the tubular furnace so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and alumina powder of different phases can be obtained according to different target temperatures. The process flow is relatively simple, so the operation efficiency is high, the yield is high, the output is large, and the production cost is reduced. On the other hand, since alumina powder can be prepared only based on aluminum hydroxide powder, the raw material price is low and it is safe. On another hand, it is only necessary to place the aluminum hydroxide powder in the constant temperature zone of the tubular furnace, and no complicated mechanical equipment is required. During the preparation process, since the alumina powder of different phases can be determined according to the target temperature, no impurity elements will be introduced, and the particle size distribution range of the prepared alumina powder is small, and no further classification and processing is required. Because of its high stability, it is suitable for mass production.

[0018] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0020] Figure 1 A flow chart schematically shows a method for preparing aluminum oxide powder in an embodiment of the present disclosure.

[0021] Figure 2 The XRD diagram of the mixture prepared in the related art is schematically shown.

[0022] Figure 3 The XRD diagram of χ-Al2O3 powder in the embodiment of the present disclosure is schematically shown.

[0023] Figure 4 The XRD diagram of δ-Al2O3 powder in the embodiment of the present disclosure is schematically shown.

[0024] Figure 5 The XRD diagram of γ-Al2O3 powder in the embodiment of the present disclosure is schematically shown.

[0025] Figure 6 The XRD diagram of κ-Al2O3 powder in the embodiment of the present disclosure is schematically shown.

[0026] Figure 7 The XRD diagram of α-Al2O3 powder in the embodiment of the present disclosure is schematically shown. DETAILED DESCRIPTION

[0027] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.

[0028] The terms "a", "an", "the" and "said" used in this specification are used to indicate the presence of one or more elements / components, etc.; the terms "including" and "having" are used to express an open-ended inclusion and mean that there may be additional elements / components, etc. in addition to the listed elements / components, etc.; the terms "first" and "second" etc. are used only as labels and are not intended to limit the quantity of their objects.

[0029] Alumina has excellent properties such as high melting point, high hardness, high mechanical strength, good wear resistance, and stable chemical properties. It is one of the materials with the widest application volume and application range. However, due to the difference in its crystal structure, it exhibits different properties, so alumina of different crystal forms are used in different fields. According to the temperature at which the phase exists stably from low to high, it can be divided into χ-Al2O3, δ-Al2O3, γ-Al2O3, κ-Al2O3 and α-Al2O3, among which α-Al2O3 is the most stable crystal structure.

[0030] χ-Al2O3 belongs to the hexagonal crystal system. The oxygen stacking layer of χ-Al2O3 is very similar to mica and β-χ-Al2O3, and is arranged in ABAC-ABAC or ABAC-CABA. It is mainly used in the drying and dehydration of air, natural gas, and petroleum cracking gas, defluorination of drinking water, special catalyst for the production of hydrogen peroxide by quinone method, dechlorination of sticky resin, catalyst carrier, air separation and oxygen production. δ-Al2O3 is a new crystal form of alumina with a hexagonal crystal system. Compared with α-Al2O3, δ-Al2O3 has a higher specific surface area and better catalytic performance, so it is widely used in catalysts, adsorbents and other fields; γ-Al2O3 has a spinel crystal structure and is easily soluble in acid and alkali solutions. At the same time, this type of alumina has a high specific surface area and chemical activity, and its structure is fluffy, with high porosity, and has extremely strong resistance to extrusion and adsorption. It is widely used as a catalyst carrier and as a filler to improve the cycle life of batteries; θ-Al2O3 is a transitional alumina between low-temperature and high-temperature types, and belongs to a metastable structure. Therefore, its reaction activity is greater than that of a single α-Al2O3, and it has broad application prospects in the preparation of transparent ceramic catalysts, nanomaterials and other fields; α-Al2O3 is an inorganic compound and an ionic crystal. α-Al2O3 has many excellent properties, such as high hardness, high strength, high melting point (2050℃), and can be ionized at high temperatures. Therefore, it is widely used in single crystal materials, ceramic materials, semiconductor materials, medical devices and many other fields. With the development of industrial technology, the application scope of alumina of different phases in different fields is becoming wider and wider, and the demand is also increasing. However, the existing alumina preparation methods can no longer meet the increasing demand. Therefore, it is very important to prepare alumina of different phases at low cost, high yield and good quality.

[0031] At present, the preparation methods of alumina powders of different physical phases include: alcohol aluminum hydrolysis method, sol-gel method, high-energy mechanical ball milling method, etc.

