Magnesia-iron spinel brick for cement kiln and preparation method thereof
By adding iron powder, alumina powder and titanium carbide powder to mafic spinel bricks for cement kilns, the TAF20 metal cermet phase was generated, which solved the problem of divalent iron transformation of mafic spinel bricks at high temperatures, and improved the hanging The kiln skin performance and high temperature strength enhance the comprehensive performance of the material.
Patent Information
- Application Number
- CN202411248214.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-06
AI Technical Summary
During the high-temperature firing process of existing mafic spinel bricks, divalent ferrous oxide is converted into trivalent iron, resulting in the reduction of the performance and toughness of the kiln skin, and the low melting point of the iron powder leads to the material strength at high temperature. reduce.
Iron powder, alumina powder and titanium carbide powder are added to the preparation of mafic spinel bricks. These materials react at high temperature to form a TAF20 cermet phase to prevent the conversion of divalent iron into trivalent iron and improve the brick body High temperature strength and toughness.
It effectively improves the high-temperature strength and toughness of mafic spinel bricks, prevents iron powder from melting into liquid iron element at high temperatures, and enhances the comprehensive performance of the material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a magnesia-iron spinel brick for a cement kiln and a preparation method thereof. Background Art
[0002] Cement rotary kiln is an important equipment in cement production. The lining material of the high temperature zone of cement rotary kiln is the key factor to ensure the stable operation of the kiln body under high temperature environment. Its lining material needs to have good high temperature resistance, chemical stability, mechanical strength, wear resistance and thermal shock stability. Magnesia-chrome bricks are widely used as lining materials in the high temperature zone of cement rotary kiln due to their inertness to alkaline cement components and good kiln skin bonding ability. However, since the highly toxic hexavalent chromium soluble in water in magnesia-chrome bricks after use will cause serious environmental pollution, chromium-free alkaline refractory materials are gradually replacing chromium-containing refractory materials. Magnesia-iron-aluminum spinel material is currently considered to be the best material to replace magnesia-chrome bricks for cement rotary kiln firing zone. It not only has the excellent performance of magnesia-chrome bricks, but also has good structural toughness and lower thermal conductivity, which meets the demand for refractory materials in the kiln lining of cement rotary kiln firing zone.
[0003] The Chinese patent document with publication number CN115124359A discloses a high-stability magnesia-iron spinel brick specially used for cement kilns and a preparation method thereof. The magnesia-iron spinel brick is prepared by using high-iron magnesia sand, high-purity magnesia sand, magnesia-iron-aluminum spinel particles, and a resin binder. The obtained magnesia-iron spinel brick has outstanding acid and alkali corrosion resistance and can be used stably for a long time. Under the working condition of the cement rotary kiln, the presence of ferrous oxide in the magnesia-iron spinel brick can promote the stability of the cement rotary kiln skin. However, the magnesia-iron spinel brick in the above patent, during the high-temperature firing process, the divalent ferrous oxide in the magnesia-iron-aluminum spinel in the brick body will be converted into trivalent iron at high temperature, thereby reducing the kiln skin performance and toughness of the brick body. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a magnesia-iron spinel brick for cement kiln and a preparation method thereof. The addition of iron powder, alumina powder and titanium carbide powder can prevent the divalent ferrous oxide in the ferroalumina spinel from being converted into trivalent iron, thereby improving the kiln skin performance of the brick body. The iron powder, alumina powder and titanium carbide powder can react to generate a TAF20 metal ceramic phase, which can promote the formation of the magnesia-iron spinel phase, improve the high-temperature strength of the brick, and avoid the influence of the iron powder melting into liquid iron element at high temperature on the high-temperature strength of the magnesia-iron spinel brick.
[0005] In order to solve the above problems, one aspect of the present invention provides a magnesia-iron spinel brick for a cement kiln, wherein the raw materials for preparing the brick include the following components in percentage by mass:
[0006] Magnesia 70%~95%, ferroaluminum spinel 4%~15%, iron powder 0.5%~5%, alumina powder 0.3%~5% and titanium carbide powder 0.2%~5%; external binder 1%~8%.
[0007] Preferably, the raw materials for its preparation include the following components in percentage by mass:
[0008] Magnesia 82%~91%, ferroaluminum spinel 7%~12%, iron powder 1%~2%, alumina powder 0.5%~3% and titanium carbide powder 0.5%~1.5%; external binder 1%~6%.
[0009] Preferably, the raw materials for its preparation include the following components in percentage by mass:
[0010] Magnesia 85.5%~88.5%, ferroaluminum spinel 8%~10%, iron powder 1%~2%, alumina powder 1%~2% and titanium carbide powder 0.5%~1%; external binder 2%~4%.
[0011] Preferably, the total mass percentage of iron powder and titanium carbide powder is 1.5% to 3%.
[0012] Preferably, the mass ratio of iron powder, alumina powder and titanium carbide powder is 1-3:1-4:1.
