Master glass, microcrystalline glass, chemically strengthened microcrystalline glass and glass preparation method
By introducing Na2O and K2O into the glass-ceramics, combined with heat treatment and chemical strengthening treatment, a stable lithium disilicate crystal phase and a compressive stress layer are formed, which solves the problem of low chemical stability of the glass-ceramics and achieves better mechanical properties. Performance and chemical stability for protective glass covers and windows in electronic devices and home appliances.
Patent Information
- Application Number
- CN202410868061.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The chemical stability of the glass phase of existing glass-ceramics after chemical strengthening treatment is low, resulting in unsatisfactory environmental reliability test results.
By introducing Na2O and K2O as glass components, the mixed alkali effect is exerted to improve the chemical stability of the glass, and the lithium disilicate crystal phase and compressive stress layer are formed through heat treatment and chemical strengthening treatment to improve the mechanical properties and chemical stability of the glass. .
It significantly improves the chemical stability and mechanical properties of glass-ceramics, extends the effective duration of the double 85 test, reduces the difficulty of glass melting, and improves the transparency and drop resistance of the glass.
Smart Images

Figure SMS_1 
Figure SMS_10 
Figure SMS_11
Abstract
Description
Technical Field
[0001] The present application relates to the field of material technology, and in particular to the field of glass technology. Specifically, the present application discloses a plain glass, a microcrystalline glass, a chemically strengthened microcrystalline glass, and a glass preparation method. Background Art
[0002] Glass-ceramics is a special inorganic material with nanocrystals in the glass phase, which has good thermal stability and high mechanical strength, impact resistance and transparency. Glass-ceramics has received extensive attention in the industry because of its superior performance compared to ordinary glass. It is currently widely used in the front and back covers of electronic devices (such as mobile phones, tablets, etc.) or windows of household appliances (such as microwave ovens, ovens, etc.).
[0003] In the related technology, microcrystalline glass needs to undergo chemical strengthening treatment to improve various mechanical performance indicators. However, the current microcrystalline glass has low chemical stability of the glass phase, resulting in unsatisfactory test results in environmental reliability tests such as the double 85 test.
[0004] It is worth noting that the techniques described in this section are not necessarily techniques that have been previously conceived or employed. Unless otherwise indicated, it should not be assumed that any technique described in this section is considered to be prior art simply because it is included in this section. Similarly, unless otherwise indicated, the issues mentioned in this section should not be considered to have been recognized in any prior art. Summary of the invention
[0005] The present application provides a plain glass, a microcrystalline glass, a chemically strengthened microcrystalline glass and a glass preparation method, aiming to solve at least one of the problems in the related art to a certain extent.
[0006] In a first aspect, the present application provides a plain glass, the components of which, by weight percentage, include: SiO2: 45-65%, Al2O3: 1-12%, Li2O: 14-18%, B2O3: 2-6%, R2O: 5-6%; wherein the R2O includes Na2O and K2O.
[0007] Optionally, the components of the plain glass, measured in weight percentage, further include: P2O5: 0.1-3.5%, and / or, ZrO2: 0.1-3%, and / or, CaO: 0-2%, and / or, ZnO: 0-9%, and / or, MgO: 0.1-7%, and / or, SrO: 0-0.3%, and / or, BaO: 0-2%, and / or, TiO2: 0-1.5%, and / or, clarifier: 0.2-2.5%.
[0008] Optionally, the components of the plain glass include, by weight percentage, SiO2: 50-53%, Al2O3: 5-10%, Li2O: 14-16%, and B2O3: 3-5%.
[0009] Optionally, the components of the plain glass, measured in weight percentage, satisfy any one of the following conditions: ZrO2+P2O5+TiO2: 4.5-6.5%; ZnO+MgO+CaO+BaO+SrO: 2.7-16.3%; Y2O3+Nb2O3+La2O3: 0-1.3%.
