A hydrophilic self-cleaning antique brick based on phase separation self-cleaning and preparation method thereof

By forming a hydrophilic self-cleaning glaze layer with a specific phase separation structure on antique bricks, the problems of poor aging resistance and insufficient binding strength of hydrophilic self-cleaning coatings in the prior art are solved, and the durable self-cleaning of antique bricks are achieved and the long-lasting self-cleaning and Cost reduction.

CN118754723BActive Publication Date: 2024-11-19FOSHAN DONGPENG CERAMIC +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411251753.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-19
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The hydrophilic self-cleaning coatings of existing antique bricks have poor aging resistance and limited binding force with the brick surface, resulting in poor self-cleaning aging, difficult to meet actual use needs, and increase production costs.

Method used

The preparation method of hydrophilic self-cleaning antique bricks based on phase separation self-cleaning is adopted. After forming a bottom glaze layer on the surface of the ceramic body, the hydrophilic self-cleaning glaze of a specific formula is calcined to form boron oxide and lithium oxide as the component. The upper layer is a hydrophilic self-cleaning glaze layer with calcium oxide, magnesium oxide, alumina and silica as the lower layer of the phase separation layer to improve aging resistance and binding strength.

Benefits of technology

It achieves excellent, uniform and long-lasting self-cleaning performance of antique bricks, reduces production costs, and improves the aging resistance of the hydrophilic self-cleaning glaze layer and its binding force with the brick surface, extending the self-cleaning aging efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of building ceramics, and in particular to a hydrophilic self-cleaning antique brick based on phase separation self-cleaning and a preparation method thereof, comprising the following steps: A. preparing a ceramic body, pressing the ceramic body, and obtaining a body having a concave-convex effect on the surface after drying; B. applying a bottom glaze on the surface of the body to form a bottom glaze layer; C. preparing a hydrophilic self-cleaning glaze; D. applying the hydrophilic self-cleaning glaze on the surface of the bottom glaze layer to form a hydrophilic self-cleaning glaze layer; E. after drying, calcining at a temperature of 1200-1220° C. to obtain a hydrophilic self-cleaning antique brick. The preparation method of the hydrophilic self-cleaning antique brick based on phase separation self-cleaning proposed by the present invention is simple in preparation method and strong in operability. The obtained hydrophilic self-cleaning antique brick not only has excellent, uniform and lasting self-cleaning property while ensuring the appearance, but also helps to reduce the cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building ceramics, in particular to a hydrophilic self-cleaning antique brick based on phase separation self-cleaning and a preparation method thereof. Background Art

[0002] Antique tiles, as an artistic building material that combines classical aesthetics with modern craftsmanship, are deeply favored by consumers for their unique antique glaze effect, rich color layers and strong historical charm. They are widely used in home decoration, commercial places, cultural and tourist attractions and other fields.

[0003] In order to ensure the antique effect of antique tiles, the surface of antique tiles is usually designed to be uneven. Although the uneven surface is conducive to increasing its anti-slip performance, it is also easy to become a breeding ground for dirt and grime, which not only affects the aesthetics of the antique tiles and reduces its decorative effect, but also makes the treatment of dirt on antique tiles time-consuming and laborious, and requires the help of cleaning agents to be effectively removed.

[0004] In order to overcome the above-mentioned defects, the prior art usually coats the surface of the antique brick with a hydrophilic self-cleaning coating, so that a layer of hydrophilic self-cleaning coating is formed on the surface of the antique brick, so that water can spread quickly when it contacts the coating surface (that is, the static contact angle between water and the coating is small) and form a uniform water film, which can penetrate into the interface between the dirt and the coating, thereby reducing the adhesion of the dirt, and under the action of gravity, the continuously flowing water film can take away and remove the dirt on the surface of the antique brick, achieving a self-cleaning effect. However, due to the poor aging resistance of the hydrophilic self-cleaning coating and its limited bonding force with the brick surface, the hydrophilic self-cleaning coating is easy to fall off, which is not conducive to extending the service life of the coating, resulting in poor self-cleaning durability of the coating, and it is difficult to meet actual use requirements. In addition, additionally coating the surface of the antique brick substrate with a hydrophilic self-cleaning coating is not conducive to reducing production costs. Summary of the invention

[0005] The first purpose of the present invention is to propose a preparation method of hydrophilic self-cleaning antique tiles based on phase separation self-cleaning. The preparation method is simple and easy to operate. The obtained hydrophilic self-cleaning antique tiles not only have excellent, uniform and lasting self-cleaning properties while ensuring the appearance, but also help to reduce costs.

