Golden yellow tungsten oxide / carbon-based composite film as well as preparation method and application thereof
By preparing a golden tungsten oxide/carbon-based composite film, the problem that the tungsten oxide film cannot achieve metallic luster and electrochromic properties is solved, and the effect of stably displaying multi-color states and reducing power consumption in electronic products is achieved, which is suitable for electronic products. Equipment back panel and personalized decoration.
Patent Information
- Application Number
- CN202410839352.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-11
AI Technical Summary
Existing tungsten oxide films cannot achieve metallic luster and electrochromic properties, which limits their application in electronic product decoration.
A golden yellow tungsten oxide/carbon-based composite film is prepared by dissolving tungstic acid powder with ethanolamine and fructose to form an aqueous precursor, coating and annealing to form a composite film with metallic luster and electrochromic properties.
It achieves stable display of reversible color switching between golden yellow and blue in electronic products, enriches the display color gamut, reduces power consumption, and avoids signal shielding problems. It is suitable for electronic device backplanes and personalized decoration.
Smart Images

Figure CN118754609A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochromism and relates to a golden tungsten oxide / carbon-based composite film and a preparation method and application thereof. Background Art
[0002] Electrochromic materials can adjust their optical properties under the stimulation of an applied voltage, and dynamically and reversibly switch between different colors. This special function makes it possible to be used in the personalized decoration of electronic products. In recent years, the appearance design of portable personal electronic products such as mobile phones has gradually become intelligent. At present, there is no breakthrough change in the screen shape. In order to make the mobile phone more recognizable, many manufacturers have turned their attention to the back cover of the mobile phone. Single color, gradient color and even transparent back cover are difficult to meet market demand. Well-known mobile phone manufacturers have successively launched concept models with electrochromic back covers, which are very popular.
[0003] Tungsten oxide is the most common inorganic electrochromic material. It has the advantages of good electrochemical stability and high optical contrast, and is the mainstream raw material for products such as electrochromic windows. However, due to the photoelectric properties of the material itself, it can usually only achieve a color transition from colorless and transparent to dark blue. In addition, as a typical inorganic non-metallic material, tungsten oxide film cannot obtain a metallic luster texture. These limiting factors have an adverse effect on its use as a decoration for electronic products. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a golden tungsten oxide / carbon-based composite film and its preparation method and application. The film has metallic luster and electrochromic properties, and the preparation method is simple and can be suitable for electronic products.
[0005] To achieve the above object, the method for preparing the golden tungsten oxide / carbon-based composite film of the present invention comprises:
[0006] 1) Synthesizing an aqueous precursor rich in tungsten source and carbon source;
[0007] 2) coating the aqueous precursor obtained in step 1) on a substrate to form a film to obtain a sample;
[0008] 3) Annealing the sample obtained in step 2) to obtain a tungsten oxide / carbon-based composite film.
[0009] The specific operations of step 1) are:
[0010] Tungstic acid powder and ethanolamine are dissolved in deionized water, and a carbon source is added and dissolved to obtain an aqueous precursor rich in tungsten source and carbon source.
[0011] The mass ratio of tungstic acid powder to ethanolamine is 1:(0.5-2).
[0012] The carbon source is fructose.
[0013] The aqueous precursor obtained in step 1) is coated on the substrate to form a film by using a drop coating method or a blade coating method.
[0014] The annealing temperature in step 3) is 450-550°C.
[0015] The annealing time in step 3) is 1-2 hours.
[0016] The golden tungsten oxide / carbon-based composite film of the present invention is prepared based on the preparation method of the golden tungsten oxide / carbon-based composite film.
[0017] The golden tungsten oxide / carbon-based composite film of the present invention is used as an electrochromic material in the field of electronic products.