[0010] Optionally, the components of the plain glass, measured in weight percentage, satisfy any one of the following conditions: (Li2O+Na2O+K2O) / B2O3: 5 to 11; (Li2O+Na2O+K2O) / Al2O3: 1.75 to 5.5; (Li2O+Na2O+K2O) / (SiO2+B2O3+Al2O3): 0.31 to 0.39.
[0011] Optionally, the components of the plain glass, measured in weight percentage, further include: Bi2O3: 0.1-3%.
[0012] Optionally, the components of the plain glass, measured in weight percentage, further include: Bi2O3: 1-2.5%.
[0013] Optionally, the melting time of the plain glass is 6 hours.
[0014] The second aspect of the present application provides a glass-ceramic, which is obtained by heat-treating the plain glass described in the first aspect of the present application, and the glass-ceramic contains a lithium disilicate crystal phase.
[0015] The third aspect of the present application provides a chemically strengthened microcrystalline glass, which is obtained by sequentially subjecting the plain glass described in the first aspect of the present application to heat treatment and chemical strengthening treatment.
[0016] The fourth aspect of the present application provides a glass preparation method, comprising: preparing raw materials with corresponding formula proportions according to the components of plain glass; wherein the components of the plain glass, in terms of weight percentage, include: SiO2: 45-65%, Al2O3: 1-12%, Li2O: 14-18%, B2O3: 2-6%, R2O: 5-6%, and the R2O includes Na2O and K2O; after the raw materials are evenly mixed, they are smelted according to a preset melting temperature and melting time to obtain the plain glass.
[0017] As can be seen from the above, according to the plain glass, microcrystalline glass, chemically strengthened microcrystalline glass and glass preparation method provided by the present application, the components of the glass products include, by weight percentage: SiO2: 45-65%, Al2O3: 1-12%, Li2O: 14-18%, B2O3: 2-6%, R2O: 5-6%; wherein R2O includes Na2O and K2O. Through the implementation of the present application, Na2O and K2O are introduced as necessary components, and the K2O and Na2O in the glass components play a mixed alkali effect, which can effectively improve the chemical stability of the glass.
[0018] It should be understood that the content described in this section is not intended to identify the key or important features of the present application, nor is it intended to limit the scope of the present application. Other features of the present application will become easily understood through the following description. DETAILED DESCRIPTION
[0019] In order to make the purpose, features, and advantages of the invention of this application more obvious and easy to understand, the technical solutions in the embodiments of this application will be clearly and completely described below in combination with the embodiments of this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.
[0020] In the description of the embodiments of the present application, the term "plurality" means two or more than two, unless otherwise clearly and specifically defined; the term "comprising" indicates the presence of the described features, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or their collections; the term "and / or" describes the association relationship of the associated objects, indicating that three relationships may exist. For example, A and / or B may include the three situations of A existing alone, A and B existing at the same time, and B existing alone. The character " / " generally indicates that the associated objects before and after are in an "or" relationship; the term "approximately" means that the content, size, parameter, etc. are not and do not need to be precise. If necessary, they can be approximate or higher or lower. Generally speaking, regardless of whether there is an explicit description, the content, size, parameter, etc. should be "approximately" or "approximately"; the terms "preferably" and "optional" are not used to limit the scope of the present application, nor do they mean that certain technical features are critical or indispensable to the implementation methods of the present application, but should be understood as only indicating specific aspects of the embodiments of the present application.
[0021] Unless otherwise specified in specific circumstances, the numerical ranges recorded in the examples of the present application are intended to include the endpoints of the numerical range and all integers and fractions within the range. When describing a certain content, solubility or other parameter in the form of a preferred range or a preferred value, it should be understood that it is equivalent to revealing any range by combining any preferred range with a preferred range, a preferred value with a preferred value, or a preferred range with a preferred value, without considering whether this combination is specifically explained in the examples.
[0022] Unless otherwise specified in specific circumstances, the component contents described in the examples of the present application are expressed in weight percentage.
[0023] In the related art, microcrystalline glass needs to undergo chemical strengthening treatment to improve its strength. However, the current microcrystalline glass has a problem that the structure of the glass changes after crystallization, and the chemical stability of the glass phase is poor, and it cannot pass environmental reliability tests such as the double 85 test.
