Blue-adjustment high-strength electronic glass and preparation method thereof

By optimizing the formula and preparation process of blue glass, combined with potassium nitrate chemical strengthening and acid solution treatment, the problems of complex preparation process, high cost and insufficient strength of existing blue glass are solved, and the coloring stability and strength improvement of the glass are achieved.

CN118754433AInactive Publication Date: 2024-10-11XIANNING NANBO PHOTOELECTRIC GLASS CO LTD +1

Patent Information

Application Number
CN202410887394.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The preparation process of existing blue glass is complex and costly, the degree of crystallization affects the color expression, and the strength is insufficient. The color of traditional high-alumina glass is not bright enough, and the strength cannot be greatly improved through chemical strengthening.

Method used

It adopts a formula of SiO2 57%~65%, Al2O3 12%~17%, B2O3 0~2%, P2O5 0~1% and other ingredients, through high-temperature melting molding and annealing treatment, combined with chemical strengthening of potassium nitrate and mixed acid solution soaking Processing, avoid high content of aluminum oxide and lithium oxide, use Co and Cu as coloring elements that are not easy to change color.

Benefits of technology

It achieves stable coloring of glass, controllable costs, and significant improvement in strength, and avoids the problem of crystallization affecting color expression. It does not require a platinum channel, and float molding is simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004926415120000051
    Figure BDA0004926415120000051
  • Figure BDA0004926415120000061
    Figure BDA0004926415120000061
Patent Text Reader

Abstract

The invention belongs to the technical field of electronic glass, and particularly discloses blue-tone high-strength electronic glass and a preparation method thereof.The glass comprises, by mass, 57%-65% of SiO2, 12%-17% of Al2O3, 0-2% of B2O3, 50%-1% of P2O, 0-1% of Li2O, 11%-17% of Na2O, 3%-8% of K2O, 3%-8% of MgO, 0.5%-2% of ZrO2, 0-2% of La2O3, 0-2% of Y2O3, 0.2%-1% of Er2O3, 0.2%-1% of Nd2O3, 0.001%-0.004% of Co2O3 and 0-0.1% of CuO, La2O3 + Y2O3 + Er2O3 + Nd2O3 is 1%-5%, and the ratio of (Er2O3 + Nd2O3) The preparation method comprises the following steps: mixing the glass raw materials according to the components in the formula, carrying out high-temperature melting and clarification homogenization, molding in a mold, carrying out annealing treatment, cooling to room temperature, and finally carrying out strengthening treatment to obtain the blue-tone high-strength electronic glass. According to the glass, the impact resistance is larger than or equal to 1.28 J, the blank pressing strength is larger than or equal to 40 Kg under the pressure head of 0.5 mm and the edge distance of 0.8 mm, the transmittance is larger than or equal to 91.5% under the reference thickness of 0.35 mm, the color value L * ranges from 96 to 97, the color value a * ranges from-0.1 to 0, and the color value b * ranges from-0.28 to-0.1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic glass and relates to blue-toned high-strength electronic glass and a preparation method thereof. Background Art

[0002] With the popularity and diversification of electronic products, the requirements for glass materials are getting higher and higher. Blue glass has a wide range of applications in electronic devices due to its unique color and optical properties, such as electronic product display screens. Traditional blue glass is mostly soda-lime glass, which has low strength.

[0003] The existing blue glass has the following disadvantages: 1) The existing blue high-strength glass, such as lithium disilicate microcrystalline glass, has a complex preparation process, requires the use of electronic glass rolling molding process, and requires a platinum channel, which has a high manufacturing cost. At the same time, its degree of crystallization will also affect the color, which is difficult to control. 2) Traditional high-aluminum glass is colorless and transparent glass, and the color is not bright enough when used in electronic display screens. And it is only chemically strengthened, and the strength will not be greatly improved. 3) In order to improve the strength of the glass, ≥20wt% alumina is added to increase the glass network space, in order to increase the ion exchange amount during the chemical strengthening process, thereby increasing the surface stress and depth, thereby improving the strength of the glass. 4) Add ≥3wt% lithium oxide, in order to achieve the exchange of Li+ and Na+ during the chemical strengthening process, so as to achieve a high stress depth, thereby improving the strength of the glass. 5) Traditionally, the color of the glass needs to be adjusted to control the atmosphere during glass melting and the COD value of the glass raw materials, because many colorant ions have variable valence, and different valence states will make the glass color unstable. Summary of the invention

