Cement particle ball, gypsum plaster board and preparation method of gypsum plaster board

By combining airgel with cement powder to prepare cement particle balls, and adding gypsum gelling system, the problem of airgel floating affecting the bonding performance is solved, and the strength and thermal insulation performance of the paper-faced gypsum board are improved to meet the needs National standards.

CN118754474AInactive Publication Date: 2024-10-11BEIJING NEW BUILDING MATERIALS PLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410822193.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The airgel powder floats in the gypsum slurry, affecting the bonding performance and causing the strength of the paper-faced gypsum board to decrease, which is lower than the national standard.

Method used

The airgel is combined with cement powder to prepare cement particle balls, which are added to the gypsum gelling system, so that the board has a thermal insulation effect while improving the strength of the paper-faced gypsum board made from airgel.

Benefits of technology

By uniformly dispersing the airgel, the mechanical strength of the gypsum board is improved, meeting the mechanical property requirements of national standards, while maintaining good thermal insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910699420000071
    Figure BDA0004910699420000071
  • Figure BDA0004910699420000081
    Figure BDA0004910699420000081
Patent Text Reader

Abstract

The invention discloses a cement particle ball, a gypsum plaster board and a preparation method thereof. The cement particle ball is prepared from the following raw materials in parts by weight: 100 parts of cement clinker, 20 to 40 parts of emulsion and 0.05 to 0.5 part of aerogel. The raw materials of the gypsum plaster board comprise the cement particle balls. According to the preparation method disclosed by the invention, in the process of preparing the gypsum plaster board, the aerogel is wrapped in the cement powder to prepare the cement particle balls, and the cement particle balls are uniformly dispersed in the gypsum slurry, so that on one hand, the aerogel is ensured to be uniformly dispersed in a gelatinization system, and on the other hand, the mechanical strength of the gypsum board is improved by adding the cement particle balls.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to but is not limited to the field of building materials, and in particular to a method for improving the strength of aerogel-prepared gypsum board and gypsum board and cement particle balls. Background Art

[0002] As the preferred material for interior decoration, gypsum board has been widely used in public places such as shopping malls and hospitals and home decoration. Because the porosity of gypsum board is large and the pore structure is properly distributed, it has high air permeability. When the indoor humidity is high, it can absorb moisture, and when the air is dry, it can release some moisture, thus playing a certain role in regulating the indoor humidity. Foreign countries call this function of gypsum board the "breathing" function. It is precisely because of this unique "breathing" property of gypsum board that it can regulate the indoor humidity within a certain range, making living conditions more comfortable.

[0003] Aerogel is a Class A fireproof insulation material with excellent thermal insulation performance. Its thermal conductivity is in the range of 0.013W / (m·K) to 0.03W / (m·K), which is much lower than the inorganic insulation materials currently available on the market for building insulation and energy saving. It has good thermal insulation and fireproof properties, and is an ideal substitute for traditional insulation materials with good application prospects. Combining aerogel with gypsum board to develop paper-faced gypsum board with better thermal insulation performance can create a safer and more comfortable indoor decoration environment.

[0004] However, aerogel powder is very light and floats in the gypsum slurry, floating to the contact interface between the board core and the facing paper, seriously affecting the bonding performance, causing a serious decrease in the strength of the board, even below the national standard, limiting its use. Summary of the invention

[0005] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of this application.

[0006] The present application provides a cement particle ball, a paper-faced gypsum board and a preparation method thereof. The cement particle ball is prepared by combining aerogel with cement powder, granulating, and adding it to a gypsum gelling system, so that the board has a thermal insulation effect and improves the strength of the paper-faced gypsum board prepared by aerogel.

[0007] The first aspect of the present application provides a cement particle ball, wherein the raw materials for preparing the cement particle ball include the following components in parts by weight: 100 parts by weight of cement clinker, 20-40 parts by weight of emulsion, and 0.05-0.5 parts by weight of aerogel.

[0008] In an exemplary embodiment, the cement clinker may be selected from one or more of Portland cement, aluminate cement and sulphoaluminate cement.