[0006] The second purpose of the present invention is to propose a hydrophilic self-cleaning antique tile prepared by the above-mentioned preparation method of super hydrophilic self-cleaning antique tile based on phase separation self-cleaning, whose static contact angle before being soaked in boiling water is 8 to 15°, and the static contact angle after being soaked in boiling water for 30 days is 15 to 22°, and it has excellent, uniform and long-lasting self-cleaning performance.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] A method for preparing hydrophilic self-cleaning antique tiles based on phase separation self-cleaning comprises the following steps:

[0009] A. preparing a ceramic body, pressing the ceramic body, and obtaining a body having a concave-convex effect on the surface after drying;

[0010] B. Applying base glaze on the surface of the body to form a base glaze layer;

[0011] Calculated by mass percentage, the chemical composition of the base glaze includes SiO257-63%, Al2O323-25%, Na2O 2.5-3.5%, CaO 0.2-0.8%, K2O 6-7% and ZrO25.5-6.5%;

[0012] C. Prepare hydrophilic self-cleaning glaze;

[0013] Calculated by mass percentage, the hydrophilic self-cleaning glaze comprises 80-90% hydrophilic frit, 5-10% black ball clay and 5-10% fluorite;

[0014] Calculated by mass percentage, the hydrophilic frit includes 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% calcined talc, 10-20% kaolin, 13-22% quartz and 8-12% alumina, and the calcination curve of the hydrophilic frit is: from room temperature to 1530°C at a heating rate of 8-10°C / min, and then kept warm for 35-45min;

[0015] D. applying a hydrophilic self-cleaning glaze material to the surface of the base glaze layer to form a hydrophilic self-cleaning glaze layer;

[0016] E. After drying, calcining at a temperature of 1200-1220°C obtains hydrophilic self-cleaning antique tiles.

[0017] Furthermore, in step C, the mesh size of the fluorite is 6000-8000 mesh.

[0018] Furthermore, in step C, calculated as a percentage by mass, the content of CaF2 in the fluorite is ≥90%.

[0019] Furthermore, in step C, the ratio of the sum of the mass percentages of the boric acid and the lithium carbonate to the sum of the mass percentages of the wollastonite and the calcined talc is 1:(4-7).

[0020] Furthermore, in step C, the hydrophilic self-cleaning glaze is passed through a 325-mesh sieve, and the residue is 0.2-0.4% by mass.

[0021] Furthermore, in step C, the specific gravity of the hydrophilic self-cleaning glaze is 1.82 to 1.9.

[0022] Further, in step C, the hydrophilic self-cleaning glaze comprises 80% hydrophilic frit, 10% black ball clay and 10% fluorite, calculated by mass percentage;

[0023] Calculated by mass percentage, the hydrophilic frit includes 3% boric acid, 8% lithium carbonate, 35% wollastonite, 12% calcined talc, 15% kaolin, 17% quartz and 10% alumina.

[0024] Furthermore, in step D, the glazing thickness of the hydrophilic self-cleaning glaze is 0.3-0.7 mm.

[0025] Furthermore, in step C, the preparation steps of the hydrophilic self-cleaning glaze are:

[0026] The raw materials of the hydrophilic frit are uniformly mixed according to the proportion, and the hydrophilic frit is obtained by water quenching after calcination;

[0027] After the raw materials of the hydrophilic self-cleaning glaze are uniformly mixed according to the proportion, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and the hydrophilic self-cleaning glaze is obtained by sieving.

[0028] A hydrophilic self-cleaning antique tile based on phase separation self-cleaning is prepared using the above-mentioned preparation method of hydrophilic self-cleaning antique tile based on phase separation self-cleaning. The hydrophilic self-cleaning antique tile has a static contact angle of 8-15° before being soaked in boiling water, and a static contact angle of 15-22° after being soaked in boiling water for 30 days.

[0029] The technical solution provided by the present invention may include the following beneficial effects:

[0030] 1. In the early stage of firing, the hydrophilic frit formula system has achieved phase separation, and boric acid and lithium carbonate are the upper phase separation layer, and the second gradient fluxing system (wollastonite and calcined talc) and high-temperature raw materials (kaolin, quartz and alumina) are the lower phase separation layer. When the calcination temperature reaches the melting point of each raw material in the lower phase separation layer, each raw material in the lower phase separation layer will also gradually melt. Further, as the calcination temperature rises again, each raw material in the upper phase separation layer and the lower phase separation layer will gradually decompose, so that the hydrophilic frit will eventually form a phase separation melt with boron oxide and lithium oxide as the upper phase separation layer, and calcium oxide, magnesium oxide, aluminum oxide and silicon oxide as the lower phase separation layer. When the hydrophilic frit, which is essentially a phase separation melt, is added to the hydrophilic self-cleaning glaze formula, the hydrophilic self-cleaning glaze will form a hydrophilic self-cleaning glaze layer with boron oxide and lithium oxide as the upper phase separation layer, and calcium oxide, magnesium oxide, aluminum oxide and silicon dioxide as the lower phase separation layer after calcination.