[0024] In order to at least solve one of the problems in the related art to a certain extent, an embodiment of the present application provides a plain glass, which may also be called substrate glass or matrix glass, which refers to glass that has not been nucleated, crystallized or strengthened, and its components, by weight percentage, include: SiO2: 45-65%, Al2O3: 1-12%, Li2O: 14-18%, B2O3: 2-6%, R2O: 5-6%; wherein R2O includes Na2O and K2O.
[0025] SiO2 is the basic component of the glass composition provided in the present application, and is a network structure former of glass and glass-ceramics, and forms lithium disilicate after crystallization. It should be noted that if the content of SiO2 is below 45%, the crystals formed in the glass-ceramics will become less and the crystals will become coarser, which will affect the haze, drop ball test height and other properties of the glass-ceramics and glass-ceramics products. Therefore, the lower limit of the SiO2 content is preferably 45%; in addition, if the SiO2 content is above 55%, the glass melting temperature is high, the material is difficult to form, and it is not easy to form, which affects the consistency of the glass. Therefore, the upper limit of the SiO2 content is preferably 55%. In some embodiments, the glass composition may contain about 65%, 60%, 55%, 54%, 53%, 52%, 51%, 50%, 49%, 48%, 47%, 46%, 45% SiO2. Preferably, the content of SiO2 is 48-53%.
[0026] Al2O3 can be a component that forms a glass network structure, or it can be a cationic network exosome that balances charge. In the present application, all Al2O3 enters the glass network structure, improves the chemical stability of the glass, improves the mechanical properties of the glass, and increases the depth of the ion exchange layer and surface stress of the microcrystalline glass product. On the one hand, if its content is less than 1%, the effect is not good, so the lower limit of the mass percentage content of Al2O3 is 1%; on the other hand, if the content of Al2O3 exceeds 12%, the melting and devitrification resistance of the glass are reduced, and the crystals are easy to increase during crystallization, reducing the strength of the microcrystalline glass and microcrystalline glass products, so the upper limit of the Al2O3 content is 12%. In some embodiments, the glass composition may contain about 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12% Al2O3. Preferably, the content of Al2O3 is 5-10%.
[0027] Li2O is an essential component that becomes a crystalline phase after crystallization, helps to form lithium-containing crystalline phases such as lithium disilicate, and is also an essential component for chemical strengthening. However, if its content is less than 5%, the effect is not good. Therefore, this application sets the lower limit of the Li2O content to 14%. On the other hand, if too much Li2O is contained, it is easy to reduce the chemical stability of the glass and increase the product cost. Therefore, the upper limit of the Li2O content is preferably 18%. In some embodiments, the glass composition may contain about 14%, 15%, 16%, 17%, 18% Li2O. Preferably, the content of Li2O is 14-16%.
[0028] B2O3 can reduce the melting temperature of glass. When its content is high, the chemical stability of glass is reduced. Therefore, the upper limit of the weight percentage of B2O3 is 6% and the lower limit is 2%. In some embodiments, the glass composition may contain about 2%, 3%, 4%, 5%, 6% B2O3. Preferably, the content of B2O3 is 3-5%.
[0029] It is worth mentioning that K2O and Na2O help improve the low-temperature melting and formability of glass, and when the glass is chemically strengthened, the mixed alkali effect can be exerted to effectively improve the chemical stability of the glass. However, excessive K2O and Na2O can easily reduce the chemical stability of the glass. Therefore, the sum of the weight percentages of K2O and Na2O is 5-6%, for example, 5%, 5.5%, 6%. Preferably, the weight percentage ratio of Na2O to K2O is greater than or equal to 1.
[0030] In an optional implementation manner of the present embodiment, the components of the plain glass, measured in weight percentage, further include: P2O5: 0.1-3.5%, and / or, ZrO2: 0.1-3%, and / or, CaO: 0-2%, and / or, ZnO: 0-9%, and / or, MgO: 0.1-7%, and / or, SrO: 0-0.3%, and / or, BaO: 0-2%, and / or, TiO2: 0-1.5%, and / or, clarifier: 0.2-2.5%.