[0009] In an exemplary embodiment, the cement clinker is ordinary Portland cement, for example, the type may be 42.5, 42.5R, 52.5, 52.5R.

[0010] In an exemplary embodiment, the emulsion can be selected from one or more of polyvinyl acetate-ethylene emulsion, water-based acrylic emulsion, styrene acrylic emulsion / pure acrylic emulsion, silicone acrylic emulsion and polyurethane emulsion, etc. Preferably, the emulsion is polyvinyl acetate-ethylene emulsion.

[0011] In an exemplary embodiment, the aerogel may have a particle size of 5 μm to 1 mm and a bulk density of 0.04 g / cm 3 Up to 0.12g / cm 3 .

[0012] In an exemplary embodiment, the raw materials for preparing the cement granule balls include the following components in parts by weight: 100 parts by weight of cement clinker, 22 parts by weight of emulsion, and 0.08 parts by weight of aerogel; or

[0013] 100 parts by weight of cement clinker, 38 parts by weight of emulsion, and 0.5 parts by weight of aerogel; or

[0014] 100 parts by weight of cement clinker, 30 parts by weight of emulsion, and 0.3 parts by weight of aerogel.

[0015] The second aspect of the present application provides a method for preparing the above-mentioned cement granule balls, comprising:

[0016] 1) Weigh each raw material component;

[0017] 2) Add aerogel to the emulsion while stirring continuously and mix well;

[0018] 3) adding cement clinker to the mixture obtained in step 2) and mixing evenly;

[0019] 4) The mixture obtained in step 3) is sieved and dried to prepare cement particle balls wrapped with aerogel powder.

[0020] In an exemplary embodiment, step 4) is: passing the mixture obtained in step 3) through an 80-mesh sieve, drying at 45° C., to prepare cement particle balls coated with aerogel powder.

[0021] The third aspect of the present application provides cement granule balls prepared by the above-mentioned preparation method of cement granule balls.

[0022] The fourth aspect of the present application provides a paper-faced gypsum board, the raw materials of which include the above-mentioned cement granular balls, gypsum clinker and water, and one or more of glass fiber, foaming agent, retarder, water reducer and starch.

[0023] In an exemplary embodiment, the raw materials of the gypsum board include the following components in parts by weight: 100 parts by weight of gypsum clinker, 60-75 parts by weight of water, 0.02-0.1 parts by weight of glass fiber, 0.1-2 parts by weight of foaming agent, 0.1-0.5 parts by weight of retarder, 0.05-0.3 parts by weight of water reducer, 0.2-2 parts by weight of starch, and 10-40 parts by weight of the cement granular balls.

[0024] In an exemplary embodiment, the gypsum clinker may be selected from one or more of desulfurized gypsum clinker, phosphogypsum clinker and natural gypsum clinker.

[0025] In an exemplary embodiment, the glass fiber may be selected from any one of medium-alkali glass fiber, alkali-free glass fiber and alkali-resistant glass fiber.

[0026] In an exemplary embodiment, the glass fiber has a fiber length of 9-15 mm and a single fiber diameter of 10-15 um.

[0027] In an exemplary embodiment, the foaming agent is selected from one or more of the inorganic foaming agents ammonium dodecyl sulfate, sodium bicarbonate, and ammonium bicarbonate.

[0028] In an exemplary embodiment, the retarder is selected from one or more of citric acid, sodium citrate, sodium hexametaphosphate, borax and protein retarders. Preferably, the retarder is a protein retarder.

[0029] In an exemplary embodiment, the protein retarder is selected from a gelatin protein retarder and a protein gypsum retarder obtained by calcium salting of degraded polyamide.

[0030] In an exemplary embodiment, the water reducer is a polycarboxylate water reducer, preferably a powdered polycarboxylate water reducer.

[0031] In an exemplary embodiment, the starch may be selected from one or more of modified potato starch, modified tapioca starch and modified corn starch.