[0031] 2. Since the surface tension of lithium oxide is 450×10 -3 N / M, the surface tension of boron oxide is 80×10 -3 N / M, while the surface tension of water is 73×10 -3N / m, that is, the surface tension of the hydrophilic self-cleaning glaze layer is much greater than the surface tension of water, so that the surface of the hydrophilic self-cleaning glaze layer has extremely strong hydrophilic self-cleaning performance, even if the surface of the hydrophilic self-cleaning glaze layer is adhered with dirt, the dirt is relatively easy to be removed. In addition, compared with the hydrophilic self-cleaning coating, the aging resistance of the hydrophilic self-cleaning glaze layer is greatly improved, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the poor aging resistance of the hydrophilic self-cleaning coating in the prior art. Further, since the hydrophilic self-cleaning glaze layer is directly calcined by the hydrophilic self-cleaning glaze, its bonding force with the antique brick is extremely high, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the limited bonding force between the hydrophilic self-cleaning coating and the brick surface of the antique brick in the prior art. The mutual coordination of the above multiple factors is conducive to realizing the long-lasting self-cleaning of the antique brick, and the self-cleaning is excellent. In addition, the technical solution does not need to additionally apply the hydrophilic self-cleaning coating on the surface of the antique brick, which is conducive to saving production costs and improving production efficiency.

[0032] 3. During the calcination of the hydrophilic self-cleaning glaze, as the calcination temperature increases, the melt viscosity gradually decreases, and the fluorite will sink together with the raw materials in the hydrophilic frit that are far from reaching the melting point (such as the second gradient fluxing system and high-temperature raw materials), so that the hydrophilic self-cleaning glaze is calcined to form a hydrophilic self-cleaning glaze layer with boron oxide and lithium oxide as the upper phase separation layer and calcium fluoride, calcium oxide, magnesium oxide, aluminum oxide and silicon dioxide as the lower phase separation layer. Among them, the surface tension of calcium fluoride is 22.3×10 -3 N / M, and the amount of fluorite whose main component is calcium fluoride added to the hydrophilic self-cleaning glaze is 5-10%, so that the content of calcium fluoride in the phase-separated lower layer of the hydrophilic self-cleaning glaze layer is relatively large, thereby greatly reducing the surface tension of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer, and making the surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the bottom glaze layer match, thereby avoiding the defect of glaze shrinkage phenomenon that the hydrophilic self-cleaning glaze is prone to appear during the calcination process when the surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the bottom glaze layer is extremely different, which is not only conducive to obtaining uniform self-cleaning properties, but also can ensure the appearance of the product. DETAILED DESCRIPTION

[0033] The present technical solution provides a method for preparing hydrophilic self-cleaning antique tiles based on phase separation self-cleaning, comprising the following steps:

[0034] A. preparing a ceramic body, pressing the ceramic body, and obtaining a body having a concave-convex effect on the surface after drying;

[0035] B. Applying base glaze on the surface of the body to form a base glaze layer;

[0036] Calculated by mass percentage, the chemical composition of the base glaze includes SiO257-63%, Al2O323-25%, Na2O 2.5-3.5%, CaO 0.2-0.8%, K2O 6-7% and ZrO25.5-6.5%;

[0037] C. Prepare hydrophilic self-cleaning glaze;

[0038] Calculated by mass percentage, the hydrophilic self-cleaning glaze comprises 80-90% hydrophilic frit, 5-10% black ball clay and 5-10% fluorite;

[0039] Calculated by mass percentage, the hydrophilic frit includes 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% calcined talc, 10-20% kaolin, 13-22% quartz and 8-12% alumina, and the calcination curve of the hydrophilic frit is: from room temperature to 1530°C at a heating rate of 8-10°C / min, and then kept warm for 35-45min;

[0040] D. applying a hydrophilic self-cleaning glaze material to the surface of the base glaze layer to form a hydrophilic self-cleaning glaze layer;

[0041] E. After drying, calcining at a temperature of 1200-1220°C obtains hydrophilic self-cleaning antique tiles.

[0042] The prior art usually coats the surface of the antique brick substrate with a hydrophilic self-cleaning coating, so that a layer of hydrophilic self-cleaning coating is formed on the surface of the antique brick, so that even if there is dirt on the surface of the antique brick, the dirt can be easily removed. However, due to the poor aging resistance of the hydrophilic self-cleaning coating and its limited bonding force with the brick surface, the hydrophilic self-cleaning coating is easy to fall off, which is not conducive to extending the service life of the coating, resulting in poor self-cleaning durability of the coating, and it is difficult to meet the actual use requirements. In addition, additionally coating the surface of the antique brick substrate with a hydrophilic self-cleaning coating is not conducive to reducing production costs.