[0004] The present invention provides a blue-toned high-strength electronic glass and a preparation method thereof. The formula design is reasonable, and coloring elements that are not easily changed with the atmosphere and the COD value of glass raw materials are used, so that the glass coloring is stable, and there is no need to add high-content aluminum oxide and lithium oxide. The chemical strength of the glass can be greatly improved through the strengthening method improved by the present invention.

[0005] In order to achieve the above object, the present invention adopts the following technical solution: a blue high-strength electronic glass, which comprises the following components by mass fraction:

[0006] SiO2 57%~65%, Al2O3 12%~17%, B2O3 0~2%, P2O5 0~1%, Li2O 0~1%, Na2O 11%~17%, K2O 3%~8%, MgO 3%~8%, ZrO2 0.5%~2%, La2O3 0~2%, Y2O3 0~2%, Er2O3 0.2%~1%, Nd2O3 0.2%~1%, Co2O3 0.001%~0.004%, CuO 0~0.1%.

[0007] Furthermore, the glass also satisfies at least one of the following conditions: B2O3 0.2-2%; P2O5 0.2-1%; Li2O 0.05-1%; La2O3 0.1-2%; Y2O3 0.1-2%; CuO 0.001-0.1%.

[0008] Furthermore, the components in the glass also meet the following conditions: La2O3+Y2O3+Er2O3+Nd2O3 is 1% to 5%.

[0009] Furthermore, the components in the glass also satisfy the following condition: (Er2O3+Nd2O3) / (Co2O3+CuO)=5~1500.

[0010] In a further preferred embodiment, the following components are included by mass fraction: SiO2 58-63%, Al2O3 13-16%, B2O30-1%, P2O5 0-0.5%, Li2O 0.-0.5%, Na2O 12-15%, K2O 4-7%, MgO 4-7%, ZrO2 0.5-1.5%, La2O3 0-1.5%, Y2O3 0-1.5%, Er2O3 0.5-1%, Nd2O3 0.5-1%, Co2O3 0.0015-0.0035%, and CuO0-0.05%.

[0011] The present invention also relates to a method for preparing the glass. Specifically, during the preparation, glass raw materials are mixed according to the ingredients in the formula, melted at high temperature and clarified and homogenized, then formed in a mold, annealed and cooled to room temperature, and finally strengthened to obtain blue high-strength electronic glass.

[0012] Furthermore, the strengthening treatment is firstly chemical strengthening in a molten salt of potassium nitrate, and then immersing in a mixed acid solution.

[0013] Furthermore, during chemical strengthening, the steel is treated in a molten salt of potassium nitrate at 360 to 440° C. for 1.5 to 4 hours.

[0014] Furthermore, in the mixed acid solution, the mass content of hydrofluoric acid is 2% to 7%, the mass content of sulfuric acid is 3% to 8%, the mass content of nitric acid is 0.2 to 2%, and the mass content of hydrochloric acid is 0 to 1%.

[0015] Furthermore, the glass is immersed in the mixed acid solution for 0.5 to 5 minutes.

[0016] The present invention has the following beneficial effects:

[0017] The glass in the present invention is non-microcrystalline glass, and there is no problem that the degree of crystallization affects the color expression. In addition, the coloring elements Co and Cu are used, which are not easily changed with the atmosphere and the COD value of the glass raw materials, so the coloring of the glass is stable.

[0018] The glass preparation process of the present invention is simple, the cost is controllable, no platinum channel is required, and float molding can be performed. It is not necessary to add a high content of aluminum oxide and lithium oxide in the formula. By adding a certain amount of rare earth elements and acid treatment after chemical strengthening, the strength can be significantly improved. DETAILED DESCRIPTION

[0019] The present invention is described in detail below in conjunction with the examples. The following examples are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following examples.