[0013] Preferably, the magnesia sand includes fused magnesia sand and high-purity magnesia sand; the mass ratio of the fused magnesia sand to the high-purity magnesia sand is 17~4:1.
[0014] Preferably, in the fused magnesia, MgO>96.3wt%, SiO2<1wt%, Fe2O3<0.8wt%, Al2O3<0.2wt%, CaO<1.5wt%, ignition loss<0.1wt%, and the bulk density of the fused magnesia>3.45g / cm 3 ;
[0015] In the high-purity magnesia, MgO>96.5wt%, SiO2<0.8wt%, Fe2O3<0.8wt%, Al2O3<0.15wt%, CaO<1.5wt%, and ignition loss<0.1wt%;
[0016] The iron-aluminum spinel has Al2O3>55wt%, Fe2O3>40wt%, SiO2<0.15wt%, CaO<1.5wt%, ignition loss<3.5wt%, and a volume density of the iron-aluminum spinel>3.9g / cm 3 .
[0017] Preferably, the fused magnesia includes fused magnesia particles with a particle size of >3mm and ≤5mm, fused magnesia particles with a particle size of >1mm and ≤3mm, fused magnesia particles with a particle size of >0mm and ≤1mm, and fused magnesia fine powder with a particle size of 200 mesh; the mass ratio of the fused magnesia particles with a particle size of >3mm and ≤5mm, the fused magnesia particles with a particle size of >1mm and ≤3mm, the fused magnesia particles with a particle size of >0mm and ≤1mm, and the fused magnesia fine powder with a particle size of 200 mesh is 1:2~4:0.8~2:2~3;
[0018] The high-purity magnesia comprises high-purity magnesia particles with a particle size of >3mm and ≤5mm, high-purity magnesia particles with a particle size of >1mm and ≤3mm, high-purity magnesia particles with a particle size of >0mm and ≤1mm, and high-purity magnesia fine powder with a particle size of 200 mesh; the mass ratio of the high-purity magnesia particles with a particle size of >3mm and ≤5mm, the high-purity magnesia particles with a particle size of >1mm and ≤3mm, the high-purity magnesia particles with a particle size of >0mm and ≤1mm, and the high-purity magnesia fine powder with a particle size of 200 mesh is 1-2:1-2:1:1;
[0019] The particle size of the iron-aluminum spinel is >0 mm and ≤1 mm;
[0020] The particle size of the iron powder is 200 meshes.
[0021] Preferably, the binder is a pulp solution.
[0022] Another aspect of the present invention provides a method for preparing the above-mentioned magnesia-iron spinel brick for cement kiln, comprising:
[0023] The raw materials for preparing the magnesia-iron spinel brick for cement kiln are mixed, then molded, and then the molded product is fired to obtain the magnesia-iron spinel brick for cement kiln.
[0024] Preferably, the sintering temperature is 1500-1530° C., and the sintering time is 2-10 hours.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The magnesia-iron spinel bricks for cement kilns of the present invention are prepared by adding iron powder to the raw materials. The iron powder can be oxidized before the divalent iron in the ferroaluminum spinel, thereby preventing the divalent ferrous oxide in the ferroaluminum spinel from being converted into trivalent iron. However, due to the low melting point of the iron powder, the unoxidized iron powder will form a liquid phase at the working temperature of the magnesia-iron spinel bricks, which reduces the high-temperature strength of the material. Therefore, the present invention further adds alumina micropowder, which can promote sintering and has good bonding force, thereby improving the high-temperature strength of the magnesia-iron spinel bricks; titanium carbide powder is also added, which can also be oxidized before the divalent iron, thereby preventing the divalent iron from being converted into trivalent iron. The addition of titanium carbide can reduce the amount of iron powder added, but its reducibility is weaker than that of iron powder. More importantly, unoxidized iron powder, alumina powder and titanium carbide powder can react at high temperature to generate a viscous liquid phase TAF20 metal ceramic phase. On the one hand, since the liquid diffusion rate is faster than the spatial diffusion, the viscous liquid phase TAF20 metal ceramic phase is dispersed in the spinel brick, which can promote the formation of the magnesia-iron spinel phase; on the other hand, the viscous liquid phase TAF20 metal ceramic phase is dispersed in the spinel brick, which can better bond and dissolve the magnesia-iron spinel phase, so that it can be better combined together to improve the strength of the brick. After firing, the TAF20 metal ceramic phase itself has good high-temperature strength properties. The high-strength phase is dispersed in the magnesia-iron spinel phase, which can improve the toughness of the magnesia-iron spinel brick; on the third hand, since the remaining iron powder generates the TAF20 metal ceramic phase, it prevents the iron powder from melting into liquid iron at high temperature, thereby avoiding its influence on the high-temperature strength of the magnesia-iron spinel brick. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] One aspect of an embodiment of the present invention provides a magnesia-iron spinel brick for a cement kiln, wherein the raw materials for preparing the brick include the following components in percentage by mass:
[0029] Magnesia 70%~95%, ferroaluminum spinel 4%~15%, iron powder 0.5%~5%, alumina powder 0.3%~5% and titanium carbide powder 0.2%~5%; external binder 1%~8%.