[0032] In an exemplary embodiment, the raw materials for preparing the gypsum board include the following components in parts by weight: 100 parts by weight of gypsum clinker, 62 parts by weight of water, 0.03 parts by weight of glass fiber, 2 parts by weight of foaming agent, 0.45 parts by weight of retarder, 0.3 parts by weight of water reducing agent, 2 parts by weight of starch, and 40 parts by weight of cement granular balls; or

[0033] 100 parts by weight of gypsum clinker, 70 parts by weight of water, 0.05 parts by weight of glass fiber, 1 part by weight of foaming agent, 0.1 parts by weight of retarder, 0.1 parts by weight of water reducing agent, 0.3 parts by weight of starch, and 25 parts by weight of cement granular balls; or

[0034] 100 parts by weight of gypsum clinker, 75 parts by weight of water, 0.1 parts by weight of glass fiber, 0.2 parts by weight of foaming agent, 0.25 parts by weight of retarder, 0.05 parts by weight of water reducing agent, 1.2 parts by weight of starch, and 10 parts by weight of cement granular balls.

[0035] The fifth aspect of the present application provides a method for preparing the above-mentioned gypsum board, the preparation method comprising:

[0036] Step 1, preparing cement ball particles;

[0037] Step 2: weigh each raw material component by weight;

[0038] Step 3: Evenly mix the cement granular balls prepared in step 1 with gypsum clinker, starch and glass fiber;

[0039] Step 4: Add foaming agent, retarder and water reducing agent into water, mix well to obtain a mixed solution;

[0040] Step 5: adding the mixed material of step 3 to the mixed solution of step 4, and stirring evenly to form gypsum slurry;

[0041] Step 6, attaching upper and lower protective papers to the gypsum slurry obtained in step 5, shaping, and drying to obtain the paper-faced gypsum board;

[0042] Step 7: Combine the dried boards, saw the edges, seal the edges, and package them to obtain a finished gypsum board with a thickness of 12 mm.

[0043] The sixth aspect of the present application provides a gypsum board prepared by the above-mentioned method for preparing the gypsum board.

[0044] Although the preparation method of the present application uses aerogel particles to prepare paper-faced gypsum board, in the process of preparing the paper-faced gypsum board, the aerogel is wrapped in cement powder to make cement particle balls, which are evenly dispersed in the gypsum slurry. On the one hand, this ensures that the aerogel is evenly dispersed in the gelling system, and on the other hand, the addition of cement particle balls improves the mechanical strength of the gypsum board.

[0045] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be realized and obtained by the schemes described in the description. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application will be described in detail below. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.

[0047] In the following examples, the desulfurized gypsum clinker used is made from the solid waste desulfurized gypsum produced by flue gas desulfurization in power plants, wherein the chloride ion content is ≤ ≤ 400 mg / kg and the specific surface area is 3500 cm 2 / g to 4000cm 2 / g range; glass fiber was purchased from Hebei Jinghang Mineral Products Co., Ltd.; foaming agent was purchased from Jinan Yihao Chemical Co., Ltd.; retarder is bone gelatin protein retarder, purchased from Sichuan Sanwei Jinkang Materials Technology Co., Ltd.; polycarboxylic acid water reducer was purchased from Linyi Yoshida New Building Materials Co., Ltd., model JT; aerogel is aerogel powder with a particle size of 0.1mm-1mm, purchased from Suzhou Tongxuan New Materials Co., Ltd., model KPore-G500P; modified corn starch was purchased from Jinan Yuantong Chemical Co., Ltd., the viscosity of starch is 3500mPa·s, and the viscosity test method adopts the test method in Chinese chemical industry standard HG / T 3932-2007, with a sample concentration of 5%, a temperature of 25°C, a rotor number of 3, and a speed of 6r / min; cement clinker is ordinary Portland cement, purchased from Tangshan Jidong Cement Co., Ltd., model 42.5; emulsion was purchased from Beijing Kemite Technology Development Co., Ltd.

[0048] Example 1

[0049] The gypsum board of this embodiment is prepared by the following method:

[0050] Step 1: Prepare cement ball particles:

[0051] 1. Weigh the components by weight: 100 parts of cement clinker, 22 parts by weight of emulsion, and 0.08 parts by weight of aerogel;

[0052] 2. Add aerogel to the emulsion while stirring continuously and mix evenly;

[0053] 3. Add cement clinker to the mixed components in step 2 and mix well;

[0054] 4. The mixture is passed through an 80-mesh sieve and dried at 45°C to form cement particle balls wrapped with aerogel powder.