[0032] Among them, the alcohol aluminum hydrolysis method: preparing alumina powder by neutralizing aluminum salt or utilizing alcohol aluminum decomposition to obtain aluminum colloid, pseudoboehmite or boehmite, and then activating it. This method has problems such as complicated process flow, low yield, and high production cost.

[0033] Sol-gel method: The sol-gel method uses organic or inorganic aluminum salts as reaction raw materials, stirs and mixes these raw materials evenly in a specific solvent, then adds water to hydrolyze and polycondense them to form a sol in the solution, and then ages and dries the sol, the sol will be transformed into a fluffy gel, which is then ground and calcined to prepare alumina particles. However, since the sol-gel method mostly uses organic aluminum salts, there are disadvantages such as high raw material prices and high toxicity.

[0034] High-energy mechanical ball milling method: High-energy mechanical ball milling method is to prepare alumina nanoparticles through high-energy ball milling without external heat supply, but its preparation requires more complex mechanical equipment, impurity elements are easily introduced during the preparation process, and the prepared particle size distribution range is wide, requiring further processing.

[0035] The above preparation methods have some defects, so it is of great significance to develop a method with a simple preparation process and easy large-scale production.

[0036] In the related art, alumina powder can be prepared according to the following steps, specifically including:

[0037] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0038] Step 2: Raise the temperature of the tube furnace to 1100°C at a rate of ≤10°C / min and keep it at that temperature for 3 hours to decompose the aluminum hydroxide powder;

[0039] Step 3: Cool to room temperature in the furnace and collect the product. Perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain a mixture of κ-Al2O3, α-Al2O3 and θ-Al2O3.

[0040] It can be seen that controlling the decomposition temperature and decomposition time is a prerequisite for obtaining a single pure phase of alumina.

[0041] In order to solve the above technical problems, the present invention provides a method for preparing aluminum oxide powder in an embodiment of the present invention, which is used to prepare aluminum oxide powder. Figure 1 As shown in , it mainly includes the following steps:

[0042] In step S110, aluminum hydroxide powder is placed in a constant temperature zone of a tube furnace;

[0043] In step S120, the heating rate, target temperature, holding time, and cooling time of the tube furnace are determined, and the tube furnace is heated to the target temperature by the heating rate so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and the sample is obtained by holding the temperature for the holding time;

[0044] In step S130, the physical phase of the sample is determined to generate aluminum oxide powders of different physical phases.

[0045] In the technical solution of the disclosed embodiment, on the one hand, it is only necessary to put the aluminum hydroxide powder into a constant temperature zone so that the aluminum hydroxide powder decomposes at the target temperature, and the aluminum oxide powder of different phases can be determined. The process flow is relatively simple, so the operation efficiency is high, the yield is high, the output is large, and the production cost is reduced. On the other hand, since the aluminum oxide powder can be prepared only based on the aluminum hydroxide powder, the raw material price is low and it is safe. On the other hand, it is only necessary to place the aluminum hydroxide powder in the constant temperature zone of the tubular furnace, and no complicated mechanical equipment is required. During the preparation process, since the aluminum oxide powder of different phases can be determined according to the target temperature, no impurity elements will be introduced, and the particle size distribution range of the prepared aluminum oxide powder is small, and no further classification and processing is required. Because of its high stability, it is suitable for mass production.

[0046] Next, combine Figure 1 The preparation method of the alumina powder in the embodiment of the present disclosure is described in detail.

[0047] In step S110, aluminum hydroxide powder is placed in a constant temperature zone of a tube furnace.

[0048] In the embodiment of the present disclosure, the particle size of the aluminum hydroxide powder can be 2 to 10 μm, which is determined according to actual needs. The weight of the aluminum hydroxide powder can be determined according to actual needs, for example, 35 g. The tubular furnace can be a high-temperature tubular furnace.

[0049] For example, aluminum hydroxide powder can be placed in a constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier.

[0050] In step S120, the heating rate, target temperature, holding time, and cooling time of the tube furnace are determined, and the tube furnace is heated to the target temperature by the heating rate so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and the sample is obtained by holding treatment according to the holding time.

