A kind of backing-free tile adhesive based on gold tailings and its preparation process

By reacting gold tailings with calcium oxide to prepare nano zero-valent iron air purification components, combined with tourmaline powder and CaTiO3:Pr3+, the problems of long construction time of existing ceramic tile glue and insufficient air purification capacity are solved, and the light-based The formaldehyde degradation and bonding performance under light-free conditions can be improved to meet the needs of environmental protection and construction efficiency.

CN118754571BActive Publication Date: 2024-11-22HENAN YUZHONG XIONGFENG BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411249686.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The existing ceramic tile glue needs to wait for the glue to cure during construction, which is time-consuming and labor-intensive, and it is difficult to achieve air purification through photocatalytic reactions, which cannot meet environmental protection needs.

Method used

Using gold tailings-based glue-free ceramic tiles, a high-load nano zero-valent iron air purification component is prepared by mixing gold tailings with calcium oxide, calcining and hydrogen reduction, combining tourmaline powder and CaTiO3:Pr3+, to Improve catalytic degradation ability and bonding properties to form materials with dual functions of photocatalytic and photocatalytic.

Benefits of technology

It realizes effective degradation of formaldehyde under light and light conditions, improves the bonding performance of ceramic tile glue and indoor air purification capabilities, and ensures construction efficiency and health and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754571B_ABST
    Figure CN118754571B_ABST
Patent Text Reader

Abstract

The invention relates to the field of building materials, in particular to a gold tailings-based adhesive-free tile adhesive and a preparation process thereof. The adhesive-free tile adhesive is prepared from the following raw materials in parts by weight: 40-50 parts of cement, 60-80 parts of sand, 5-10 parts of air purification components, 0.1-1 parts of tourmaline powder, 1-5 parts of latex powder, 0.01-0.1 parts of methyl hydroxypropyl cellulose ether, 0.01-0.1 parts of hydroxypropyl starch ether, 0-1 parts of auxiliary agents, and 20-40 parts of water. The air purification component is obtained by mixing gold tailings and calcium oxide, ball milling, calcining, and then reducing with hydrogen. After testing, the adhesive-free tile adhesive prepared by the invention has good bonding performance to tiles, can ensure that indoor tiles are laid firmly and safely, and has a certain formaldehyde degradation effect under both light and dark conditions, and can protect the health of users.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials, and in particular to a backing-free tile adhesive based on gold tailings and a preparation process thereof. Background Art

[0002] In recent years, with the development of the ceramic tile industry, the size of ceramic tiles has increased rapidly. The mainstream brick type on the market has changed from 300mm×300mm to 400 mm×800mm. Various ceramic tile manufacturers have even launched ceramic thin plates, whose size specifications are generally above 1200mm×2400mm. However, the increase in ceramic tile size specifications has also brought new challenges to the laying of ceramic tiles.

[0003] To this end, tile adhesive manufacturers have launched adhesive products to match tile adhesive for laying tiles, thereby greatly improving the adhesion between tiles and the base wall. However, the installation period of using tile adhesive is long, and it is necessary to wait for the adhesive to cure before proceeding to the next step of construction, which is time-consuming and labor-intensive. Moreover, with the current increase in environmental protection needs, tile adhesive cannot be compatible with the current photocatalytic system, and it is difficult to achieve the purpose of air purification through photocatalytic reactions. Although there are relevant journals and papers on non-photocatalytic degradation of organic matter, there are few reports on its application in tile adhesive.

[0004] The article "Study on Photocatalytic and Lightless Degradation Behavior of Methyl Orange by Cu2O / Zeolite Composite Photocatalyst" studied the degradation characteristics of methyl orange by Cu2O / zeolite composite photocatalyst under lightless conditions.

[0005] "Structural Evolution and Photocatalytic Degradation Performance of Nano-Zero-Valent Zinc" studied how nano-zero-valent metals with strong reduction activity can effectively degrade organic pollutants in dye wastewater under lightless conditions.

[0006] The article "Preparation of Nano-ZnO / Zn / CNT Porous Composite Structures and Their Photocatalytic Degradation of Methylene Blue" studied that the ZnO nanorods play a major role in the catalytic degradation of methylene blue by the composite structure. The ZnO nanorods are deformed under force in the porous structure to produce electron-hole pairs, which can degrade organic pollutants under lightless conditions. The larger the pore size and the stronger the impact of the water flow, the better the catalytic degradation effect on methylene blue. Summary of the invention

[0007] Purpose of the invention: In view of the above technical problems, the present invention proposes a backing-free tile adhesive based on gold tailings and a preparation process thereof.