[0055] Step 2: Weigh each component by weight: 100 parts of gypsum clinker, 62 parts of water, 0.03 parts by weight of glass fiber, 2 parts by weight of foaming agent, 0.45 parts by weight of retarder, 0.3 parts of polycarboxylic acid water reducer, 2 parts by weight of starch, and 40 parts of cement granular balls.

[0056] Step 3: Mix the cement granule balls, gypsum clinker, starch and glass fiber evenly.

[0057] Step 4: Add foaming agent, retarder and polycarboxylic acid water reducer into water and mix well.

[0058] Step 5: Add the mixture of step 3 to the mixed solution of step 4 and stir evenly to form a slurry.

[0059] Step 6: attaching upper and lower protective papers to the gypsum slurry obtained in step 5, shaping, and drying to obtain the paper-faced gypsum board.

[0060] Step 7: Combine the dried boards, saw the edges, seal the edges, and package them to obtain a finished gypsum board with a thickness of 12 mm.

[0061] Example 2

[0062] The gypsum board of this embodiment is prepared by the following method:

[0063] Step 1: Prepare cement ball particles:

[0064] 1. Weigh the components by weight: 100 parts of cement clinker, 38 parts by weight of emulsion, and 0.5 parts by weight of aerogel;

[0065] 2. Add aerogel to the emulsion while stirring continuously and mix evenly;

[0066] 3. Add cement clinker to the mixed components in step 2 and mix well;

[0067] 4. The mixture is passed through an 80-mesh sieve and dried at 45°C to form cement particle balls wrapped with aerogel powder.

[0068] Step 2: Weigh each component by weight: 100 parts of gypsum clinker, 70 parts of water, 0.05 parts by weight of glass fiber, 1 part by weight of foaming agent, 0.1 part by weight of retarder, 0.1 part of polycarboxylic acid water reducer, 0.3 part by weight of starch, and 25 parts of cement granular balls.

[0069] Steps 3 to 7 are the same as those in Example 1.

[0070] Example 3

[0071] The gypsum board of this embodiment is prepared by the following method:

[0072] Step 1: Prepare cement ball particles:

[0073] 1. Weigh the components by weight: 100 parts of cement clinker, 30 parts by weight of emulsion, and 0.3 parts by weight of aerogel;

[0074] 2. Add aerogel to the emulsion while stirring continuously and mix evenly;

[0075] 3. Add cement clinker to the mixed components in step 2 and mix well;

[0076] 4. The mixture is passed through an 80-mesh sieve and dried at 45°C to form cement particle balls wrapped with aerogel powder.

[0077] Step 2: Weigh each component by weight: 100 parts of gypsum clinker, 75 parts of water, 0.1 parts by weight of glass fiber, 0.2 parts by weight of foaming agent, 0.25 parts by weight of retarder, 0.05 parts of polycarboxylic acid water reducer, 1.2 parts by weight of starch, and 10 parts of cement granular balls.

[0078] Steps 3 to 7 are the same as those in Example 1.

[0079] Comparative Example 1

[0080] The gypsum board of this embodiment is prepared by the following method:

[0081] Step 1: Weigh each component by weight: 100 parts of gypsum clinker, 62 parts of water, 0.03 parts by weight of glass fiber, 2 parts by weight of foaming agent, 0.45 parts by weight of retarder, 0.3 parts of polycarboxylic acid water reducer, 2 parts by weight of starch, and 0.08 parts by weight of aerogel.

[0082] Step 2: Mix gypsum clinker, starch and glass fiber evenly.

[0083] Step 3: Add foaming agent, retarder, polycarboxylic acid water reducer and aerogel into water and mix. At this time, the aerogel floats on the surface of the solution due to its light weight.

[0084] Step 4: Add the mixed material of step 2 to the mixed liquid of step 3, and stir evenly to form a slurry. In this step, the aerogel powder will fly away.