[0030] During the high-temperature firing process, the divalent ferrous oxide in the ferroaluminum spinel in the magnesia-iron spinel brick body will be converted into trivalent iron at high temperature, which will reduce the kiln skin performance and toughness of the brick body. In the magnesia-iron spinel brick for cement kiln of the embodiment of the present invention, iron powder is added to the raw materials for preparation. The iron powder can be oxidized before the divalent iron in the ferroaluminum spinel, thereby preventing the divalent ferrous oxide in the ferroaluminum spinel from being converted into trivalent iron. However, due to the low melting point of iron powder, the unoxidized iron powder will form a liquid phase at the working temperature of the magnesia-iron spinel brick, which will reduce the high-temperature strength of the material. Therefore, the present invention further adds alumina powder, which can promote sintering and has good bonding force, thereby improving the high-temperature strength of the magnesia-iron spinel brick; titanium carbide powder is also added, which can also be oxidized before the divalent iron, thereby preventing the divalent iron from being converted into trivalent iron. The addition of titanium carbide can reduce the amount of iron powder added, but its reducibility is weaker than that of iron powder. More importantly, unoxidized iron powder, alumina powder and titanium carbide powder can react at high temperature to generate a viscous liquid phase TAF20 metal ceramic phase. On the one hand, since the liquid diffusion rate is faster than the spatial diffusion, the viscous liquid phase TAF20 metal ceramic phase is dispersed in the spinel brick, which can promote the formation of the magnesia-iron spinel phase; on the other hand, the viscous liquid phase TAF20 metal ceramic phase is dispersed in the spinel brick, which can better bond and dissolve the magnesia-iron spinel phase, so that it can be better combined together to improve the strength of the brick. After firing, the TAF20 metal ceramic phase itself has good high-temperature strength properties. The high-strength phase is dispersed in the magnesia-iron spinel phase, which can improve the toughness of the magnesia-iron spinel brick; on the third hand, since the remaining iron powder generates the TAF20 metal ceramic phase, it prevents the iron powder from melting into liquid iron at high temperature, thereby avoiding its influence on the high-temperature strength of the magnesia-iron spinel brick.
[0031] In some embodiments, the raw materials for preparing magnesia-iron spinel bricks for cement kilns include the following components in percentage by mass:
[0032] Magnesia sand 82%~91%, ferroaluminum spinel 7%~12%, iron powder 1%~2%, alumina powder 0.5%~3% and titanium carbide powder 0.5%~1.5%; additional binder 1%~6%. Within the above mass percentage range, the comprehensive performance of the magnesia-iron spinel brick can be better.
[0033] Further preferably, the raw materials for preparing magnesia-iron spinel bricks for cement kiln include the following components in percentage by mass:
[0034] Magnesia 85.5%~88.5%, ferroaluminum spinel 8%~10%, iron powder 1%~2%, alumina powder 1%~2% and titanium carbide powder 0.5%~1%; external binder 2%~4%.
[0035] Since the addition of iron powder and titanium carbide powder can prevent the oxidation of divalent iron in ferroaluminum spinel to trivalent iron, titanium carbide powder will not melt at high temperature to affect the strength performance of magnesia-iron spinel bricks, but the anti-oxidation performance of titanium carbide powder is not as good as that of iron powder. Therefore, the addition of titanium carbide powder can reduce the amount of iron powder added, but in order to ensure the effect of preventing the oxidation of divalent iron to trivalent iron, in some embodiments, the total mass percentage of iron powder and titanium carbide powder is 1.5% to 3%. Under this total mass percentage, the strength performance of the magnesia-iron spinel brick is better, and as the lining material of the cement kiln, the kiln skin performance and toughness are also better.
[0036] Iron powder, alumina powder and titanium carbide powder react at high temperature to generate TAF20 metal ceramic phase, and the three need to be in an appropriate proportion to generate an appropriate amount of TAF20 metal ceramic phase. If the amount of TAF20 metal ceramic phase is too small, the strength of the magnesia-iron spinel brick will not be sufficient. If the amount of TAF20 metal ceramic phase is too much, the liquid phase will be generated too much during high-temperature use, which will reduce the high-temperature performance and make it easy to peel off during use. On the other hand, the ratio of the three is best to make the remaining iron powder consumed by the reaction, while not affecting the consumption of iron powder as a reducing agent. After comprehensive consideration, experimental attempts have found that the mass ratio of iron powder, alumina powder and titanium carbide powder is 1~3:1~4:1, which can make the strength performance of magnesia-iron spinel bricks better. At the same time, as the lining material of cement kilns, the kiln skin performance and toughness are also better.