[0031] P2O5 helps to improve the low-temperature melting property of glass, can separate phases in glass to form crystal nuclei, and improve the thermal expansion stability of glass during the crystallization process. The lower limit of the weight percentage of P2O5 is preferably 0.1%; however, if too much P2O5 is contained, it is easy to reduce the resistance to devitrification and phase separation of glass, and the mechanical properties of glass tend to deteriorate. Therefore, the upper limit of the P2O5 content is 3.5%; in some embodiments, the glass composition may contain about 0.1%, 0.5%, 1%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5% P2O5. Preferably, the content of P2O5 is 1.5-3%.
[0032] ZrO2 is a crystal nucleating agent and helps to improve the chemical stability of the glass. The lower limit of the ZrO2 content in this application is 0.1, but if too much ZrO2 is contained, the devitrification resistance of the glass is easily reduced, and the difficulty of controlling the glass crystallization process increases. Therefore, the upper limit of the ZrO2 content is 3%. In some embodiments, the glass composition may contain about 0.1%, 0.5%, 1%, 1.5%, 2.0%, 2.5%, 3.0% ZrO2. Preferably, the content of ZrO2 is 1.5-2.6%.
[0033] ZnO can improve the melting properties of glass, improve the chemical stability of glass, and refine grains during crystallization. Controlling the upper limit of the ZnO mass percentage content to below 9% can inhibit the reduction of devitrification. Therefore, the upper limit of the ZnO content is 9%. In some embodiments, the glass composition may include approximately 0, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% ZnO, preferably 4%, and more preferably 2.2%.
[0034] MgO helps to reduce the viscosity of glass, inhibit the tendency of crystallization during glass forming, and improve low-temperature melting. MgO is an optional component, but if the MgO content is too high, it may cause a decrease in devitrification resistance, and undesirable crystals will be obtained after crystallization, resulting in a decrease in the performance of microcrystalline glass and microcrystalline glass products. Therefore, the upper limit of the MgO mass percentage content is 7%. In some embodiments, the glass composition may contain about 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7% MgO. Preferably, the content of MgO is 0.3-3%.
[0035] SrO can improve the low temperature melting property of glass and inhibit the tendency of forming and crystallization. It is added as an unnecessary component and its mass percentage content is less than 0.3%. In some embodiments, the glass composition may include about 0, 0.1%, 0.2%, 0.3% SrO.
[0036] BaO can improve the glass-forming properties of glass. In order to avoid the reduction of the devitrification resistance of glass, the mass percentage of BaO is preferably controlled below 2%, such as 0, 0.5%, 1%, 1.5%, 2%. Preferably, the glass composition may contain 0-0.7% BaO, and more preferably, no BaO is introduced.
[0037] TiO2 helps to lower the melting temperature of glass and improve chemical stability. By introducing TiO2 below 1.5% by mass, the crystallization process of glass can be easily controlled. In some embodiments, the glass composition may include about 0, 0.5%, 1%, 1.5% TiO2. Preferably, the content of TiO2 is 0-1%, and more preferably, no TiO2 is introduced.
[0038] The clarifier includes one or more components of Sb2O3 and SnO2, and the upper limit of the mass percentage of the clarifier is 2.5% and the lower limit is 0.2%. In some embodiments, the glass composition may include about 0.2%, 0.5%, 1%, 1.5%, 2.0%, 2.5% of the clarifier. Preferably, the content of the clarifier is 0.2-2.2%, more preferably 0.2-2%.
[0039] In an optional implementation manner of the present embodiment, the components of the plain glass, measured in weight percentage, satisfy any one of the following conditions: (1) ZrO2+P2O5+TiO2: 4.5-6.5%, exemplary values may be 4.5%, 5%, 5.5%, 6%, 6.5%; (2) ZnO+MgO+CaO+BaO+SrO: 2.7-16.3%, exemplary values may be 2.7%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 16.3%; (3) Y2O3+Nb2O3+La2O3: 0-1.3%, exemplary values may be 0, 0.5%, 1%, 1.3%.