[0051] In the embodiment of the present disclosure, the tubular furnace is programmed. Exemplarily, the heating rate, target temperature, insulation time and cooling time of the tubular furnace can be set. Among them, the heating rate is used to indicate the rate of heating to the target temperature, and the heating rate may vary according to the preset temperature. When the temperature is below the preset temperature, the heating rate may be a first rate. When the temperature is above the preset temperature, the heating rate may be a second rate. Among them, the first rate may be greater than the second rate. The preset temperature may be 1000°C. Exemplarily, when the temperature is above the preset temperature, the first rate used to indicate the heating rate may be a rate of ≤10°C / min. When the temperature is above the preset temperature, the second rate used to indicate the heating rate may be a rate of ≤3°C / min.

[0052] The target temperature may be a temperature for causing the aluminum hydroxide powder to undergo a decomposition reaction. The target temperature may vary depending on the type of aluminum oxide powder being prepared. For example, when the aluminum oxide powder is pure phase χ-Al2O3 powder, the target temperature may be 650-750°C; when the aluminum oxide powder is pure phase δ-Al2O3 powder, the target temperature may be 750-800°C; when the aluminum oxide powder is pure phase γ-Al2O3 powder, the target temperature may be 800-840°C; when the aluminum oxide powder is pure phase κ-Al2O3 powder, the target temperature may be 900-1050°C; when the aluminum oxide powder is pure phase α-Al2O3 powder, the target temperature may be 1150-1300°C.

[0053] The holding time refers to the holding time at the target temperature, which may vary according to the type of alumina powder prepared. For example, when the alumina powder is pure phase χ-Al2O3 powder, the target temperature may be 650-750°C, and the holding time may be 2-4 hours; when the alumina powder is pure phase δ-Al2O3 powder, the target temperature may be 750-800°C, and the holding time may be 3-5 hours; when the alumina powder is pure phase γ-Al2O3 powder, the target temperature may be 800-840°C, and the holding time may be 3-5 hours; when the alumina powder is pure phase κ-Al2O3 powder, the target temperature may be 900-1050°C, and the holding time may be 2-4 hours; when the alumina powder is pure phase α-Al2O3 powder, the target temperature may be 1150-1300°C, and the holding time may be 2-4 hours.

[0054] Cooling time refers to the time it takes to drop from the target temperature to room temperature, which is determined based on actual needs.

[0055] Exemplarily, the tube furnace can be heated to a target temperature according to a heating rate, so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and then a heat preservation treatment is performed according to a heat preservation time to obtain a sample.

[0056] Next, continue to refer to Figure 1 As shown in , in step S130, the physical phase of the sample is determined to generate aluminum oxide powders of different physical phases.

[0057] In the disclosed embodiment, after the tubular furnace is programmed, the heating rate, target temperature, holding time, and cooling time are set, and then the aluminum hydroxide powder is decomposed. After the decomposition reaction is completed, the physical phase of the sample can be determined to generate aluminum oxide powders of different physical phases. Exemplarily, the sample can be subjected to X-ray diffraction to determine the physical phase of the sample. During the X-ray diffraction process, the angle range of the X-ray diffraction is 5 to 95°.

[0058] It should be noted that before determining the physical phase of the sample, the tube furnace may also be cooled. Exemplarily, when the target temperature is above 1000°C, the temperature is lowered to the preset temperature at a third rate, and after reaching the preset temperature, the furnace is cooled to room temperature; the third rate is greater than the second rate and less than the first rate. The third rate may be, for example, ≤5°C / min. The preset temperature may be 900°C. After the temperature reaches the preset temperature, the furnace may be cooled to room temperature. When the target temperature is below 1000°C, the furnace is cooled to room temperature.

[0059] Next, the preparation method of the alumina powder in the embodiment of the present disclosure will be specifically described in conjunction with the examples.

[0060] In some embodiments, during the preparation of alumina powder, the target temperature set during the preparation of alumina powder can be adjusted, and the holding time can also be adjusted. For example, when the alumina powder is pure phase χ-Al2O3 powder, the holding time can be 2 hours, 3 hours or 4 hours. The target temperature can be 680°C, 700°C, or 720°C.

[0061] In other embodiments, when the alumina powder is pure phase δ-Al2O3 powder, the target temperature may be 790° C. or 800° C. The holding time may be 3 hours, 4 hours or 5 hours.

[0062] When the alumina powder is pure phase γ-Al2O3 powder, the target temperature may be 810° C., 820° C., or 830° C. The holding time may be 3 hours, 4 hours, or 5 hours.

[0063] When the alumina powder is pure phase κ-Al2O3 powder, the target temperature may be 950° C., 1000° C., or 1050° C. The holding time may be 2 hours, 3 hours, or 4 hours.

[0064] When the alumina powder is pure phase α-Al2O3 powder, the target temperature may be 1150° C., 1200° C., or 1250° C. The holding time may be 2 hours, 3 hours, or 4 hours.