[0037] In some embodiments, the magnesia includes fused magnesia and high-purity magnesia. The porosity, bulk density and other properties of fused magnesia and high-purity magnesia are quite different. If the bulk density is too high, the thermal shock resistance of the material is poor and cracks and peeling are easy to occur. If the bulk density is too low, it is not resistant to corrosion. The use of two kinds of magnesia and adjusting the ratio of the two can make the bulk density, porosity and other properties of the material more suitable, and the material has good thermal shock stability and corrosion resistance. Preferably, the mass ratio of the fused magnesia to the high-purity magnesia is 17~4:1.
[0038] In some embodiments, in the fused magnesia, MgO>96.3wt%, SiO2<1wt%, Fe2O3<0.8wt%, Al2O3<0.2wt%, CaO<1.5wt%, ignition loss<0.1wt%, and the bulk density of the fused magnesia>3.45g / cm 3 .
[0039] In some embodiments, in the high-purity magnesia, MgO>96.5wt%, SiO2<0.8wt%, Fe2O3<0.8wt%, Al2O3<0.15wt%, CaO<1.5wt%, and loss on ignition<0.1wt%.
[0040] In some embodiments, the iron-aluminum spinel has Al2O3>55wt%, Fe2O3>40wt%, SiO2<0.15wt%, CaO<1.5wt%, ignition loss<3.5wt%, and a bulk density of the iron-aluminum spinel>3.9g / cm 3 .
[0041] In some embodiments, the fused magnesia includes fused magnesia particles with a particle size of >3mm and ≤5mm, fused magnesia particles with a particle size of >1mm and ≤3mm, fused magnesia particles with a particle size of >0mm and ≤1mm, and fused magnesia fine powder with a particle size of 200 mesh; the mass ratio of the fused magnesia particles with a particle size of >3mm and ≤5mm, the fused magnesia particles with a particle size of >1mm and ≤3mm, the fused magnesia particles with a particle size of >0mm and ≤1mm, and the fused magnesia fine powder with a particle size of 200 mesh is 1:2~4:0.8~2:2~3.
[0042] In some embodiments, the high-purity magnesia includes high-purity magnesia particles with a particle size of >3mm and ≤5mm, high-purity magnesia particles with a particle size of >1mm and ≤3mm, high-purity magnesia particles with a particle size of >0mm and ≤1mm, and high-purity magnesia fine powder with a particle size of 200 mesh; the mass ratio of high-purity magnesia particles with a particle size of >3mm and ≤5mm, high-purity magnesia particles with a particle size of >1mm and ≤3mm, high-purity magnesia particles with a particle size of >0mm and ≤1mm, and high-purity magnesia fine powder with a particle size of 200 mesh is 1~2:1~2:1:1.
[0043] In some embodiments, the particle size of the ferroaluminum spinel is >0 mm and ≤1 mm.
[0044] In some embodiments, the iron powder has a particle size of 200 mesh.
[0045] Preferably, the binder is a pulp solution.
[0046] Another aspect of the embodiments of the present invention provides a method for preparing the above-mentioned magnesia-iron spinel brick for cement kiln, comprising:
[0047] The raw materials for preparing the magnesia-iron spinel brick for cement kiln are mixed, then molded, and then the molded product is fired to obtain the magnesia-iron spinel brick for cement kiln.
[0048] Preferably, the sintering temperature is 1500-1530° C., and the sintering time is 2-10 hours.
[0049] In the following embodiments, in the fused magnesia, MgO>96.3wt%, SiO2<1wt%, Fe2O3<0.8wt%, Al2O3<0.2wt%, CaO<1.5wt%, loss on ignition<0.1wt%, and the bulk density of the fused magnesia>3.45g / cm3 In high-purity magnesia, MgO>96.5wt%, SiO2<0.8wt%, Fe2O3<0.8wt%, Al2O3<0.15wt%, CaO<1.5wt%, and loss on ignition<0.1wt%. In ferroaluminum spinel, Al2O3>55wt%, Fe2O3>40wt%, SiO2<0.15wt%, CaO<1.5wt%, and loss on ignition<3.5wt%, and the volume density of ferroaluminum spinel>3.9g / cm 3 . Example 1
[0050] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0051] 15% of fused magnesia particles with a particle size of >3mm and ≤5mm, 31% of fused magnesia particles with a particle size of >1mm and ≤3mm, 18% of fused magnesia particles with a particle size of >0mm and ≤1mm, 27% of fused magnesia fine powder with a particle size of 200 mesh, 7% of ferroaluminum spinel with a particle size of >0mm and ≤1mm, 1% of iron powder of 200 mesh, 0.5% of alumina powder, and 0.5% of titanium carbide powder; 3% of external binder pulp solution. Example 2
[0052] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0053] 10% fused magnesia particles with a particle size of >3mm and ≤5mm, 31% fused magnesia particles with a particle size of >1mm and ≤3mm, 16% fused magnesia particles with a particle size of >0mm and ≤1mm, 26.5% fused magnesia fine powder with a particle size of 200 mesh, 2% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 1% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 1% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 1% high-purity magnesia fine powder with a particle size of 200 mesh, 8% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 1% iron powder of 200 mesh, 2% alumina powder, and 0.5% titanium carbide powder; 3% external binder pulp solution. Example 3
[0054] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0055] 10% fused magnesia particles with a particle size of >3mm and ≤5mm, 26% fused magnesia particles with a particle size of >1mm and ≤3mm, 15% fused magnesia particles with a particle size of >0mm and ≤1mm, 26% fused magnesia fine powder with a particle size of 200 mesh, 3% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 3% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 2% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 2% high-purity magnesia fine powder with a particle size of 200 mesh, 9% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 2% iron powder of 200 mesh, 1% alumina powder, 1% titanium carbide powder; 3% external binder pulp solution. Example 4