[0043] First, in order to achieve long-lasting self-cleaning properties under the premise of reducing costs, the technical solution proposes a hydrophilic self-cleaning glaze, the raw materials of which include hydrophilic frit, black ball clay and fluorite. Among them, the hydrophilic frit uses boric acid, lithium carbonate, wollastonite and calcined talc as fluxes, and the melting point of boric acid is about 577°C, the melting point of lithium carbonate is about 723°C, the melting point of wollastonite is about 1500°C, and the melting point of calcined talc is about 1400°C, so that the hydrophilic frit formula forms a first gradient fluxing system composed of boric acid and lithium carbonate, and a second gradient fluxing system composed of wollastonite and calcined talc, and the melting temperatures of the two gradient fluxing systems are extremely different.

[0044] Since the melting temperatures of the first gradient fluxing system and the high-temperature raw materials in the hydrophilic frit formula (i.e., the raw materials that form the solid phase, such as kaolin, quartz and alumina, where the melting temperature of kaolin is about 1780°C, the melting temperature of quartz is about 1713°C, and the melting temperature of alumina is 2054°C) are quite different, the melting temperatures of the second gradient fluxing system and the high-temperature raw materials in the hydrophilic frit formula are relatively different, so that in the early stage of firing of the tile, the raw materials of the first gradient fluxing system melt first, so that the hydrophilic frit obtains a melt mainly composed of boric acid and lithium carbonate in the early stage of calcination. As the calcination temperature increases, the melt viscosity gradually decreases, and other raw materials that are far from reaching the melting point (such as the raw materials of the second gradient fluxing system and the high-temperature raw materials) will sink. That is, in the early stage of firing, the hydrophilic frit formula system has achieved phase separation, and boric acid and lithium carbonate are the upper layer of the phase separation, and the second gradient fluxing system (wollastonite and calcined talc) and the high-temperature raw materials (kaolin, quartz and alumina) are the lower layer of the phase separation. When the calcination temperature reaches the melting point of each raw material in the lower phase separation layer, each raw material in the lower phase separation layer will also gradually melt. Further, as the calcination temperature rises again, each raw material in the upper phase separation layer and the lower phase separation layer will gradually decompose, so that the hydrophilic melt will eventually form a phase separation melt with boron oxide and lithium oxide as the upper phase separation layer and calcium oxide, magnesium oxide, aluminum oxide and silicon oxide as the lower phase separation layer.

[0045] When the hydrophilic frit, which is essentially a phase-separated melt, is added to the hydrophilic self-cleaning glaze formula, the hydrophilic self-cleaning glaze will form, after calcination, a hydrophilic self-cleaning glaze layer with boron oxide and lithium oxide components as the phase-separated upper layer and calcium oxide, magnesium oxide, aluminum oxide and silicon dioxide components as the phase-separated lower layer.

[0046] Furthermore, since the surface tension of lithium oxide is 450×10 -3 N / M, the surface tension of boron oxide is 80×10 - 3 N / M, while the surface tension of water is 73×10 -3N / m, that is, the surface tension of the hydrophilic self-cleaning glaze layer is much greater than the surface tension of water, so that the surface of the hydrophilic self-cleaning glaze layer has extremely strong hydrophilic self-cleaning performance, even if the surface of the hydrophilic self-cleaning glaze layer is adhered with dirt, the dirt is relatively easy to be removed. In addition, compared with the hydrophilic self-cleaning coating, the aging resistance of the hydrophilic self-cleaning glaze layer is greatly improved, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the poor aging resistance of the hydrophilic self-cleaning coating in the prior art. Further, since the hydrophilic self-cleaning glaze layer is directly calcined by the hydrophilic self-cleaning glaze, its bonding force with the antique brick is extremely high, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the limited bonding force between the hydrophilic self-cleaning coating and the brick surface of the antique brick in the prior art. The mutual coordination of the above multiple factors is conducive to realizing the long-lasting self-cleaning of the antique brick, and the self-cleaning is excellent. In addition, the technical solution does not need to additionally apply the hydrophilic self-cleaning coating on the surface of the antique brick, which is conducive to saving production costs and improving production efficiency.