[0065] Next, the preparation method of alumina powder is specifically described with reference to examples.

[0066] Example 1

[0067] The specific process of the preparation method of the alumina powder comprises the following steps:

[0068] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0069] Step 2: Raise the temperature of the tube furnace to 700°C at a rate of ≤10°C / min and keep it at this temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase χ-Al2O3 powder;

[0070] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase χ-Al2O3 powder.

[0071] Example 2

[0072] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0073] Step 2: Raise the temperature of the tube furnace to 680°C at a rate of ≤10°C / min and keep it at this temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase χ-Al2O3 powder;

[0074] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase χ-Al2O3 powder.

[0075] Example 3

[0076] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0077] Step 2: Raise the temperature of the tube furnace to 720°C at a rate of ≤10°C / min and keep it at this temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase χ-Al2O3 powder;

[0078] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase χ-Al2O3 powder.

[0079] Example 4

[0080] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0081] Step 2: Raise the temperature of the tube furnace to 700°C at a rate of ≤10°C / min and keep it at this temperature for 2 hours to decompose the aluminum hydroxide powder to prepare pure phase χ-Al2O3 powder;

[0082] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase χ-Al2O3 powder.

[0083] Example 5

[0084] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0085] Step 2: Raise the temperature of the tube furnace to 700°C at a rate of ≤10°C / min and keep it at this temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase χ-Al2O3 powder;

[0086] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase χ-Al2O3 powder.

[0087] The XRD patterns of the pure phase χ-Al2O3 powders prepared according to Examples 1 to 5 are as follows: Figure 2 shown.

[0088] Example 6

[0089] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0090] Step 2: Raise the temperature of the tube furnace to 800°C at a rate of ≤10°C / min and keep it at that temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase δ-Al2O3 powder;

[0091] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase δ-Al2O3 powder.

[0092] Example 7

[0093] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0094] Step 2: Raise the temperature of the tube furnace to 790°C at a rate of ≤10°C / min and keep it at this temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase δ-Al2O3 powder;

[0095] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase δ-Al2O3 powder.

[0096] Example 8

[0097] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0098] Step 2: Raise the temperature of the tube furnace to 800°C at a rate of ≤10°C / min and keep it at that temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase δ-Al2O3 powder;

[0099] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase δ-Al2O3 powder.

[0100] Example 9

[0101] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0102] Step 2: Raise the temperature of the tube furnace to 800°C at a rate of ≤10°C / min and keep it at that temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase δ-Al2O3 powder;

[0103] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase δ-Al2O3 powder.

[0104] The XRD patterns of the pure phase δ-Al2O3 powders prepared according to Examples 6 to 10 are as follows: Figure 3 shown.

[0105] Example 10

[0106] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0107] Step 2: Raise the temperature of the tube furnace to 820°C at a rate of ≤10°C / min and keep it at that temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase γ-Al2O3 powder;

[0108] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase γ-Al2O3 powder.

[0109] Embodiment 11

[0110] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0111] Step 2: Raise the temperature of the tube furnace to 810°C at a rate of ≤10°C / min and keep it at that temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase γ-Al2O3 powder;

[0112] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase γ-Al2O3 powder.

[0113] Example 12

[0114] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0115] Step 2: Raise the temperature of the tube furnace to 830°C at a rate of ≤10°C / min and keep it at that temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase γ-Al2O3 powder;

[0116] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase γ-Al2O3 powder.

[0117] Example 13

[0118] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0119] Step 2: Raise the temperature of the tube furnace to 820°C at a rate of ≤10°C / min and keep it at that temperature for 5 hours to decompose the aluminum hydroxide powder to prepare pure phase γ-Al2O3 powder;

[0120] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase γ-Al2O3 powder.

[0121] Embodiment 14

[0122] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0123] Step 2: Raise the temperature of the tube furnace to 820°C at a rate of ≤10°C / min and keep it at that temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase γ-Al2O3 powder;

[0124] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase γ-Al2O3 powder.

[0125] The XRD patterns of the pure phase γ-Al2O3 powders prepared according to Examples 10 to 14 are as follows: Figure 4 shown.

[0126] Embodiment 15

[0127] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0128] Step 2: Raise the temperature of the tube furnace to 1000°C at a rate of ≤10°C / min and keep it at that temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase κ-Al2O3 powder;

[0129] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase κ-Al2O3 powder.