[0018] The present invention has the following beneficial effects:
[0019] The golden tungsten oxide / carbon-based composite film and its preparation method and application described in the present invention are annealed after the aqueous precursor rich in tungsten source and carbon source is formed into a film to form a composite film with metallic luster. The film can maintain its stable color and physical and chemical properties after being placed in the air for several months. After the film is assembled into a device with an electrolyte and a counter electrode, a reversible and stable golden yellow to blue color change can occur under the action of voltage, and it undergoes multiple color states such as cyan and green, which greatly enriches the display color range, improves the appearance quality, and is green and environmentally friendly with low cost. In addition, it should be noted that since the tungsten oxide electrochromic device has a good open circuit memory effect, its color can still be stably maintained for a certain period of time after the voltage is removed, which can reduce the power consumption of electronic equipment. At the same time, the color-changing device is equipped with a non-metallic backplane, which avoids the problem of signal shielding of electronic equipment by the metal backplane in the past. The various functions and advantages of the above-mentioned film do not interfere with each other, so that the film has broad application prospects in the field of electronic equipment backplane and personalized decoration. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a Raman spectrum of the tungsten oxide / carbon-based composite film prepared in Example 1;
[0021] Figure 2 is the XRD pattern of the tungsten oxide / carbon-based composite film prepared in Example 1;
[0022] Figure 3 is a SEM image of the tungsten oxide / carbon-based composite film prepared in Example 1;
[0023] Figure 4 This is a photo of the colorful optical state of the tungsten oxide / carbon-based composite film prepared in Example 1;
[0024] Figure 5 The reflectivity spectra of the tungsten oxide / carbon-based composite film prepared in Example 1 in the golden state and the blue state. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only an embodiment of a part of the present invention, not all embodiments, and is not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concepts disclosed in the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work should fall within the scope of protection of the present invention.
[0026] The method for preparing the golden tungsten oxide / carbon-based composite film of the present invention comprises the following steps:
[0027] 1) Synthesizing an aqueous precursor rich in tungsten source and carbon source;
[0028] 2) coating the aqueous precursor obtained in step 1) on a substrate to form a film to obtain a sample;
[0029] 3) The sample obtained in step 2) is subjected to high temperature annealing treatment to obtain a tungsten oxide / carbon-based composite film.
[0030] The specific operations of step 1) are:
[0031] Tungstic acid powder and ethanolamine are dissolved in deionized water at a mass ratio of 1:(0.5-2), and a carbon source is added and dissolved to obtain an aqueous precursor rich in tungsten source and carbon source, wherein the carbon source is fructose.
[0032] In step 2), the aqueous precursor obtained in step 1) is coated on the substrate to form a film by using a drop coating method or a blade coating method.
[0033] The annealing temperature in step 3) is 450-550° C. and the annealing time is 1-2 hours.
[0034] The invention discloses a golden tungsten oxide / carbon-based composite film. The golden tungsten oxide / carbon-based composite film is prepared based on a preparation method of the golden tungsten oxide / carbon-based composite film.
[0035] The color of the golden tungsten oxide / carbon-based composite film of the present invention can be reversibly switched between golden and blue, and can be applied to the personalized decoration of electronic products such as mobile phone covers.
[0036] Embodiment 1
[0037] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0038] 1) Dissolve 1 g of tungstic acid and 0.7 g of ethanolamine in 9 g of water, and then heat in a 65°C oil bath for 2 h to fully react. After the solution is cooled, add 3 g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0039] 2) The precursor solution was applied to the FTO conductive substrate by drop coating, and allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally. The film was then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0040] 3) The sample obtained in step 2) is placed in an air atmosphere, heated to 450° C. at a heating rate of 7° C. / min, kept at this temperature for 2 h, and then naturally cooled to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0041] Figure 1 is the Raman spectrum of the tungsten oxide / carbon-based composite film prepared in Example 1, referring to Figure 1 , 261cm -1 、327cm -1 、705cm -1 、805cm -1 The wave number belongs to the signal of monoclinic tungsten oxide, while 1364cm -1 , and 1588cm -1 The wave numbers belong to typical vibration modes of carbon materials.
[0042] Figure 2 The XRD diagram of the tungsten oxide / carbon-based composite film of the present invention is shown in FIG. Figure 2 , in addition to the diffraction peak of the FTO substrate, the diffraction peak of monoclinic tungsten oxide was detected.