[0020] The blue-toned high-strength electronic glass provided by the present invention comprises the following components by mass fraction:

[0021] SiO2 57%~65%, Al2O3 12%~17%, B2O3 0~2%, P2O5 0~1%, Li2O 0~1%, Na2O 11%~17%, K2O 3%~8%, MgO 3%~8%, ZrO2 0.5%~2%, La2O3 0~2%, Y2O3 0~2%, Er2O3 0.2%~1%, Nd2O3 0.2%~1%, Co2O3 0.001%~0.004%, CuO 0~0.1%.

[0022] SiO2 is an important glass former and a component of the glass skeleton, and is necessary. It can improve the mechanical strength, chemical stability, thermal stability, etc. of the glass. If the SiO2 content is less than 57%, the mechanical strength, chemical stability, and thermal stability of the glass will decrease. However, SiO2 has a very high melting point and tends to increase viscosity. Too much SiO2 will make the glass material difficult to use for float molding. If its content exceeds 65%, the melting temperature of the glass will rise, the viscosity will increase, and it will be more difficult to melt and clarify. Therefore, the optimal range of SiO2 content in the present invention is 57% to 65%; more preferably 58 to 63%.

[0023] Al2O3 is a glass network intermediate. When it participates in the formation of the glass network, it can reduce the crystallization tendency of the glass, improve the chemical stability, thermal stability, mechanical strength and hardness of the glass, and provide a larger glass network space for rapid and deep ion exchange, so it is necessary. However, its melting temperature is high, which will significantly increase the viscosity of the glass. When its content is high, it is more difficult to melt and clarify. Therefore, its content needs to be controlled at 12% to 17%; more preferably 13 to 16%.

[0024] B2O3 is a network former. When there are alkali metals and alkaline earth metals in the glass in appropriate proportions, a network will be formed. The volume of [BO4] tetrahedron is smaller than that of [SiO4] tetrahedron, so the network will be more compact, and the strength of the original glass will be improved. At the same time, [BO4] tetrahedron will increase the stress of the glass after strengthening, so the stress after strengthening will be improved to a certain extent. However, when its content is too high, the [BO4] tetrahedron in the glass will easily transform into [BO3] triangle, which will reduce the strength of the original glass. Therefore, its content needs to be controlled at 0-2%; more preferably 0-1%.

[0025] P2O5 is a network former. It participates in the glass network with [PO4] tetrahedron, which can increase the glass network space and the stress depth of the chemically strengthened glass, thereby improving the glass strength. However, when its content is too high, it will greatly reduce the chemical stability of the glass and easily cause glass phase separation during the manufacturing process. Its content needs to be controlled at 0-1%, and more preferably 0-0.5%.

[0026] MgO is an oxide outside the glass network, which helps the glass melt, reduces the tendency to crystallize, improves the chemical stability and mechanical strength of the glass, and can slow down the hardening of the glass and improve the glass forming properties. When its content is too high, it will cause great damage to the glass network structure, causing the Si-O bonds in the [SiO4] tetrahedron of the glass network to break, and the glass strength and chemical stability will decrease. Therefore, its content needs to be controlled at 3-8%, and more preferably 4-7%.

[0027] Li2O is a network-external oxide that can promote the melting of glass raw materials and reduce the melting temperature of glass, but it is not essential. It has a small radius and a strong ion field, which has a gathering effect on the glass network. However, a large amount of Li2O can easily cause serious "network breakage" in the glass structure, thereby reducing the strength of the glass. Therefore, its content is 0% to 1%; more preferably 0 to 0.5%.

[0028] Na2O is also a network exo-oxide, which can promote the melting of glass raw materials, reduce glass viscosity, and is also an essential component in the glass chemical strengthening ion exchange process. However, if its content is too high, the thermal expansion coefficient of the glass will increase, and the thermal stability, chemical stability and mechanical strength of the glass will be reduced. Therefore, its content is 11% to 17%; more preferably 12 to 15%.