[0056] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0057] 10% fused magnesia particles with a particle size of >3mm and ≤5mm, 26% fused magnesia particles with a particle size of >1mm and ≤3mm, 9% fused magnesia particles with a particle size of >0mm and ≤1mm, 25.5% fused magnesia fine powder with a particle size of 200 mesh, 4% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 4% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 4% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 3% high-purity magnesia fine powder with a particle size of 200 mesh, 10% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 2% iron powder of 200 mesh, 1.5% alumina powder, 1% titanium carbide powder; 3% external binder pulp solution. Example 5
[0058] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0059] 10% fused magnesia particles with a particle size of >3mm and ≤5mm, 21% fused magnesia particles with a particle size of >1mm and ≤3mm, 11% fused magnesia particles with a particle size of >0mm and ≤1mm, 20% fused magnesia fine powder with a particle size of 200 mesh, 5% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 5% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 5% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 5% high-purity magnesia fine powder with a particle size of 200 mesh, 12% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 2% iron powder of 200 mesh, 3% alumina powder, 1% titanium carbide powder; 3% external binder pulp solution. Example 6
[0060] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0061] 5% fused magnesia particles with a particle size of >3mm and ≤5mm, 21% fused magnesia particles with a particle size of >1mm and ≤3mm, 11% fused magnesia particles with a particle size of >0mm and ≤1mm, 20% fused magnesia fine powder with a particle size of 200 mesh, 10% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 5% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 5% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 5% high-purity magnesia fine powder with a particle size of 200 mesh, 12% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 1.5% iron powder of 200 mesh, 3% alumina powder, 1.5% titanium carbide powder; 3% external binder pulp solution. Example 7
[0062] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0063] 8% fused magnesia particles with a particle size of >3mm and ≤5mm, 21% fused magnesia particles with a particle size of >1mm and ≤3mm, 5% fused magnesia particles with a particle size of >0mm and ≤1mm, 19.5% fused magnesia fine powder with a particle size of 200 mesh, 10% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 10% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 5% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 5% high-purity magnesia fine powder with a particle size of 200 mesh, 12% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 1.5% iron powder of 200 mesh, 1.5% alumina powder, 1.5% titanium carbide powder; 3% external binder pulp solution. Example 8
[0064] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0065] 5% fused magnesia particles with a particle size of >3mm and ≤5mm, 20% fused magnesia particles with a particle size of >1mm and ≤3mm, 5% fused magnesia particles with a particle size of >0mm and ≤1mm, 20% fused magnesia fine powder with a particle size of 200 mesh, 5% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 5% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 5% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 5% high-purity magnesia fine powder with a particle size of 200 mesh, 15% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 5% iron powder of 200 mesh, 5% alumina powder, 5% titanium carbide powder; 3% external binder pulp solution. Example 9
[0066] The raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment include the following components in percentage by mass:
[0067] 10% fused magnesia particles with a particle size of >3mm and ≤5mm, 20% fused magnesia particles with a particle size of >1mm and ≤3mm, 15% fused magnesia particles with a particle size of >0mm and ≤1mm, 25% fused magnesia fine powder with a particle size of 200 mesh, 10% high-purity magnesia particles with a particle size of >3mm and ≤5mm, 5% high-purity magnesia particles with a particle size of >1mm and ≤3mm, 5% high-purity magnesia particles with a particle size of >0mm and ≤1mm, 5% high-purity magnesia fine powder with a particle size of 200 mesh, 4% ferroaluminum spinel with a particle size of >0mm and ≤1mm, 0.5% iron powder of 200 mesh, 0.3% alumina powder, 0.2% titanium carbide powder; 3% external binder pulp solution. Example 10
[0068] The remaining components and proportions of the raw materials for preparing the magnesia-iron spinel bricks for cement kiln in this embodiment are the same as those in Example 2, with the following differences: 1.2% 200-mesh iron powder, 1.2% alumina powder, and 1.1% titanium carbide powder; that is, the mass ratio of iron powder, alumina powder, and titanium carbide powder is approximately 1:1:1; and the total mass proportion of iron powder and titanium carbide powder is 2.3%. Embodiment 11
[0069] The remaining components and proportions of the raw materials for preparing the magnesia-iron spinel bricks for cement kiln in this embodiment are the same as those in Example 2, except that: 1.25% of 200-mesh iron powder, 1.8% of alumina powder, and 0.45% of titanium carbide powder; that is, the mass ratio of iron powder, alumina powder, and titanium carbide powder is 2.8:4:1; and the total mass proportion of iron powder and titanium carbide powder is 1.7%. Example 12