[0008] The technical solutions adopted are as follows:

[0009] A gold tailings-based, adhesive-free tile adhesive is prepared from the following raw materials in parts by weight:

[0010] 40-50 parts of cement, 60-80 parts of sand, 5-10 parts of air purification components, 0.1-1 parts of tourmaline powder, 1-5 parts of latex powder, 0.01-0.1 parts of methyl hydroxypropyl cellulose ether, 0.01-0.1 parts of hydroxypropyl starch ether, 0-1 parts of additives, and 20-40 parts of water;

[0011] The air purification component is obtained by mixing gold tailings and calcium oxide, ball milling, calcining and then reducing with hydrogen;

[0012] The latex powder includes styrene-butyl acrylate copolymer and ethylene-vinyl acetate copolymer;

[0013] The mass ratio of the styrene-butyl acrylate copolymer to the ethylene-vinyl acetate copolymer is 1-5:1-5;

[0014] Also includes CaTiO3:Ln 3+ , Ln is Pr, the CaTiO3:Ln 3+ The dosage is 0.1-1% by weight of the air purification component.

[0015] Furthermore, the mass ratio of the gold tailings to calcium oxide is 1-30:1.

[0016] Furthermore, the calcination temperature is 1200-1300° C., and the calcination time is 1-5 hours.

[0017] Furthermore, the temperature during hydrogen reduction is 900-950°C.

[0018] Furthermore, the auxiliary agent includes any one or more combinations of an early strength agent, a water reducing agent, and a water repellent agent.

[0019] The present invention also provides a preparation process of a backing-free tile adhesive based on gold tailings:

[0020] First, the latex powder is dispersed in water to obtain a dispersion, and the air purification component, tourmaline powder, and CaTiO3:Ln 3+ After ball milling, the mixture is dried to obtain a mixture, cement, sand and the mixture are added to the dispersion and mixed evenly, and finally methyl hydroxypropyl cellulose ether, hydroxypropyl starch ether and additives are added and stirred sufficiently.

[0021] Beneficial effects of the present invention:

[0022] The present invention provides a backing-free tile adhesive based on gold tailings. The gold tailings contain a high content of iron oxide. The applicant prepares an air purification component with a high reduction performance nano zero-valent iron by reacting the gold tailings with calcium oxide, calcining and reducing the iron oxide. Tourmaline can oxidize the water molecules on its surface into hydroxyl radicals, thereby increasing the catalytic degradation ability of the nano zero-valent iron on gaseous pollutants. In addition, tourmaline itself also has certain catalytic degradation and antibacterial and antibacterial properties, which can prevent the tile adhesive from getting moldy and promote indoor air purification.

[0023] The latex powder composed of styrene-butyl acrylate copolymer and ethylene-vinyl acetate copolymer can improve the interfacial bonding performance between tile adhesive and substrate, and due to the introduction of styrene chain segments, the water resistance, alkali resistance and bonding strength of the formed polymer film are improved;

[0024] CaTiO3 is a typical representative of ABO3 perovskite crystal structure. It has good ferroelectric, dielectric, thermoelectric and photocatalytic activities and is widely used. After being doped with lanthanide rare earth elements, it can cooperate with nano zero-valent iron to improve the photocatalytic activity of air purification components, allowing tile adhesive to still maintain a certain formaldehyde purification activity.

[0025] Our company's original research direction was to combine fluorescent materials with photocatalytic activity with gold tailings in order to achieve all-weather photocatalytic reaction. However, after research, we found that the prepared material can achieve lightless degradation of formaldehyde. Although the microscopic mechanism of its macroscopic characteristics is not clear, it is compatible with the characteristics of tile adhesive materials, so this application is proposed;

[0026] After testing, it is found that the adhesive-free tile adhesive prepared by the present invention has good bonding performance to tiles, which can ensure that indoor tile paving is both stable and safe, and has a certain formaldehyde degradation effect under both light and dark conditions, which can protect the health of users. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a microscopic morphology of the air purification component prepared in Example 1. DETAILED DESCRIPTION

[0028] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0029] Cement: P·O42.5 ordinary Portland cement, Conch brand;

[0030] Sand: 40-70 mesh and 70-140 mesh river sand are mixed in a mass ratio of 1:1;

[0031] Air purification components: Homemade, the specific method is as follows:

[0032] The gold tailings with a mass ratio of 10:1 were crushed and added to the ball mill with calcium oxide. Anhydrous ethanol was used as the ball milling medium. The mixture was mixed and ball milled on a planetary ball mill for 5 hours. The mixture was taken out and dried.