[0040] In another optional implementation manner of the present embodiment, the components of the plain glass, measured in weight percentage, satisfy any one of the following conditions: (Li2O+Na2O+K2O) / B2O3: 5-11, exemplary values may be 5, 6, 7, 8, 9, 10, 11; (Li2O+Na2O+K2O) / Al2O3: 1.75-5.5, exemplary values may be 1.75, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5; (Li2O+Na2O+K2O) / (SiO2+B2O3+Al2O3): 0.31-0.39, exemplary values may be 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39.
[0041] It is worth mentioning that the content relationship of (Li2O+Na2O+K2O) / B2O3 indicates the content ratio between alkali metal oxides and B2O3 glass formers; in the present application, the numerical range is 5 to 11, that is, greater than 1.35, indicating that B is a BO4 structure in the glass network structure, which replaces part of SiO2 while improving the connectivity of the glass network structure, thereby reducing the difficulty of melting the glass.
[0042] The content relationship of (Li2O+Na2O+K2O) / Al2O3 indicates the content ratio between alkali metal oxides and Al2O3 glass formers; in the present application, the numerical range is 1.75 to 5.5, that is, greater than 0.93, indicating that all Al enters the glass network structure and exists in the form of AlO4, which can improve the connectivity and mechanical properties of the glass network structure.
[0043] The content relationship of (Li2O+Na2O+K2O) / (SiO2+B2O3+Al2O3) indicates the content ratio between alkali metal oxides and glass formers; in practical applications, if the value exceeds 0.5, it will affect the chemical stability of the glass, so the numerical range in this application is 0.31~0.39.
[0044] ZrO2+P2O5+TiO2 is the mass content range of all crystal nucleating agents. In practical applications, if this value exceeds 7%, the crystal growth process during heat treatment will be uncontrollable. Therefore, in this application, the value range is 4.5-6.5%.
[0045] ZnO+MgO+CaO+BaO+SrO is the mass content range of all alkaline earth metals. In practical applications, if this value exceeds 17%, the mechanical properties and ion exchange capacity of the glass will be reduced. Therefore, in this application, the value range is 2.7-16.3%.
[0046] Y2O3+Nb2O3+La2O3 is the mass content range of all trivalent rare metals, and this value is generally below 2%. In this application, this value range is 0-1.3%, which can effectively adjust the mechanical properties and refractive index of the glass.
[0047] SnO2+Sb2O3 is the mass content range of all clarifiers, and this value is generally below 3%. In this application, this value range is 0.2-2.5%, which can effectively improve the optical quality of the glass and reduce the generation of defects such as bubbles inside the glass due to insufficient clarification of the glass liquid.
[0048] In an optional implementation manner of this embodiment, the components of the plain glass, measured in weight percentage, further include: Bi2O3: 0.1-3%.
[0049] In the related art, glass raw materials are melted to obtain plain glass, and the glass melting time in the related art is usually more than 10 hours, which makes the glass melting difficult. Based on this, this embodiment introduces Bi2O3 components into the glass composition. In order to avoid excessive Bi2O3 content causing glass coloring, the upper limit of the Bi2O3 content is set to 3%. In some embodiments, the glass composition may contain approximately 0.1%, 0.5%, 1%, 1.5%, 2.0%, 2.5%, and 3% Bi2O3. Preferably, the content of Bi2O3 is 1 to 2.5%. It is worth mentioning that after the introduction of Bi2O3, the temperature at which the glass viscosity reaches 100 poise during the glass melting process is significantly reduced, effectively reducing the difficulty of glass melting.