[0085] Step 5: attaching upper and lower protective papers to the gypsum slurry obtained in step 5, shaping, and drying to obtain the paper-faced gypsum board.

[0086] Step 6: Combine the dried boards, saw the edges, seal the edges, and package them to obtain a finished gypsum board with a thickness of 12 mm.

[0087] Comparative Example 2

[0088] The commercially available ordinary paper-faced gypsum board was purchased from Pingyi Ounuo New Building Materials Co., Ltd., with a length × width × thickness of 3000mm × 1200mm × 12mm, and there is no aerogel in the board core.

[0089] Test Example 1

[0090] The gypsum boards of the embodiments and comparative examples were tested with reference to the Chinese national standard GB / T 9775-2008 "Gypsum Board" to detect the physical and mechanical properties of the gypsum boards. The test results are shown in Table 1.

[0091] Table 1 Performance test results of gypsum board

[0092]

[0093]

[0094] As can be seen from Table 1, the gypsum board prepared in the embodiment of the present application can meet the requirements of national standards in terms of mechanical properties, and the thermal conductivity is significantly reduced. Examples 1, 2, and 3 overcome the problems of flying and uneven dispersion of aerogel powder, or the poor adhesion of gypsum board, improve the strength of gypsum board, and are slightly higher than the commercially available ordinary gypsum board of Comparative Example 2. Comparative Example 1 changed the process and only used the aerogel component of Example 1 to prepare gypsum board. As a result, the aerogel particles affected the bonding performance of the gypsum board, thereby reducing the mechanical properties. This is because in the process of preparing the gypsum slurry, some aerogel particles cannot be completely wrapped by the gypsum slurry, float on the surface of the slurry, and after overlapping with the upper and lower layers of the facing paper, they remain on the base surface of the facing paper and the gypsum core layer, resulting in poor bonding of the board and a decrease in mechanical properties.

[0095] Conclusion: Although the preparation method of the present application uses aerogel particles to prepare paper-faced gypsum board, in the process of preparing the paper-faced gypsum board, the aerogel is wrapped in cement powder to make cement particle balls, which are evenly dispersed in the gypsum slurry. On the one hand, it ensures that the aerogel is evenly dispersed in the gelling system. On the other hand, the addition of cement particle balls improves the mechanical strength of the gypsum board.

[0096] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of patent protection of this application shall still be based on the scope defined in the attached claims.

Claims

1. A cement granule ball, the raw materials of which include the following components in parts by weight: 100 parts by weight of cement clinker, 20-40 parts by weight of emulsion, and 0.05-0.5 parts by weight of aerogel.

2. The cement granule ball according to claim 1, wherein: The cement clinker is selected from one or more of Portland cement, aluminate cement and sulphoaluminate cement; preferably, the cement clinker is ordinary Portland cement; and / or The emulsion is selected from one or more of polyvinyl acetate-ethylene emulsion, water-based acrylic emulsion, styrene-acrylic emulsion / pure acrylic emulsion, silicone-acrylic emulsion and polyurethane emulsion, etc. Preferably, the emulsion is polyvinyl acetate-ethylene emulsion; and / or The particle size of the aerogel is 5 μm to 1 mm, and the bulk density is 0.04 g / cm3 to 0.12 g / cm 3 .

3. The cement granule ball according to claim 1 or 2, wherein: The raw materials for preparing the cement granule balls include the following components in parts by weight: 100 parts by weight of cement clinker, 22 parts by weight of emulsion, and 0.08 parts by weight of aerogel; or 100 parts by weight of cement clinker, 38 parts by weight of emulsion, and 0.5 parts by weight of aerogel; or 100 parts by weight of cement clinker, 30 parts by weight of emulsion, and 0.3 parts by weight of aerogel.

4. A method for preparing cement granule balls according to any one of claims 1 to 3, comprising: 1) Weigh each raw material component; 2) Add aerogel to the emulsion while stirring continuously and mix well; 3) adding cement clinker to the mixture obtained in step 2) and mixing evenly; 4) The mixture obtained in step 3) is sieved and dried to prepare cement particle balls wrapped with aerogel powder.