[0070] The remaining components and proportions of the raw materials for preparing the magnesia-iron spinel bricks for cement kiln in this embodiment are the same as those in Example 2, except that: 0.8% of 200-mesh iron powder, 0.7% of alumina powder, and 2% of titanium carbide powder; that is, the mass ratio of iron powder, alumina powder, and titanium carbide powder is 0.4:0.35:1; and the total mass proportion of iron powder and titanium carbide powder is 2.8%. Example 13
[0071] The remaining components and proportions of the raw materials for preparing the magnesia-iron spinel bricks for cement kiln of this embodiment are the same as those of Example 2, except that: 1.4% of 200-mesh iron powder, 1.75% of alumina powder, and 0.35% of titanium carbide powder; that is, the mass ratio of iron powder, alumina powder, and titanium carbide powder is about 4:5:1; and the total mass proportion of iron powder and titanium carbide powder is 1.75%. Embodiment 14
[0072] The remaining components and proportions of the raw materials for preparing the magnesia-iron spinel bricks for cement kiln in this embodiment are the same as those in Example 2, except that: 200-mesh iron powder 2.1%, alumina powder 0.2%, titanium carbide powder 1.2%; that is, the mass ratio of iron powder, alumina powder, and titanium carbide powder is approximately 1.75:0.17:1; the total mass proportion of iron powder and titanium carbide powder is 3.3%. Embodiment 15
[0073] The remaining components and proportions of the raw materials for preparing the magnesia-iron spinel bricks for cement kiln in this embodiment are the same as those in Example 2, except that: 0.6% 200-mesh iron powder, 2.3% alumina powder, and 0.6% titanium carbide powder; that is, the mass ratio of iron powder, alumina powder, and titanium carbide powder is about 1:4:1; and the total mass proportion of iron powder and titanium carbide powder is 1.2%. Example 16
[0074] The remaining components and the number of parts of the raw materials for preparing the magnesia-iron spinel brick for cement kiln in this embodiment are the same as those in Example 2, except that the ratio of fused magnesia to high-purity magnesia is different. In this embodiment, 10% of fused magnesia particles with a particle size of >3mm and ≤5mm, 21% of fused magnesia particles with a particle size of >1mm and ≤3mm, 16% of fused magnesia particles with a particle size of >0mm and ≤1mm, 24% of fused magnesia fine powder with a particle size of 200 mesh, 5% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 4.5% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 4% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, and 4% of high-purity magnesia fine powder with a particle size of 200 mesh are included. The mass ratio of fused magnesia to high-purity magnesia is 4:1. Embodiment 17
[0075] The remaining components and the number of parts of the raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment are the same as those of Example 2, except that the ratio of fused magnesia to high-purity magnesia is different. In this embodiment, 8% of fused magnesia particles with a particle size of >3mm and ≤5mm, 16% of fused magnesia particles with a particle size of >1mm and ≤3mm, 16% of fused magnesia particles with a particle size of >0mm and ≤1mm, 19% of fused magnesia fine powder with a particle size of 200 mesh, 9% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 8.5% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 6% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, and 6% of high-purity magnesia fine powder with a particle size of 200 mesh are included. The mass ratio of fused magnesia to high-purity magnesia is 2:1. Embodiment 18
[0076] The remaining components and the number of parts of the raw materials for preparing the magnesia-iron spinel brick for cement kiln of this embodiment are the same as those of Example 2, except that the ratio of fused magnesia to high-purity magnesia is different. In this embodiment, 12% of fused magnesia particles with a particle size of >3mm and ≤5mm, 24% of fused magnesia particles with a particle size of >1mm and ≤3mm, 24% of fused magnesia particles with a particle size of >0mm and ≤1mm, 24% of fused magnesia fine powder with a particle size of 200 mesh, 1.5% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 1% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 1% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, and 1% of high-purity magnesia fine powder with a particle size of 200 mesh are included. The mass ratio of fused magnesia to high-purity magnesia is 18.5:1.
[0077] Comparative Example 1
[0078] The magnesia-iron spinel brick for cement kiln in this comparative example does not contain iron powder, alumina powder and titanium carbide powder in its preparation raw materials, and its preparation raw materials include the following components in mass percentage:
[0079] 12% of fused magnesia particles with a particle size of >3mm and ≤5mm, 31% of fused magnesia particles with a particle size of >1mm and ≤3mm, 16% of fused magnesia particles with a particle size of >0mm and ≤1mm, 26.5% of fused magnesia fine powder with a particle size of 200 mesh, 2.5% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 2% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 1% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 1% of high-purity magnesia fine powder with a particle size of 200 mesh, 8% of iron-aluminum spinel with a particle size of >0mm and ≤1mm; 3% of external binder pulp solution.