[0050] Next, an embodiment of the present application further provides a glass-ceramic, which is obtained by heat-treating the plain glass provided in any of the above embodiments, also known as glass ceramics, which is a solid material including both a glass phase and a crystalline phase. The glass-ceramic of this embodiment includes a lithium disilicate crystal phase (i.e., Li2Si2O5 crystal phase), and Li2O and SiO2 are important components for forming the lithium disilicate crystal phase. It is worth mentioning that the heat treatment here can be understood as a nucleation treatment and a crystallization treatment.
[0051] In an optional implementation manner of this embodiment, the crystallinity of the above-mentioned microcrystalline glass is 60-90%, and exemplary values may be 60%, 65%, 70%, 75%, 80%, 85%, and 90%, and the grain size is 20-40nm, and exemplary values may be 20, 25, 30, 35, and 40nm.
[0052] Next, an embodiment of the present application further provides a chemically strengthened glass-ceramic, which is obtained by sequentially subjecting the plain glass provided by any of the aforementioned embodiments to a heat treatment and a chemical strengthening treatment (also referred to as an ion exchange treatment). It is worth mentioning that the chemically strengthened glass-ceramic includes a compressive stress layer extending from the surface of the glass-ceramic to the depth of the ion exchange layer.
[0053] In an optional implementation manner of the present embodiment, the surface compressive stress of the chemically strengthened microcrystalline glass is 225-315 MPa, and exemplary values may be 220, 225, 230, 235, 240, 245, 250, 255, 260, 265, 270, 275, 280, 285, 290, 295, 300, 305, 310, 315 MPa, and the depth of the ion exchange layer is 70-125 μm, and exemplary values may be 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125 μm.
[0054] In an optional implementation of this embodiment, the Vickers hardness of the chemically strengthened microcrystalline glass is 730-830 kgf / mm 2 , Young's modulus is 75~165GPa, fracture toughness is 0.4~2.5Mpa·m 1 / 2 , four-point bending strength is 690~820MPa, drop ball test height is 1030~2200mm, drop resistance performance index is 1250~2350mm, haze at 0.5mm thickness is 0.12~0.13%, |B| value is 0.3, average transmittance of visible light with a wavelength of 370 to 760nm is more than 90%, and transmittance of visible light with a wavelength of 550nm is more than 90%.
[0055] Accordingly, an embodiment of the present application further provides a glass preparation method, which specifically includes the following process:
[0056] Step A, preparing raw materials in corresponding formula proportions according to the components of plain glass;
[0057] Step B: after the raw materials are uniformly mixed, they are melted according to a preset melting temperature and melting time to obtain plain glass.
[0058] On the one hand, the components of the plain glass include, by weight percentage, SiO2: 45-65%, Al2O3: 1-12%, Li2O: 14-18%, B2O3: 2-6%, R2O: 5-6%, R2O includes Na2O and K2O. On the other hand, the melting temperature of the glass is 1580°C, and the melting time is 6 hours.
[0059] Furthermore, the glass preparation method of this embodiment further includes: step C, performing nucleation treatment and crystallization treatment on the plain glass to obtain microcrystalline glass.
[0060] It should be noted that nucleation treatment refers to growing crystal nuclei in glass through heat treatment, and crystallization treatment refers to growing specific crystals based on the crystal nuclei through heat treatment.
[0061] In an optional implementation manner of this embodiment, the nucleation treatment temperature is 620° C., and the nucleation treatment time is 240 min; the crystallization treatment temperature is 760° C., and the crystallization treatment time is 30 min.
[0062] Furthermore, the glass preparation method of this embodiment also includes: step D, chemically strengthening the microcrystalline glass to obtain chemically strengthened microcrystalline glass.
[0063] It is worth mentioning that chemical strengthening treatment refers to placing the microcrystalline glass in a salt bath for ion exchange treatment, so that the microcrystalline glass forms a compressive stress layer and a tensile stress layer. The chemical strengthening salt bath includes a sodium ion salt bath or a potassium ion salt bath. The components of the sodium ion salt bath include one or more of sodium nitrate, sodium carbonate, and sodium sulfate. The components of the potassium ion salt bath include one or more of potassium nitrate, potassium carbonate, and potassium sulfate. The number of ion exchange treatments is at least one. When the number of ion exchange treatments is multiple, the salt baths used for multiple ion exchange treatments may be different.