[0033] After calcination at 1250°C for 5 h in air atmosphere, the alloy was reduced at 950°C for 2 h in hydrogen atmosphere in a tubular furnace.

[0034] Gold tailings: China Gold Group Hunan Xinrui Mining Co., Ltd., the composition is shown in Table 1 below:

[0035] Table 1: Chemical composition (mass fraction) / %:

[0036] ;

[0037] Tourmaline powder:

[0038] CaTiO3:Pr 3+ : Homemade, the specific method is as follows:

[0039] CaTiO3:Pr was prepared by hydrothermal method using n-butyl titanate, calcium nitrate and praseodymium nitrate as raw materials. 3+ First, a 1 mol / L n-butyl titanate solution was prepared with dilute hydrochloric acid as a hydrolysis inhibitor, and then a calcium nitrate solution and a praseodymium nitrate solution with concentrations of 1 mol / L and 0.005 mol / L were prepared respectively. The three solutions of equal volume were mixed, and polyethylene glycol 6000 was added as a dispersant. After stirring evenly, a NaOH solution was dropped into the mixture to completely precipitate all metal ions. The pH value of the solution was measured to be 8. The reaction solution was transferred to a high-pressure reactor, sealed and heated to 200°C for reaction for 6 hours. After cooling, the precipitate was taken out, filtered, washed and dried repeatedly, and finally calcined at 900°C for 1 hour.

[0040] Styrene-butyl acrylate copolymer latex powder: FX7000, Elite Corporation;

[0041] Ethylene-vinyl acetate copolymer latex powder: 4018 N, Wacker, Germany;

[0042] Methyl hydroxypropyl cellulose ether: Hebei Zexu Building Materials Technology Development Co., Ltd.;

[0043] Hydroxypropyl starch ether: Hebei Yida Cellulose Co., Ltd.

[0044] Polycarboxylate water reducer: Qingdao Xinzhongwei;

[0045] Water: tap water.

[0046] Embodiment 1:

[0047] A gold tailings-based, adhesive-free tile adhesive is prepared from the following raw materials in parts by weight:

[0048] 45 parts of cement, 70 parts of sand, 8 parts of air purification components, 0.5 parts of tourmaline powder, CaTiO3:Pr 3+ 0.08 parts, styrene-butyl acrylate copolymer latex powder 1 part, ethylene-vinyl acetate copolymer latex powder 2 parts, methyl hydroxypropyl cellulose ether 0.05 parts, hydroxypropyl starch ether 0.05 parts, polycarboxylate water reducer 0.1 parts, water 30 parts;

[0049] The preparation process of the above-mentioned adhesive-free tile adhesive based on gold tailings:

[0050] First, add styrene-butyl acrylate copolymer latex powder and ethylene-vinyl acetate copolymer latex powder into water, stir to disperse and obtain dispersion liquid, then add air purification component, tourmaline powder and CaTiO3:Pr 3+ Add to a ball mill, use anhydrous ethanol as the ball milling medium, mix and ball mill on a planetary ball mill for 5 hours and then dry to obtain a mixture, add cement, sand and the mixture to the dispersion and mechanically stir to mix, finally add methyl hydroxypropyl cellulose ether, hydroxypropyl starch ether and polycarboxylate water reducer and stir well;

[0051] The tensile bond strength of the sample prepared in this embodiment was tested with reference to JC / T 5472017 "Ceramic Tile Adhesive". The tensile bond strength was 2.63 MPa after curing at room temperature for 28 days.