[0047] It should be noted that the prior art generally adds potassium feldspar and / or sodium feldspar as fluxes in the frit used to achieve hydrophilic properties, and the melting point of potassium feldspar is about 1150°C and the melting point of sodium feldspar is about 1120°C. When potassium feldspar and / or sodium feldspar are added to the hydrophilic frit formula, the melting temperature difference between the first gradient fluxing system and the second gradient fluxing system will be greatly reduced, resulting in the inability of the formula system to achieve phase separation. At the same time, since potassium feldspar and sodium feldspar contain a large amount of aluminum oxide and silicon dioxide components, the high-temperature viscosity of the early melt will not drop significantly, further resulting in the inability of the formula system to achieve phase separation. In addition, the potassium oxide produced during the calcination of potassium feldspar and the sodium oxide produced during the calcination of sodium feldspar have a surface tension that is smaller than the surface tension of water, that is, when potassium feldspar and / or sodium feldspar are added to the formula, it is not conducive to the self-cleaning property of the hydrophilic self-cleaning glaze. Therefore, the hydrophilic frit containing potassium feldspar and / or sodium feldspar as flux cannot be added in the present technical solution.

[0048] Secondly, in order to ensure the fluxing effect and the expansion coefficient is compatible with the expansion coefficient of the body, potassium feldspar and sodium feldspar are usually added to the base glaze formula, and the chemical composition of the existing base glaze generally includes silicon dioxide, aluminum oxide, sodium oxide, calcium oxide, potassium oxide and zirconium oxide. When the hydrophilic frit, which is essentially a phase-separated melt, is added to the hydrophilic self-cleaning glaze formula, the hydrophilic self-cleaning glaze is calcined to form a hydrophilic self-cleaning glaze layer with calcium oxide, magnesium oxide, aluminum oxide and silicon dioxide as the phase-separated lower layer. That is, the chemical composition of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the chemical composition of the base glaze layer both contain silicon dioxide, aluminum oxide and calcium oxide with high surface tension (the surface tension of calcium oxide is 470×10 -3 N / M, the surface tension of silicon dioxide is 290×10 -3N / M, the surface tension of aluminum oxide is 380×10 -3 N / M), but the lower layer of the hydrophilic self-cleaning glaze layer also contains magnesium oxide, while the bottom glaze layer also contains sodium oxide, potassium oxide and zirconium oxide. Among them, the surface tension of magnesium oxide is 545×10 -3 N / M, the surface tension of sodium oxide is 150×10 -3 N / M, the surface tension of potassium oxide is 10×10 -3 N / M, the surface tension of zirconium oxide is 410×10 -3 N / M. Since the surface tension of the chemical components in the phase-separated lower layer of the hydrophilic self-cleaning glaze layer is relatively high, and the potassium oxide in the bottom glaze layer can easily greatly reduce the surface tension of the bottom glaze layer, resulting in the surface tension of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer being much greater than the surface tension of the bottom glaze layer. The surface tension difference between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the bottom glaze layer causes the hydrophilic self-cleaning glaze layer to easily shrink, and the hydrophilic self-cleaning glaze layer obtained after calcination is prone to shrinkage holes, and the bottom glaze layer is partially exposed, which not only easily affects the uniformity of self-cleaning properties, but also easily affects the appearance of the product.

[0049] In order to improve the uniformity of self-cleaning and ensure the appearance of the product, this technical solution adds fluorite to the hydrophilic self-cleaning glaze. Among them, the chemical composition of fluorite is mainly calcium fluoride, and the melting point of fluorite is about 1360°C, which is a high-temperature raw material. During the calcination process of the hydrophilic self-cleaning glaze, as the calcination temperature increases, the melt viscosity gradually decreases, and the fluorite will sink together with the raw materials in the hydrophilic melt that are far from reaching the melting point (such as the second gradient fluxing system and high-temperature raw materials), so that the hydrophilic self-cleaning glaze is calcined to form a hydrophilic self-cleaning glaze layer with boron oxide and lithium oxide components as the upper phase separation layer, and calcium fluoride, calcium oxide, magnesium oxide, aluminum oxide and silicon dioxide components as the lower phase separation layer. Among them, the surface tension of calcium fluoride is 22.3×10 -3 N / M, and the amount of fluorite whose main component is calcium fluoride added to the hydrophilic self-cleaning glaze is 5-10%, so that the content of calcium fluoride in the phase-separated lower layer of the hydrophilic self-cleaning glaze layer is relatively large, thereby greatly reducing the surface tension of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer, and making the surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the bottom glaze layer match, thereby avoiding the defect of glaze shrinkage phenomenon that the hydrophilic self-cleaning glaze is prone to appear during the calcination process when the surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the bottom glaze layer is extremely different, which is not only conducive to obtaining uniform self-cleaning properties, but also can ensure the appearance of the product.

[0050] It should be noted that after the hydrophilic self-cleaning glaze separates into phases during the calcination process, a large amount of liquid phase will appear in the upper and lower layers of the phase separation, and the composition difference between the upper and lower layers of the phase separation is also relatively large, which makes it easy for ion exchange to take place between the upper and lower layers of the phase separation and form an intermediate layer. The existence of the intermediate layer will shorten the difference in surface tension between the upper and lower layers of the phase separation, so that even if there is a large tension difference between the upper and lower layers of the phase separation, the glaze shrinkage phenomenon will not occur inside the hydrophilic self-cleaning glaze layer.