[0043] Figure 3 The SEM image of the tungsten oxide / carbon-based composite film prepared in Example 1 is shown in FIG. Figure 3 Tungsten oxide presents a typical polycrystalline structure with a grain size ranging from tens to one hundred nanometers. The composite film contains abundant pores, which is conducive to the embedding and extraction of cations during the electrochromic process.
[0044] Figure 4 This is a photo of the colorful optical state of the tungsten oxide / carbon-based composite film prepared in Example 1, refer to Figure 4 Under different applied voltages, the film gradually changes color from golden yellow to dark blue, and has the ability to change colors in multiple colors.
[0045] Figure 5 The golden state and blue state reflectivity spectra of the tungsten oxide / carbon-based composite film prepared in Example 1 are shown in FIG. Figure 5 ,The reflection spectra of the two color states are quite different, indicating that the color of the composite film is determined by its reflection spectrum.
[0046] Embodiment 2
[0047] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0048] 1) Dissolve 1 g of tungstic acid and 0.7 g of ethanolamine in 9 g of water, and then heat in an oil bath at 65° C. for 2 h to fully react. After the solution is cooled, add 3 g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0049] 2) The precursor solution was applied to the FTO conductive substrate by drop coating, and allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally. The film was then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0050] 3) The sample obtained by carbonization in step 2) was placed in an air atmosphere, heated to 550°C at a heating rate of 9°C / min, kept at that temperature for 1 hour, and then naturally cooled to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0051] Embodiment 3
[0052] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0053] 1) Dissolve 1 g of tungstic acid and 0.5 g of ethanolamine in 8.5 g of water, and then heat in an oil bath at 65° C. for 2 h to fully react. After the solution is cooled, add 3 g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0054] 2) The precursor solution was applied to the FTO conductive substrate by drop coating, and then allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally, and then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0055] 3) The sample obtained by carbonization in step 2) was placed in an air atmosphere, heated to 500°C at a heating rate of 8°C / min, kept at that temperature for 1 hour, and then naturally cooled to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0056] Embodiment 4
[0057] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0058] 1) Dissolve 0.5 g of tungstic acid and 1 g of ethanolamine in 8.5 g of water, and then heat in an oil bath at 65° C. for 2 h to fully react. After the solution is cooled, add 3 g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0059] 2) The precursor solution was applied to the FTO conductive substrate by drop coating, and allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally. The film was then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0060] 3) The sample obtained in step 2) was placed in an air atmosphere, heated to 500°C at a heating rate of 8°C / min, kept at that temperature for 1 hour, and then naturally cooled to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0061] Embodiment 5
[0062] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0063] 1) Dissolve 1 g of tungstic acid and 0.5 g of ethanolamine in 8.5 g of water, and then heat in an oil bath at 65° C. for 2 h to fully react. After the solution is cooled, add 3 g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0064] 2) The precursor solution was applied to the FTO conductive substrate by drop coating, and allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally. The film was then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0065] 3) placing the sample obtained in step 2) in an air atmosphere, heating it to 450°C at a heating rate of 7°C / min, keeping it at that temperature for 2 hours, and then naturally cooling it to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0066] Embodiment 6
[0067] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0068] 1) Dissolve 0.5 g of tungstic acid and 1 g of ethanolamine in 8.5 g of water, and then heat in an oil bath at 65° C. for 2 h to fully react. After the solution is cooled, add 3 g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0069] 2) The precursor solution was applied to the FTO conductive substrate by drop coating, and allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally. The film was then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0070] 3) The sample obtained by carbonization in step 2) was placed in an air atmosphere, heated to 450°C at a heating rate of 7°C / min, kept at this temperature for 2 hours, and then naturally cooled to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0071] Embodiment 7
[0072] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0073] 1) Dissolve 1 g of tungstic acid and 0.5 g of ethanolamine in 8.5 g of water, and then heat in a 65°C oil bath for 2 h to fully react. After the solution is cooled, add 2 g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0074] 2) The precursor solution was applied to the FTO conductive substrate by drop coating, and allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally. The film was then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0075] 3) The sample obtained in step 2) is placed in an air atmosphere, heated to 450° C. at a heating rate of 7° C. / min, kept at this temperature for 2 h, and then naturally cooled to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0076] Embodiment 8
[0077] The method for preparing the golden tungsten oxide / carbon-based composite film described in this embodiment comprises the following steps:
[0078] 1) Dissolve 1g of tungstic acid and 1g of ethanolamine in 8g of water, and then heat in an oil bath at 65°C for 2h for full reaction. After the solution is cooled, add 1g of fructose to obtain a precursor solution of tungsten oxide / carbon-based composite film.