[0052] Embodiment 2:

[0053] A gold tailings-based, adhesive-free tile adhesive is prepared from the following raw materials in parts by weight:

[0054] 50 parts of cement, 60 parts of sand, 5 parts of air purification components, 0.5 parts of tourmaline powder, CaTiO3:Pr 3+ 0.01 parts, styrene-butyl acrylate copolymer latex powder 1 parts, ethylene-vinyl acetate copolymer latex powder 2 parts, methyl hydroxypropyl cellulose ether 0.01 parts, hydroxypropyl starch ether 0.01 parts, polycarboxylate water reducer 0.1 parts, water 30 parts;

[0055] The preparation process of the above-mentioned adhesive-free tile adhesive based on gold tailings:

[0056] First, add styrene-butyl acrylate copolymer latex powder and ethylene-vinyl acetate copolymer latex powder into water, stir to disperse and obtain dispersion liquid, then add air purification component, tourmaline powder and CaTiO3:Pr 3+ Add to a ball mill, use anhydrous ethanol as the ball milling medium, mix and ball mill on a planetary ball mill for 5 hours and then dry to obtain a mixture, add cement, sand and the mixture to the dispersion and mechanically stir to mix, finally add methyl hydroxypropyl cellulose ether, hydroxypropyl starch ether and polycarboxylate water reducer and stir well;

[0057] The tensile bond strength of the samples prepared in this embodiment was tested with reference to JC / T 5472017 "Ceramic Tile Adhesives". The tensile bond strength was 2.55 MPa after curing at room temperature for 28 days.

[0058] Embodiment 3:

[0059] A gold tailings-based, adhesive-free tile adhesive is prepared from the following raw materials in parts by weight:

[0060] 40 parts of cement, 80 parts of sand, 10 parts of air purification components, 0.5 parts of tourmaline powder, CaTiO3:Pr 3+ 0.05 parts, styrene-butyl acrylate copolymer latex powder 1 part, ethylene-vinyl acetate copolymer latex powder 2 parts, methyl hydroxypropyl cellulose ether 0.02 parts, hydroxypropyl starch ether 0.02 parts, polycarboxylate water reducer 0.2 parts, water 40 parts;

[0061] The preparation process of the above-mentioned adhesive-free tile adhesive based on gold tailings:

[0062] First, add styrene-butyl acrylate copolymer latex powder and ethylene-vinyl acetate copolymer latex powder into water, stir to disperse and obtain dispersion liquid, then add air purification component, tourmaline powder and CaTiO3:Pr 3+ Add into the ball mill, use anhydrous ethanol as the ball milling medium, mix and ball mill on a planetary ball mill for 5 hours and then dry to obtain a mixture. Add cement, sand and the mixture into the dispersion and stir mechanically to mix. Finally, add methyl hydroxypropyl cellulose ether, hydroxypropyl starch ether and polycarboxylic acid water reducer and stir thoroughly.

[0063] The tensile bond strength of the sample prepared in this embodiment was tested with reference to JC / T 5472017 "Ceramic Tile Adhesive". The tensile bond strength was 2.32 MPa after curing at room temperature for 28 days.

[0064] Comparative Example 1: Basically the same as Example 1, except that no styrene-butyl acrylate copolymer latex powder is added. The tensile bonding strength of the samples prepared in this example is tested with reference to JC / T 5472017 "Ceramic Tile Adhesive". The tensile bonding strength after 28 days of curing at room temperature is 1.93 MPa.

[0065] Comparative Example 2: is basically the same as Example 1, except that no ethylene-vinyl acetate copolymer latex powder is added. The tensile bonding strength of the samples prepared in this example is tested with reference to JC / T 5472017 "Ceramic Tile Adhesives". The tensile bonding strength after 28 days of curing at room temperature is 2.14 MPa.

[0066] Comparative Example 3: The same as Example 1, except that no CaTiO3:Pr 3+ , referring to JC / T 5472017 "Ceramic Tile Adhesive", the tensile bond strength of the sample prepared in this embodiment was tested, and the tensile bond strength after curing at room temperature for 28 days was 2.51 MPa.

[0067] Comparative Example 4: The same as Example 1, except that CaTiO3 is used instead of CaTiO3:Pr 3+ , referring to JC / T5472017 "Ceramic Tile Adhesive", the tensile bonding strength of the sample prepared in this embodiment was tested, and the tensile bonding strength after curing at room temperature for 28 days was 2.50 MPa.

[0068] Comparative Example 5: is basically the same as Example 1, except that tourmaline powder is not added. The tensile bonding strength of the samples prepared in this example is tested with reference to JC / T 547-2017 "Ceramic Tile Adhesive". The tensile bonding strength after curing at room temperature for 28 days is 2.48 MPa.