[0064] In an optional implementation manner of this embodiment, the chemical strengthening treatment temperature is 460° C., and the chemical strengthening treatment time is 4 hours.
[0065] In order to illustrate the technical effects of the glass products of the above-mentioned embodiments of the present application, the present application has conducted tests on glass products with different components and contents to determine the characteristics of each glass product, and the test results of glass formulas containing K2O and Bi2O3 are shown in the embodiments of Tables 1 to 4, the test results of glass formulas without K2O are shown in the comparative examples of Tables 5 to 8, and the test results of glass formulas without Bi2O3 are shown in the comparative examples of Tables 9 to 12.
[0066] Table 1
[0067]
[0068]
[0069]
[0070] Table 2
[0071]
[0072]
[0073]
[0074]
[0075] Table 3
[0076]
[0077]
[0078]
[0079] Table 4
[0080]
[0081]
[0082]
[0083] Table 5
[0084]
[0085]
[0086]
[0087] Table 6
[0088]
[0089]
[0090]
[0091] Table 7
[0092]
[0093]
[0094]
[0095]
[0096] Table 8
[0097]
[0098]
[0099]
[0100] Table 9
[0101]
[0102]
[0103]
[0104] Table 10
[0105]
[0106]
[0107]
[0108]
[0109] Table 11
[0110]
[0111]
[0112]
[0113] Table 12
[0114]
[0115]
[0116]
[0117] It can be seen from the examples in Tables 1 to 4 and the comparative examples in Tables 5 to 8 that, compared with the glass formula not containing K2O components, the glass formula containing K2O components has a deeper ion exchange layer and a longer effective time in the double 85 test under the same chemical strengthening molten salt ratio (NaNO3:KNO3=1:1) and chemical strengthening temperature / time, and has more excellent mechanical properties and chemical stability.
[0118] In addition, by comparing the embodiments in Tables 1 to 4, the comparative examples in Tables 5 to 8 and the comparative examples in Tables 9 to 12, it can be seen that when melting glass with 2 kg of raw materials, the glass formula containing Bi2O3 components has a lower temperature when the glass viscosity reaches 100 poise than the glass formula without Bi2O3 components, which effectively reduces the difficulty of glass melting.
[0119] Based on the technical solutions of the above-mentioned embodiments of the present application, on the one hand, the present application uses K2O and Na2O as necessary components, and exerts a mixed alkali effect through K2O and Na2O in the glass components, thereby effectively improving the chemical stability of the glass; on the other hand, after introducing Bi2O3, the present application can reduce the temperature at which the glass viscosity reaches 100 poise, thereby reducing the difficulty of glass melting.
[0120] It is also worth mentioning that due to the above-mentioned performance advantages of the plain glass, microcrystalline glass, and chemically strengthened microcrystalline glass provided in the embodiments of the present application, they can be widely used in the manufacture of glass protective cover plates for electronic devices, glass components, or windows for household appliances.
[0121] Finally, it should be noted that in the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0122] The above is a description of the plain glass, microcrystalline glass, chemically strengthened microcrystalline glass and glass preparation method provided in the present application. For those skilled in the art, based on the ideas of the embodiments of the present application, equivalent substitutions made in the specific implementation methods and application scopes should all be included in the scope of the claims of the present application. In summary, the content of this specification should not be understood as a limitation on the scheme of the present application.
Claims
1. A plain glass, characterized in that: Its components, by weight percentage, include: SiO2: 45-65%, Al2O3: 1-12%, Li2O: 14-18%, B2O3: 2-6%, R2O: 5-6%; Wherein, the R2O includes Na2O and K2O.
2. The plain glass according to claim 1, characterized in that: Its components, measured in weight percentage, also include: P2O5: 0.1-3.5%, and / or, ZrO2: 0.1-3%, and / or, CaO: 0-2%, and / or, ZnO: 0-9%, and / or, MgO: 0.1-7%, and / or, SrO: 0-0.3%, and / or, BaO: 0-2%, and / or, TiO2: 0-1.5%, and / or, clarifier: 0.2-2.5%.