[0079] 2) The precursor solution was coated on the FTO conductive substrate by a blade coating method, and allowed to stand at room temperature for 12 hours to allow the water to evaporate naturally. The film was then transferred to a 100°C heating plate to completely dry the film. After the film was dried, it was heated on a 350°C heating plate for 30 minutes to carbonize the organic matter to obtain a black sample.
[0080] 3) The sample obtained by carbonization in step 2) was placed in an air atmosphere, heated to 500°C at a heating rate of 8°C / min, kept at that temperature for 1 hour, and then naturally cooled to room temperature to obtain a golden tungsten oxide / carbon-based composite film.
[0081] Application Examples
[0082] The golden tungsten oxide / carbon-based composite electrochromic film prepared according to the embodiment is connected to one pole of a DC regulated power supply, and the other pole is connected to a blank FTO conductive glass. The electrochromic film and the blank FTO conductive glass are placed face to face and immersed in an electrolyte at the same time. By applying different voltages, the film can be switched between golden yellow and blue. The electrolyte can be a lithium perchlorate solution.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a golden tungsten oxide / carbon-based composite film, characterized in that: include: 1) Synthesizing an aqueous precursor rich in tungsten source and carbon source; 2) coating the aqueous precursor obtained in step 1) on a substrate to form a film to obtain a sample; 3) Annealing the sample obtained in step 2) to obtain a tungsten oxide / carbon-based composite film.
2. The method for preparing the golden tungsten oxide / carbon-based composite film according to claim 1, characterized in that: The specific operations of step 1) are: Tungstic acid powder and ethanolamine are dissolved in deionized water, and a carbon source is added and dissolved to obtain an aqueous precursor rich in tungsten source and carbon source.
3. The method for preparing the golden tungsten oxide / carbon-based composite film according to claim 1, characterized in that: The mass ratio of tungstic acid powder to ethanolamine is 1:(0.5-2).
4. The method for preparing the golden tungsten oxide / carbon-based composite film according to claim 1, characterized in that: The carbon source is fructose.
5. The method for preparing the golden tungsten oxide / carbon-based composite film according to claim 1, characterized in that: The aqueous precursor obtained in step 1) is coated on the substrate to form a film by using a drop coating method or a blade coating method.
6. The method for preparing the golden tungsten oxide / carbon-based composite film according to claim 1, characterized in that: The annealing temperature in step 3) is 450-550°C.
7. The method for preparing the golden tungsten oxide / carbon-based composite film according to claim 1, characterized in that: The annealing time in step 3) is 1-2 hours.
8. A golden tungsten oxide / carbon-based composite film, characterized in that: It is prepared based on the preparation method of the golden tungsten oxide / carbon-based composite film according to any one of claims 1-7.
9. Use of the golden tungsten oxide / carbon-based composite film according to claim 8 as an electrochromic material in the field of electronic products.
Citation Information
Patent Citations
Method for preparing organic composite WO3 electrochomeric films
CN101633566A
Electrochromic device based intelligent electronic curtain and production method thereof
CN105093769A
Preparation method suitable for large-area production of low-cost and environment-friendly tungsten oxide electrochromic film
CN110590180A
Green production process for preparing oxide electrochromic film by using waste carbonated beverage
CN114804653A
Process for preparing a multi-layer electrochromic structure
US20140205746A1