[0130] Example 16

[0131] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0132] Step 2: Raise the temperature of the tube furnace to 950°C at a rate of ≤10°C / min and keep it at this temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase κ-Al2O3 powder;

[0133] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase κ-Al2O3 powder.

[0134] Embodiment 17

[0135] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0136] Step 2: Raise the temperature of the tube furnace to 1050°C at a rate of ≤10°C / min and keep it at that temperature for 3 hours to decompose the aluminum hydroxide powder to prepare pure phase κ-Al2O3 powder;

[0137] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase κ-Al2O3 powder.

[0138] Embodiment 18

[0139] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0140] Step 2: Raise the temperature of the tube furnace to 1000°C at a rate of ≤10°C / min and keep it at that temperature for 2 hours to decompose the aluminum hydroxide powder to prepare pure phase κ-Al2O3 powder;

[0141] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase κ-Al2O3 powder.

[0142] Embodiment 19

[0143] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0144] Step 2: Raise the temperature of the tube furnace to 1000°C at a rate of ≤10°C / min and keep it at that temperature for 4 hours to decompose the aluminum hydroxide powder to prepare pure phase κ-Al2O3 powder;

[0145] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase κ-Al2O3 powder.

[0146] The XRD patterns of the pure phase κ-Al2O3 powders prepared according to Examples 15 to 19 are as follows: Figure 5 shown.

[0147] Embodiment 20

[0148] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0149] Step 2: The temperature of the tube furnace is first raised to 1000°C at a rate of ≤10°C / min, then raised to 1200°C at a rate of ≤3°C / min and kept at that temperature for 3h, and then lowered to a preset temperature of 900°C at a rate of ≤5°C / min;

[0150] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase α-Al2O3 powder.

[0151] Embodiment 21

[0152] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0153] Step 2: The temperature of the tube furnace is first raised to 1000°C at a rate of ≤10°C / min, then raised to 1150°C at a rate of ≤3°C / min and kept at that temperature for 3h, and then lowered to a preset temperature of 900°C at a rate of ≤5°C / min;

[0154] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase α-Al2O3 powder.

[0155] Embodiment 22

[0156] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0157] Step 2: The temperature of the tube furnace is first raised to 1000°C at a rate of ≤10°C / min, then raised to 1250°C at a rate of ≤3°C / min and kept at that temperature for 3h, and then lowered to a preset temperature of 900°C at a rate of ≤5°C / min;

[0158] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase α-Al2O3 powder.

[0159] Embodiment 23

[0160] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0161] Step 2: The temperature of the tube furnace is first raised to 1000°C at a rate of ≤10°C / min, then raised to 1200°C at a rate of ≤3°C / min and kept at that temperature for 4 hours, and then lowered to a preset temperature of 900°C at a rate of ≤5°C / min;

[0162] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase α-Al2O3 powder.

[0163] Embodiment 24

[0164] Step 1, weigh 35g of aluminum hydroxide powder with a particle size of 2 to 10 microns, and put the weighed aluminum hydroxide powder into the constant temperature zone of a high-temperature tube furnace using a corundum crucible as a carrier;

[0165] Step 2: The temperature of the tube furnace is first raised to 1000°C at a rate of ≤10°C / min, then raised to 1200°C at a rate of ≤3°C / min and kept at that temperature for 2h, and then lowered to a preset temperature of 900°C at a rate of ≤5°C / min;

[0166] Step 3: Cool to room temperature with the furnace, collect the product, and perform X-ray diffraction test on the collected product in the range of 5 to 95° to obtain pure phase α-Al2O3 powder.

[0167] The XRD patterns of the pure phase α-Al2O3 powders prepared according to Examples 20 to 24 are as follows: Figure 6 shown.

[0168] In summary, in the embodiments of the present disclosure, it is only necessary to place the aluminum hydroxide powder in a constant temperature zone so that the aluminum hydroxide powder decomposes at the target temperature, and the aluminum oxide powder of different phases can be determined. The process flow is relatively simple, so the operation efficiency is high, the yield is high, the output is large, and the production cost is reduced. Since the aluminum oxide powder can be prepared only based on the aluminum hydroxide powder, the raw material price is low and it is safe. It is only necessary to place the aluminum hydroxide powder in the constant temperature zone of the tubular furnace, and no complicated mechanical equipment is required. During the preparation process, since the aluminum oxide powder of different phases can be determined according to the target temperature, no impurity elements will be introduced, and the particle size distribution range of the prepared aluminum oxide powder is small, and no further classification and processing is required. Because of its high stability, it is suitable for large-scale batch production.