[0069] Performance Testing:

[0070] ① The anti-formaldehyde performance of the adhesive-free tile adhesive prepared in Examples 1-3 and Comparative Examples 1-5 was tested with reference to the method in JC / T 1074-2008 "Purification Performance of Indoor Air Purification Functional Coating Materials";

[0071] Test conditions: temperature (20±2)℃, relative humidity (50±10)%, cube test chamber: 1m 3 , 50W fluorescent lamp, 10W air fan, take 8 identical test boxes and number them respectively, the inner wall size of the test box is 1250mm×800mm×1000mm, and introduce 10mg / m 3The formaldehyde-free tile adhesive was poured into a 500mm×500mm×5mm mold, dried naturally at room temperature for 7 days, and then placed in a test box for experiment. The experimental time was 24 hours.

[0072] The test results are shown in Table 2 below:

[0073] Table 2:

[0074] ;

[0075] It can be seen from Table 2 above that the adhesive-free tile adhesive prepared in the present invention has excellent formaldehyde removal performance under visible light.

[0076] ② The anti-formaldehyde performance of the adhesive-free tile adhesive prepared in Examples 1-3 and Comparative Examples 1-5 was tested under lightless conditions, referring to the method in JC / T 1074-2008 "Purification Performance of Indoor Air Purification Functional Coating Materials";

[0077] Test conditions: temperature (20±2)℃, relative humidity (50±10)%, cube test chamber: 1m 3 , in the dark condition, 10W air fan, take 8 identical test boxes, number them respectively, the inner wall size of the test box is 1250mm×800mm×1000mm, and introduce 10mg / m 3 The formaldehyde-free tile adhesive was poured into a 500mm×500mm×5mm mold. After natural drying for 7 days at room temperature, it was placed in a test box for 24 hours.

[0078] The test results are shown in Table 3 below:

[0079] Table 3:

[0080] ;

[0081] It can be seen from Table 3 above that the adhesive-free tile adhesive prepared in the present invention still has a certain ability to remove formaldehyde under dark conditions.

[0082] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A backing-free tile adhesive based on gold tailings, characterized in that: Made from the following raw materials in parts by weight: 40-50 parts of cement, 60-80 parts of sand, 5-10 parts of air purification components, 0.1-1 parts of tourmaline powder, 1-5 parts of latex powder, 0.01-0.1 parts of methyl hydroxypropyl cellulose ether, 0.01-0.1 parts of hydroxypropyl starch ether, 0-1 parts of additives, and 20-40 parts of water; The preparation method of the air purification component is as follows: The gold tailings were crushed and added to a ball mill with calcium oxide, and anhydrous ethanol was used as the ball milling medium. The mixture was mixed and ball milled for 5 hours on a planetary ball mill to obtain a mixture. The mixture was taken out and dried, calcined in an air atmosphere, and then reduced in a tubular furnace under a hydrogen atmosphere for 2 hours. The mass ratio of the gold tailings to calcium oxide is 1-30:1; The calcination temperature is 1200-1300°C and the calcination time is 1-5h; The temperature during hydrogen reduction is 900-950°C; The latex powder includes styrene-butyl acrylate copolymer and ethylene-vinyl acetate copolymer; The mass ratio of the styrene-butyl acrylate copolymer to the ethylene-vinyl acetate copolymer is 1-5:1-5; Also includes CaTiO3:Ln 3+ , Ln is Pr, the CaTiO3:Ln 3+ The dosage is 0.1-1% by weight of the air purification component.

2. The adhesive-free tile adhesive based on gold tailings according to claim 1, characterized in that: The auxiliary agent includes any one or more combinations of an early strength agent, a water reducing agent, and a water repellent agent.

3. A preparation process of the adhesive-free tile adhesive based on gold tailings as claimed in claim 1 or 2, characterized in that: First, the latex powder is dispersed in water to obtain a dispersion, and the air purification component, tourmaline powder, CaTiO3:Ln 3+ After ball milling, the mixture is dried to obtain a mixture, cement, sand and the mixture are added to the dispersion and mixed evenly, and finally methyl hydroxypropyl cellulose ether, hydroxypropyl starch ether and additives are added and stirred sufficiently.