[0029] K2O is also a network exogenous oxide, which can promote the melting of glass raw materials, reduce glass viscosity, and improve glass forming properties. However, when its content is too high, the glass network structure is destroyed, and its chemical stability and strength will decrease. Therefore, its content is 3% to 8%, and more preferably 4 to 7%.

[0030] ZrO2 is a glass network intermediate, and when its content is appropriate, it can also form a tetrahedral structure to form a glass network. At the same time, due to its strong field strength, it has a good gathering effect on the broken glass network, improving the strength and scratch resistance of the glass surface. However, too high a content of ZrO2 will make the glass difficult to melt, so its content needs to be controlled at 0.5% to 2%, and more preferably 0.5 to 1.5%.

[0031] La2O3 and Y2O3 are rare earth elements that can significantly increase the content of non-bridging oxygen in glass, significantly reduce the high-temperature viscosity of glass, and increase the Young's modulus, shear modulus and micro-Vickers hardness of glass. When their content is too high, the cost of glass manufacturing will increase a lot, and the stress of glass will also decrease after chemical strengthening. Therefore, La2O3 is controlled at 0-2%, and Y2O3 is controlled at 0-2%; more preferably 0-1.5%.

[0032] Er2O3 and Nd2O3 are also rare earth elements that can improve the strength of glass. When the content is too high, the cost of glass manufacturing will increase a lot, and the stress of glass will also decrease after chemical strengthening. At the same time, they can also make slight adjustments to the color of glass. Therefore, both Er2O3 and Nd2O3 need to be controlled at 0.2% to 1%, and more preferably 0.5 to 1%.

[0033] La2O3, Y2O3, Er2O3, and Nd2O3 are all rare earth elements, which can significantly increase the content of non-bridging oxygen in glass, significantly reduce the high-temperature viscosity of glass, and increase the Young's modulus, shear modulus, and micro-Vickers hardness of glass. Moreover, when its content is low, the stress of the glass after chemical strengthening will also increase. However, when its content is too high, the cost of glass manufacturing will increase a lot, and the stress of the glass after chemical strengthening will also decrease. Therefore, the total content of La2O3+Y2O3+Er2O3+Nd2O3 needs to be controlled at 1% to 5%; more preferably 1.5 to 4%.

[0034] Er2O3, Nd2O3, Co2O3, and CuO are the glass color adjusters. In order to obtain blue glass with high transmittance, they need to satisfy (Er2O3+Nd2O3) / (Co2O3+CuO)=5~1500; more preferably 7~1200.

[0035] When preparing the above glass, the oxides are mixed according to their proportions, melted, clarified and homogenized in a high-temperature furnace, and then the glass liquid is formed in a mold, annealed in an annealing furnace, and cooled to room temperature. The glass size can be prepared as 140×70×0.35mm. The prepared glass is strengthened by chemically strengthening the glass in a molten salt of potassium nitrate at 360-440°C for 1.5-4h, and then soaking it in a solution containing 2%-7% hydrofluoric acid, 3%-8% sulfuric acid, 0.2-2% nitric acid, and 0-1% hydrochloric acid by mass fraction for 0.5-5min, and then measuring its impact resistance, edge strength, transmittance and color value.

[0036] The specific embodiments and glass components are shown in Table 1 below, and the preparation process parameters and performance test data are shown in Table 2.

[0037] Impact resistance test: Use a drop ball impact tester to test the ultimate impact strength of the glass. The specific method is to take a 64g ball and release it from a certain height above the center of the glass to observe the breakage of the glass. If the glass does not break, continue to rise 5cm and repeat the drop ball test until it breaks. Then calculate the impact energy of the glass. W = mgh, m is the mass of the metal ball, g is the acceleration of gravity, and 10m / s 2 , h is the rupture height.

[0038] Edge pressing strength test: Use a glass strength edge pressing tester to test the glass edge pressing strength, select a 0.5mm pressure head and a 0.8mm margin.