[0051] In addition, in order to ensure the effects of sealing and whitening, the existing base glaze contains more zirconium dioxide in its chemical composition, and the amount of fluxing components added in its chemical composition is less (the sum of the amount of fluxing components such as potassium oxide, sodium oxide and calcium oxide added is 8.7-10.3%), which greatly reduces the amount of liquid phase produced during the calcination process relative to the amount of liquid phase produced during the calcination process of the hydrophilic self-cleaning glaze, resulting in a greatly reduced ion exchange efficiency between the phase-separated lower layer of the hydrophilic self-cleaning glaze and the base glaze, and the intermediate layer formed between the phase-separated lower layer of the hydrophilic self-cleaning glaze and the base glaze is thinner, and its composition is closer to the phase-separated lower layer of the hydrophilic self-cleaning glaze, making it difficult to close the difference in surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze and the base glaze. Therefore, when the surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the base glaze layer is extremely different, it is easy to cause the hydrophilic self-cleaning glaze layer to easily shrink.

[0052] Since the decomposition temperature of calcium fluoride, the main component of fluorite, is between 1350 and 1470°C, and the maximum calcination temperature of the hydrophilic frit is 1530°C, when it is added to the hydrophilic frit, the calcium fluoride will be decomposed into calcium oxide, so that the calcium fluoride remaining in the lower layer of the phase separation becomes calcium oxide, and the surface tension of calcium oxide is large, so that the surface tension of the lower layer of the phase separation of the hydrophilic self-cleaning glaze layer cannot be reduced, and the glaze shrinkage defect cannot be solved. Therefore, in this technical solution, fluorite can only be added directly to the hydrophilic self-cleaning glaze, and it cannot be added to the hydrophilic frit and then indirectly added to the hydrophilic self-cleaning glaze through the hydrophilic frit.

[0053] Thirdly, the introduction of boric acid in the technical solution can not only effectively promote the phase separation of the hydrophilic self-cleaning glaze during the calcination process, but also help to inhibit the crystallization of the intermediate layer between the two phase-separated melts of the phase-separated upper layer and the phase-separated lower layer during the calcination of the hydrophilic self-cleaning glaze, thereby avoiding the liquid phase of the phase-separated upper layer being too low, resulting in the unstable self-cleaning performance of the hydrophilic self-cleaning glaze. In addition, the kaolin, quartz and alumina in the hydrophilic frit are not only conducive to improving the hardness, wear resistance and other properties of the hydrophilic frit, but the above three raw materials are all high-temperature raw materials, which are conducive to increasing the temperature difference between the upper raw materials and the lower raw materials in the hydrophilic frit, and promoting the glaze to be phase-separated in the early stage of firing.

[0054] Finally, according to the mass percentage calculation, the hydrophilic frit includes 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% talc, 10-20% kaolin, 13-22% quartz and 8-12% alumina, so that the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is 1:(3-8). When the ratio is greater than 1:3, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination will be too much, and the fluxing effect will be too strong, which will easily cause the fluorite that is difficult to melt in the early stage and the solid phase raw materials in the hydrophilic frit to melt in advance, resulting in difficulty in phase separation; when it is less than 1:8, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination will be too small, which will make it difficult for fluorite and the second gradient fluxing system and high-temperature raw materials in the hydrophilic frit to sink, resulting in difficulty in phase separation; on the other hand, it will cause the liquid phase in the upper layer of the phase separation to be too thin, affecting the surface tension of the glaze, and thus affecting its self-cleaning performance.

[0055] Preferably, the base glaze includes the following raw materials in parts by mass: 30-40 parts of potassium feldspar, 10-15 parts of sodium feldspar, 3-10 parts of washed kaolin, 10-30 parts of calcined kaolin, 5-15 parts of quartz, 5-15 parts of calcined alumina, 3-5 parts of talc, 2-6 parts of limestone and 5-15 parts of zirconium silicate. But it is not limited thereto.

[0056] Further description, in step C, the mesh size of the fluorite is 6000-8000 mesh.

[0057] In this scheme, fluorite with a mesh size of 6000-8000 is preferably added to the formula. Finer fluorite particles are conducive to a more uniform distribution of fluorite in the hydrophilic self-cleaning glaze, avoiding the phenomenon of devitrification caused by excessively large fluorite particles and excessive local concentration. At the same time, finer fluorite particles are also conducive to accelerating its melting, thereby promoting phase separation during the calcination process of the hydrophilic self-cleaning glaze and ensuring its performance.