[0169] In this exemplary embodiment, a device is also provided. The device may be a device having the aluminum oxide powder, such as a mobile phone, a tablet computer, a laptop computer, a smart bracelet, a smart watch, a smart helmet, smart glasses, a vehicle, a robot, and any type of industrial equipment, etc., as long as the aluminum oxide powder can be contained, and this exemplary embodiment does not specifically limit this.

[0170] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.

[0171] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.

[0172] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A method for preparing aluminum oxide powder, characterized in that: include: Placing aluminum hydroxide powder in a constant temperature zone of a tube furnace; Determine the heating rate, target temperature, holding time, and cooling time of the tube furnace, heat the tube furnace to the target temperature by the heating rate, so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and perform a holding treatment according to the holding time to obtain a sample; The physical phase of the sample is determined, and aluminum oxide powders of different physical phases are generated.

2. The method for preparing alumina powder according to claim 1, characterized in that: The alumina powder is any one of χ-Al2O3, δ-Al2O3, γ-Al2O3, κ-Al2O3 and α-Al2O3.

3. The method for preparing alumina powder according to claim 1, characterized in that: The heating rate of the tubular furnace below 1000° C. is a first rate, and the heating rate of the tubular furnace above 1000° C. is a second rate; wherein the first rate is greater than the second rate.

4. The method for preparing alumina powder according to claim 1, characterized in that: The step of heating the tube furnace to a target temperature by a heating rate so that the aluminum hydroxide powder undergoes a decomposition reaction at the target temperature, and performing a heat preservation treatment according to a heat preservation time to obtain a sample comprises: The temperature of the tube furnace is raised to 650-750° C. at a first rate, so that the aluminum hydroxide powder undergoes a decomposition reaction and is heat-insulated for a certain time to prepare a pure-phase χ-Al2O3 powder; The temperature of the tube furnace is raised to 750-800° C. at a first rate to decompose the aluminum hydroxide powder and then the aluminum hydroxide powder is kept warm for a certain time to prepare the δ-Al2O3 powder. The temperature of the tube furnace is raised to 800-840° C. at a first rate to decompose the aluminum hydroxide powder and then the aluminum hydroxide powder is kept warm for a certain time to prepare pure phase γ-Al2O3 powder. The temperature of the tube furnace is raised to 900-1050° C. at a first rate to decompose the aluminum hydroxide powder and then the aluminum hydroxide powder is kept warm for a certain time to prepare pure phase κ-Al2O3 powder. The temperature of the tube furnace is raised to 1000° C. at a first rate, and then raised to 1150-1300° C. at a second rate to decompose the aluminum hydroxide powder and perform heat preservation treatment according to the heat preservation time to prepare pure phase α-Al2O3 powder.

5. The method for preparing alumina powder according to claim 1, characterized in that: The insulation time is: The insulation time of pure phase χ-Al2O3 powder is 2 to 4 hours, the insulation time of pure phase δ-Al2O3 powder is 3 to 5 hours, the insulation time of pure phase γ-Al2O3 powder is 3 to 5 hours, the insulation time of pure phase θ-Al2O3 powder is 2 to 4 hours, and the insulation time of pure phase α-Al2O3 powder is 2 to 4 hours.

6. The method for preparing alumina powder according to claim 1, characterized in that: The method further comprises: After the heat preservation treatment is carried out according to the heat preservation time, the tube furnace is subjected to a temperature reduction treatment.

7. The method for preparing alumina powder according to claim 1, characterized in that: The step of cooling the tube furnace comprises: When the target temperature is above 1000°C, the temperature is lowered to a preset temperature at a third rate, and after reaching the preset temperature, the temperature is cooled to room temperature with the furnace; the third rate is greater than the second rate and less than the first rate; When the target temperature is below 1000° C., the furnace is cooled to room temperature.

8. The method for preparing alumina powder according to claim 1, characterized in that: Determining the physical phase of the sample comprises: X-ray diffraction is performed on the sample to determine the phase of the sample.

9. The method for preparing alumina powder according to claim 8, characterized in that: The X-ray diffraction angle range is 5 to 95 degrees.

10. An alumina powder, characterized in that: The alumina powder is prepared according to the method for preparing alumina powder according to any one of claims 1-9.

Citation Information

Cited By

  • Preparation method and application of alumina supported ruthenium catalyst

    CN119657124A