[0039] Transmittance and color value test: Place the sheet glass into a spectrophotometer, measure the visible light transmittance of 0.35mm glass in the range of 380nm to 780nm, and use a colorimeter to calculate the L*, a*, and b* chromaticity values ​​of CIE (International Commission on Illumination) using a D65 light source.

[0040] The above embodiments describe the preferred implementation of the present invention, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including combining various technical features in any other manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

[0041] Table 1

[0042]

[0043] Table 2

[0044]

Claims

1. A blue high-strength electronic glass, characterized in that: It contains the following ingredients by mass fraction: SiO2 57%~65%, Al2O3 12%~17%, B2O3 0~2%, P2O5 0~1%, Li2O 0~1%, Na2O11%~17%, K2O 3%~8%, MgO 3%~8%, ZrO2 0.5%~2%, La2O3 0~2%, Y2O3 0~2%, Er2O3 0.2%~1%, Nd2O3 0.2%~1%, Co2O3 0.001%~0.004%, CuO 0~0.1%.

2. The glass according to claim 1, characterized in that At least one of the following conditions is met: B2O3 0.2-2%; P2O5 0.2-1%; Li2O 0.05-1%; La2O3 0.1-2%; Y2O3 0.1-2%; CuO 0.001-0.1%.

3. The glass according to claim 1 or 2, characterized in that: The components in the glass also meet the following conditions: La2O3+Y2O3+Er2O3+Nd2O3 is 1% to 5%.

4. The glass according to claim 3, characterized in that The components in the glass also satisfy the following conditions: (Er2O3+Nd2O3) / (Co2O3+CuO)=5~1500.

5. The glass according to claim 1, characterized in that It contains the following components by mass fraction: SiO2 58-63%, Al2O3 13-16%, B2O3 0-1%, P2O5 0-0.5%, Li2O 0.-0.5%, Na2O 12-15%, K2O 4-7%, MgO 4-7%, ZrO2 0.5-1.5%, La2O3 0-1.5%, Y2O3 0-1.5%, Er2O3 0.5-1%, Nd2O3 0.5-1%, Co2O3 0.0015-0.0035%, and CuO 0-0.05%.

6. The method for preparing the glass according to any one of claims 1 to 5, characterized in that: The glass raw materials are mixed according to the ingredients in the formula, melted at high temperature, clarified and homogenized, then formed in a mold, annealed and cooled to room temperature, and finally strengthened to produce blue high-strength electronic glass.

7. The preparation method according to claim 6, characterized in that: The strengthening treatment is to first perform chemical strengthening in a molten salt of potassium nitrate and then perform immersion treatment in a mixed acid solution.

8. The preparation method according to claim 7, characterized in that: During chemical strengthening, the steel is treated in a molten salt of potassium nitrate at 360-440°C for 1.5-4 hours.

9. The preparation method according to claim 7, characterized in that: In the mixed acid solution, the mass content of hydrofluoric acid is 2% to 7%, the mass content of sulfuric acid is 3% to 8%, the mass content of nitric acid is 0.2% to 2%, and the mass content of hydrochloric acid is 0% to 1%.

10. The preparation method according to claim 7, characterized in that: The glass is immersed in the mixed acid solution for 0.5 to 5 minutes.

Citation Information

Patent Citations

  • Enhancement method for enhancing surface strength of glass

    CN105819700A

  • Glass and preparation method

    CN108975688A

  • Low-viscosity and high-aluminum glass, preparation method and applications thereof

    CN111018346A

  • Colored microcrystalline glass as well as preparation method and application thereof

    CN116199427A

  • Lithium aluminosilicate glass composition, lithium aluminosilicate reinforced glass and preparation method

    CN117800594A

Cited By

  • Colored chemically strengthened glass as well as preparation method and application thereof

    CN117865464A

  • A colored chemically strengthened glass and its preparation method and application

    CN117865464B

  • Ultrathin glass, reinforced impact-resistant ultrathin glass and preparation method and application thereof