[0080] Comparative Example 2
[0081] The ferromagnesia spinel brick for cement kiln in this comparative example has iron powder added to its raw materials for preparation, but no alumina powder or titanium carbide powder is added, and its raw materials for preparation include the following components in mass percentage:
[0082] 12% of fused magnesia particles with a particle size of >3mm and ≤5mm, 31% of fused magnesia particles with a particle size of >1mm and ≤3mm, 16% of fused magnesia particles with a particle size of >0mm and ≤1mm, 26.5% of fused magnesia fine powder with a particle size of 200 mesh, 2.5% of high-purity magnesia particles with a particle size of >3mm and ≤5mm, 1% of high-purity magnesia particles with a particle size of >1mm and ≤3mm, 1% of high-purity magnesia particles with a particle size of >0mm and ≤1mm, 1% of high-purity magnesia fine powder with a particle size of 200 mesh, 8% of iron-aluminum spinel with a particle size of >0mm and ≤1mm, and 1% of iron powder of 200 mesh; 3% of external binder pulp solution.
[0083] The raw materials for preparing the ferromagnesian spinel bricks for cement kilns in the above embodiments and comparative examples, except for the pulp, are configured into a mixture, stirred for 5 minutes, and then stirred for 25 minutes after adding the pulp, and formed by a 1200-ton electric screw press, with a molding size of 230mm×114mm×75mm, dried in a drying kiln for 24 hours, and then fired in a firing kiln, with a firing temperature of 1500℃, a cart speed of 120 minutes per cart, and a 6-hour heat preservation in the firing section to obtain ferromagnesian spinel brick samples, and each sample is tested, and the test sample preparation is carried out according to GB / T7321. The test results are shown in Table 1 below.
[0084] Kiln lining performance: Cement raw materials are sandwiched between two refractory brick samples, and heated in an electric furnace at 1500℃*3h. After cooling, three-point bending test is performed. (Sample shape: 62.5mm*25mm*25mm, cement raw materials: 95% ordinary silicate rock + 3% potassium sulfate + 2% potassium chloride). The test results are shown in Table 2 below.
[0085] It can be seen from the data in Table 1 below that iron powder is not added to the raw materials of the ferromagnesian spinel bricks of Comparative Example 1, and as the lining material of the cement kiln, the kiln skin performance is poor and the toughness is poor; iron powder is added to the raw materials of the ferromagnesian spinel bricks of Comparative Example 2, but alumina powder and titanium carbide powder are not added. Although the kiln skin performance is good, the high temperature strength performance of the ferromagnesian spinel bricks is significantly reduced due to the melting of the remaining iron powder to produce a liquid phase. In contrast, the ferromagnesian spinel bricks of each embodiment of the present invention have good kiln skin performance and high temperature strength performance.
[0086] In each embodiment of the present invention, in Embodiment 1-9, the mass percentage of each component of the raw material is different, among which, compared with Embodiments 8 and 9, the mass percentage of each component in Embodiment 1-7 is in a preferred range, and the kiln lining performance and high-temperature strength performance of the magnesia-iron spinel brick are better. Furthermore, compared with Embodiments 1 and 5-7, the kiln lining performance and high-temperature strength performance of Embodiment 2-4 are better, and the mass percentage of each component is in a further preferred range.
[0087] Compared with Example 2, Examples 10-15 differ in that the content of added iron powder, alumina powder and titanium carbide powder is different. Among them, the mass ratio of iron powder, alumina powder and titanium carbide powder, and the total content of iron powder and titanium carbide in Examples 2, 10 and 11 are more optimal, and the obtained magnesia-iron spinel bricks have significantly better kiln lining performance and high-temperature strength performance. In Examples 12 and 13, the mass ratio of iron powder, alumina powder and titanium carbide powder is not within the preferred range, and its kiln lining performance and high-temperature strength performance are not as good as Examples 2, 10 and 11; In Examples 14 and 15, the mass ratio of iron powder, alumina powder and titanium carbide powder is not within the preferred range, and the total content of iron powder and titanium carbide is not within the preferred range, and its kiln lining performance and high-temperature strength performance are not as good as Examples 2, 10-13.
[0088] Compared with Example 2, Examples 16-18 differ in that the mass ratio of fused magnesia to high-purity magnesia is different. Among them, the mass ratio of fused magnesia to high-purity magnesia in Examples 2 and 16 is more optimal, and the obtained magnesia-iron spinel bricks have significantly better kiln skin performance and high-temperature strength performance.