[0058] Further description, in step C, calculated by mass percentage, the content of CaF2 in the fluorite is ≥90%.

[0059] The technical solution preferably uses fluorite with a CaF2 (calcium fluoride) content ≥ 90% as the formula raw material for the hydrophilic self-cleaning glaze, which is more conducive to reducing the surface tension of the lower phase-separated layer in the hydrophilic self-cleaning glaze layer, so that the surface tension of the lower phase-separated layer in the hydrophilic self-cleaning glaze layer is more matched with the surface tension of the base glaze layer, thereby improving the uniformity of self-cleaning and the appearance of the product.

[0060] It is further described that in step C, the ratio of the sum of the mass percentages of the boric acid and the lithium carbonate to the sum of the mass percentages of the wollastonite and the calcined talc is 1:(4-7).

[0061] In a preferred embodiment of the present technical solution, by optimizing the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc, it is beneficial to promote the phase separation of the hydrophilic self-cleaning glaze in the early stage of calcination, thereby ensuring the performance of the hydrophilic self-cleaning glaze.

[0062] Further, in step C, according to the mass percentage, the hydrophilic self-cleaning glaze is passed through a 325-mesh sieve, and the residue is 0.2-0.4%.

[0063] In a preferred embodiment of the present technical solution, by limiting the fineness of the hydrophilic self-cleaning glaze, the sieve residue of the hydrophilic self-cleaning glaze is relatively low, which is beneficial for making the hydrophilic self-cleaning glaze have fine uniformity, reducing the rough glaze surface caused by uneven particles, and improving the self-cleaning performance.

[0064] Further, in step C, the specific gravity of the hydrophilic self-cleaning glaze is 1.82-1.9.

[0065] When the specific gravity of the hydrophilic self-cleaning glaze is too high, the glaze will be too thick and the fluidity will be poor, which will make the application uniformity of the hydrophilic self-cleaning glaze poor and easily form defects such as glaze path. In addition, the specific gravity of the hydrophilic self-cleaning glaze is too high, which will easily hinder the discharge of gas and water generated during the calcination process of the hydrophilic self-cleaning glaze, causing the glaze layer obtained by calcining the hydrophilic self-cleaning glaze to crack easily.

[0066] When the specific gravity of the hydrophilic self-cleaning glaze is too low, the fluidity of the hydrophilic self-cleaning glaze is too good, and it is easy to flow during the glazing process, which also leads to poor uniformity of the hydrophilic self-cleaning glaze and easy formation of defects such as glaze paths. In addition, the specific gravity of the hydrophilic self-cleaning glaze is too low, resulting in excessive water in the glaze, which is prone to brick explosion during the calcination process.

[0067] It should be noted that glaze path means that the glaze layer is thicker in some areas and thinner or missing in other areas.

[0068] Further, in step C, the hydrophilic self-cleaning glaze comprises 80% hydrophilic frit, 10% black ball clay and 10% fluorite, calculated by mass percentage;

[0069] Calculated by mass percentage, the hydrophilic frit includes 3% boric acid, 8% lithium carbonate, 35% wollastonite, 12% calcined talc, 15% kaolin, 17% quartz and 10% alumina.

[0070] In a preferred embodiment of the present technical solution, by limiting the addition amount of each raw material in the hydrophilic frit and the hydrophilic self-cleaning glaze, it is beneficial to optimize the performance of the hydrophilic self-cleaning glaze.

[0071] Further, in step D, the glazing thickness of the hydrophilic self-cleaning glaze is 0.3-0.7 mm.

[0072] In a preferred embodiment of the present technical solution, by limiting the glazing thickness, it is beneficial to have a certain thickness of the melt mainly composed of boric acid and lithium carbonate in the early stage of calcination, so that the raw materials that have not yet reached the melting point have enough space to sink, thereby promoting phase separation and ensuring its performance.

[0073] Further, in step C, the preparation steps of the hydrophilic self-cleaning glaze are:

[0074] The raw materials of the hydrophilic frit are uniformly mixed according to the proportion, and the hydrophilic frit is obtained by water quenching after calcination;

[0075] After the raw materials of the hydrophilic self-cleaning glaze are uniformly mixed according to the proportion, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and the hydrophilic self-cleaning glaze is obtained by sieving.

[0076] The technical scheme also proposes a preparation method for a hydrophilic self-cleaning glaze, which is simple and easy to operate. Preferably, calculated by mass percentage, the amount of sodium carboxymethyl cellulose added is 0.2% of the amount of dry material added to the hydrophilic self-cleaning glaze, the amount of sodium tripolyphosphate added is 0.3% of the amount of dry material added to the hydrophilic self-cleaning glaze, and the amount of water added is 35-38% of the amount of dry material added to the hydrophilic self-cleaning glaze. After adding the above additives to the mixed material, ball milling is performed for 12 hours, and then sieving is performed to obtain the hydrophilic self-cleaning glaze.