5. The method according to claim 4, wherein: Step 4) is: passing the mixture obtained in step 3) through an 80-mesh sieve and drying at 45° C. to prepare the cement particle balls wrapped with aerogel powder.

6. A gypsum board, the raw materials of which include the cement granules as described in any one of claims 1 to 3 or the cement granules prepared by the method as described in claim 4 or 5, gypsum clinker and water, and one or more of glass fiber, foaming agent, retarder, water reducer and starch.

7. The gypsum board according to claim 6, wherein: The raw materials of the gypsum board include the following components in parts by weight: 100 parts by weight of gypsum clinker, 60-75 parts by weight of water, 0.02-0.1 parts by weight of glass fiber, 0.1-2 parts by weight of foaming agent, 0.1-0.5 parts by weight of retarder, 0.05-0.3 parts by weight of water reducing agent, 0.2-2 parts by weight of starch, and 10-40 parts by weight of cement granular balls.

8. The gypsum board according to claim 7, wherein: The gypsum clinker is selected from one or more of desulfurized gypsum clinker, phosphogypsum clinker and natural gypsum clinker; and / or The glass fiber is selected from any one of medium-alkali glass fiber, alkali-free glass fiber and alkali-resistant glass fiber; and / or The fiber length of the glass fiber is 9-15 mm, and the fiber monofilament diameter is 10-15 um; and / or The foaming agent is selected from one or more of the inorganic foaming agents ammonium lauryl sulfate, sodium bicarbonate, and ammonium bicarbonate; and / or The retarder is selected from one or more of citric acid, sodium citrate, sodium hexametaphosphate, borax and protein retarders. Preferably, the retarder is a protein retarder; and / or The water reducer is a polycarboxylate water reducer, preferably a powder polycarboxylate water reducer; and / or The starch is selected from one or more of modified potato starch, modified cassava starch and modified corn starch.

9. The gypsum board according to any one of claims 6 to 8, wherein: The raw materials of the gypsum board include the following components in parts by weight: 100 parts by weight of gypsum clinker, 62 parts by weight of water, 0.03 parts by weight of glass fiber, 2 parts by weight of foaming agent, 0.45 parts by weight of retarder, 0.3 parts by weight of water reducing agent, 2 parts by weight of starch, and 40 parts by weight of cement granular balls; or 100 parts by weight of gypsum clinker, 70 parts by weight of water, 0.05 parts by weight of glass fiber, 1 part by weight of foaming agent, 0.1 parts by weight of retarder, 0.1 parts by weight of water reducing agent, 0.3 parts by weight of starch, and 25 parts by weight of cement granular balls; or 100 parts by weight of gypsum clinker, 75 parts by weight of water, 0.1 parts by weight of glass fiber, 0.2 parts by weight of foaming agent, 0.25 parts by weight of retarder, 0.05 parts by weight of water reducing agent, 1.2 parts by weight of starch, and 10 parts by weight of cement granular balls.

10. A method for preparing the gypsum board according to any one of claims 6 to 9, comprising: Step 1, preparing cement ball particles; Step 2: weigh each raw material component by weight; Step 3: Evenly mix the cement granular balls prepared in step 1 with gypsum clinker, starch and glass fiber; Step 4: Add foaming agent, retarder and water reducing agent into water, mix well to obtain a mixed solution; Step 5: adding the mixed material of step 3 to the mixed solution of step 4, and stirring evenly to form gypsum slurry; Step 6, attaching upper and lower protective papers to the gypsum slurry obtained in step 5, shaping, and drying to obtain the paper-faced gypsum board; Step 7: Combine the dried boards, saw the edges, seal the edges, and package them to obtain a finished gypsum board with a thickness of 12 mm.

Citation Information

Patent Citations

  • Manufacturing method of foam cement insulation board added with polyphenyl granules

    CN104844265A

  • Method for preparing hydrophobic silica aerogel cement-based heat-preservation material

    CN107344837A

  • Gypsum plaster board and preparation method thereof

    CN113429185A