[0089] Table 1
[0090] <![CDATA[Bulk density after firing / g / cm 3 > Porosity after firing / % Compressive strength after burning / MPa Example 1 2.97 15 76 Example 2 2.98 14 89 Example 3 2.98 14 87 Example 4 2.97 14 86 Example 5 2.97 15 73 Example 6 2.97 15 75 Example 7 2.96 15 74 Example 8 2.96 16 65 Example 9 2.96 16 62 Example 10 2.98 14 85 Embodiment 11 2.98 14 83 Example 12 2.97 15 78 Example 13 2.97 15 75 Embodiment 14 2.96 16 69 Embodiment 15 2.96 16 68 Example 16 2.98 14 85 Embodiment 17 2.97 15 73 Embodiment 18 2.97 15 75 Comparative Example 1 2.98 14 83 Comparative Example 2 2.95 16 49
[0091] Table 2
[0092] Flexural strength / Mpa Example 1 1.2 Example 2 1.5 Example 3 1.5 Example 4 1.5 Example 5 1.3 Example 6 1.4 Example 7 1.2 Example 8 1.1 Example 9 1.1 Example 10 1.4 Embodiment 11 1.4 Example 12 1.1 Example 13 1.2 Embodiment 14 1 Embodiment 15 1 Example 16 1.3 Embodiment 17 1.1 Embodiment 18 1 Comparative Example 1 0.6 Comparative Example 2 1.2
[0093] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A magnesia-iron spinel brick for cement kiln, characterized in that: The raw materials for its preparation include the following components in percentage by mass: 82% to 91% magnesia, 7% to 12% ferroaluminum spinel, 1% to 2% iron powder, 0.5% to 3% alumina powder and 0.5% to 1.5% titanium carbide powder; 1% to 6% external binder; the total mass percentage of iron powder and titanium carbide powder is 1.5% to 3%; the mass ratio of iron powder, alumina powder and titanium carbide powder is 1 to 3:1 to 4:1; the magnesia includes fused magnesia and high-purity magnesia; the mass ratio of the fused magnesia to the high-purity magnesia is 17 to 4:
1.
2. The magnesia-iron spinel brick for cement kiln according to claim 1, characterized in that: The raw materials for its preparation include the following components in percentage by mass: Magnesia 85.5%~88.5%, ferroaluminum spinel 8%~10%, iron powder 1%~2%, alumina powder 1%~2% and titanium carbide powder 0.5%~1%; external binder 2%~4%.
3. The magnesia-iron spinel brick for cement kiln according to claim 1, characterized in that: In the fused magnesia, MgO>96.3wt%, SiO2<1wt%, Fe2O3<0.8wt%, Al2O3<0.2wt%, CaO<1.5wt%, ignition loss<0.1wt%, and the bulk density of the fused magnesia>3.45g / cm 3 ; In the high-purity magnesia, MgO>96.5wt%, SiO2<0.8wt%, Fe2O3<0.8wt%, Al2O3<0.15wt%, CaO<1.5wt%, and ignition loss<0.1wt%; The iron-aluminum spinel has Al2O3>55wt%, Fe2O3>40wt%, SiO2<0.15wt%, CaO<1.5wt%, ignition loss<3.5wt%, and a volume density of the iron-aluminum spinel>3.9g / cm 3 .
4. The ferromagnesian spinel brick for cement kiln according to claim 1, characterized in that: The fused magnesia includes fused magnesia particles with a particle size of more than 3 mm and less than 5 mm, fused magnesia particles with a particle size of more than 1 mm and less than 3 mm, fused magnesia particles with a particle size of more than 0 mm and less than 1 mm, and fused magnesia fine powder with a particle size of 200 meshes; the mass ratio of the fused magnesia particles with a particle size of more than 3 mm and less than 5 mm, the fused magnesia particles with a particle size of more than 1 mm and less than 3 mm, the fused magnesia particles with a particle size of more than 0 mm and less than 1 mm, and the fused magnesia fine powder with a particle size of 200 meshes is 1:2~4:0.8~2:2~3; The high-purity magnesia comprises high-purity magnesia particles with a particle size of >3mm and ≤5mm, high-purity magnesia particles with a particle size of >1mm and ≤3mm, high-purity magnesia particles with a particle size of >0mm and ≤1mm, and high-purity magnesia fine powder with a particle size of 200 mesh; the mass ratio of the high-purity magnesia particles with a particle size of >3mm and ≤5mm, the high-purity magnesia particles with a particle size of >1mm and ≤3mm, the high-purity magnesia particles with a particle size of >0mm and ≤1mm, and the high-purity magnesia fine powder with a particle size of 200 mesh is 1-2:1-2:1:1; The particle size of the iron-aluminum spinel is >0 mm and ≤1 mm; The particle size of the iron powder is 200 meshes.
5. A method for preparing magnesia-iron spinel bricks for cement kiln according to any one of claims 1 to 4, characterized in that: include: The raw materials for preparing the magnesia-iron spinel brick for cement kiln are mixed, then molded, and then the molded product is fired to obtain the magnesia-iron spinel brick for cement kiln.
6. The preparation method according to claim 5, characterized in that: The sintering temperature is 1500-1530° C. and the sintering time is 2-10 hours.