3. The plain glass according to claim 1, characterized in that: The components thereof are calculated by weight percentage and include: SiO2: 50-53%, Al2O3: 5-10%, Li2O: 14-16%, and B2O3: 3-5%.
4. The plain glass according to claim 2, characterized in that: Its components, measured by weight percentage, meet any of the following conditions: ZrO2+P2O5+TiO2: 4.5~6.5%; ZnO+MgO+CaO+BaO+SrO: 2.7~16.3%; Y2O3+Nb2O3+La2O3: 0~1.3%.
5. The plain glass according to claim 1, characterized in that: Its components, measured by weight percentage, meet any of the following conditions: (Li2O+Na2O+K2O) / B2O3: 5~11; (Li2O+Na2O+K2O) / Al2O3: 1.75~5.5; (Li2O+Na2O+K2O) / (SiO2+B2O3+Al2O3): 0.31~0.
39.
6. The plain glass according to any one of claims 1 to 5, characterized in that: The components thereof, in terms of weight percentage, also include: Bi2O3: 0.1-3%.
7. The plain glass according to claim 6, characterized in that: The components thereof, in terms of weight percentage, also include: Bi2O3: 1-2.5%.
8. The plain glass according to claim 6, characterized in that: The melting time of the plain glass is 6 hours.
9. A glass-ceramic, characterized in that: The microcrystalline glass is obtained by heat-treating the plain glass according to any one of claims 1 to 8, and the microcrystalline glass contains a lithium disilicate crystal phase.
10. The glass-ceramic according to claim 9, characterized in that: The crystallinity is 60-90%, and the grain size is 30-36 nm.
11. A chemically strengthened glass-ceramic, characterized in that: The chemically strengthened glass-ceramics is obtained by sequentially subjecting the plain glass according to any one of claims 1 to 8 to a heat treatment and a chemical strengthening treatment.
12. The chemically strengthened glass-ceramics according to claim 11, characterized in that: The surface compressive stress of the chemically strengthened glass is 225-315 MPa, and the depth of the ion exchange layer is 70-125 μm.
13. A method for preparing glass, characterized in that: include: Prepare raw materials with corresponding formula proportions according to the components of plain glass; wherein the components of the plain glass include, by weight percentage, SiO2: 45-65%, Al2O3: 1-12%, Li2O: 14-18%, B2O3: 2-6%, R2O: 5-6%, and the R2O includes Na2O and K2O; After the raw materials are uniformly mixed, they are melted according to a preset melting temperature and melting time to obtain the plain glass.
14. The glass preparation method according to claim 13, characterized in that: Also includes: The plain glass is subjected to nucleation treatment and crystallization treatment to obtain microcrystalline glass.
15. The glass preparation method according to claim 14, characterized in that: Also includes: The microcrystalline glass is subjected to chemical strengthening treatment to obtain chemically strengthened microcrystalline glass.
16. The glass preparation method according to any one of claims 13 to 15, characterized in that: The melting temperature is 1580° C. and the melting time is 6 hours.
17. The method for preparing glass according to claim 14 or 15, characterized in that: The nucleation treatment temperature is 620° C., and the nucleation treatment time is 240 min; and / or, the crystallization treatment temperature is 760° C., and the crystallization treatment time is 30 min.
18. The method for preparing glass-ceramics according to claim 15, characterized in that: The chemical strengthening treatment temperature is 460°C and the chemical strengthening treatment time is 4 hours.
Citation Information
Patent Citations
Glass ceramic and glass ceramic product
CN112939469A
Glass ceramics, glass ceramic product and manufacturing method thereof
CN113754291A
High-strength transparent microcrystalline glass and preparation method thereof
CN114671616A
Glass ceramic, glass ceramic product and manufacturing method thereof
CN114907016A
Colored glass articles with improved mechanical durability
CN117069373A