[0077] A hydrophilic self-cleaning antique tile based on phase separation self-cleaning is prepared using the above-mentioned preparation method of hydrophilic self-cleaning antique tile based on phase separation self-cleaning. The hydrophilic self-cleaning antique tile has a static contact angle of 8-15° before being soaked in boiling water, and a static contact angle of 15-22° after being soaked in boiling water for 30 days.

[0078] A hydrophilic self-cleaning antique tile prepared by the above-mentioned preparation method of hydrophilic self-cleaning antique tile based on phase separation self-cleaning has a static contact angle of 8 to 15° before being soaked in boiling water and a static contact angle of 15 to 22° after being soaked in boiling water for 30 days, and has excellent, uniform and lasting self-cleaning performance.

[0079] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0080] Performance Test:

[0081] Appearance: Observe the glaze surface of the antique tile with the naked eye.

[0082] Static contact angle before immersion: According to the test method of "GB / T 30447-2013 Nanofilm Contact Angle Measurement Method", the static contact angle of the hydrophilic self-cleaning antique tile before immersion in boiling water is tested. If the static contact angle is <15°, it is qualified.

[0083] Static contact angle after immersion: According to the test method of "GB / T 30447-2013 Nanofilm Contact Angle Measurement Method", the hydrophilic self-cleaning antique tiles are tested for their static contact angle after being immersed in boiling water for 30 days. If the contact angle is less than 25°, it is qualified.

[0084] Anti-slip performance: Anti-slip performance is tested according to the DIN 51130:2014 anti-slip standard.

[0085] Mohs hardness: The Mohs hardness of the hydrophilic self-cleaning antique tile is tested using a Mohs hardness tester.

[0086] Example 1

[0087] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0088] B. Applying a base glaze on the surface of the body to form a base glaze layer; calculated by mass percentage, the chemical composition of the base glaze includes SiO259%, Al2O325%, Na2O33%, CaO0.6%, K2O6% and ZrO26.4%;

[0089] C. According to the mass percentage, 3% boric acid, 8% lithium carbonate, 35% wollastonite, 12% calcined talc, 15% kaolin, 17% quartz and 10% alumina are mixed evenly, calcined and water quenched to obtain a hydrophilic frit; according to the mass percentage, 80% hydrophilic frit, 10% black ball clay and 10% fluorite with a mesh number of 7000 mesh and a CaF2 content of 90% are mixed evenly, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and sieved to obtain a hydrophilic self-cleaning glaze with a specific gravity of 1.85 ; Wherein, according to the mass percentage, the hydrophilic self-cleaning glaze passes through a 325-mesh sieve, and the sieve residue is 0.2%; according to the mass percentage, the addition amount of sodium carboxymethyl cellulose is 0.2% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, the addition amount of sodium tripolyphosphate is 0.3% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, and the addition amount of water is 35% of the addition amount of the dry material of the hydrophilic self-cleaning glaze; the calcination curve of the hydrophilic frit is: from room temperature to 1530°C at a heating rate of 8-10°C / min, and then kept warm for 40 minutes;

[0090] D. applying a hydrophilic self-cleaning glaze to the surface of the bottom glaze layer to form a hydrophilic self-cleaning glaze layer; wherein the glazing thickness of the hydrophilic self-cleaning glaze is 0.5 mm;

[0091] E. After drying, calcining at a temperature of 1200-1220°C obtains hydrophilic self-cleaning antique tiles.

[0092] Example 2

[0093] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0094] B. Applying base glaze on the surface of the body to form a base glaze layer; calculated by mass percentage, the chemical composition of the base glaze includes SiO262%, Al2O323%, Na2O 2.5%, CaO 0.5%, K2O 6.5% and ZrO25.5%;

[0095] C. Calculated by mass percentage, 2% boric acid, 9% lithium carbonate, 30% wollastonite, 16% calcined talc, 20% kaolin, 15% quartz and 8% alumina are mixed evenly, calcined and water quenched to obtain a hydrophilic frit; Calculated by mass percentage, 90% hydrophilic frit, 5% black ball clay and 5% fluorite with a mesh size of 6000 mesh and a CaF2 content of 95% are mixed evenly, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and sieved to obtain a hydrophilic self-cleaning glaze with a specific gravity of 1.82; In the invention, according to the mass percentage, the hydrophilic self-cleaning glaze passes through a 325-mesh sieve, and the residue is 0.4%; according to the mass percentage, the addition amount of sodium carboxymethyl cellulose is 0.2% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, the addition amount of sodium tripolyphosphate is 0.3% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, and the addition amount of water is 36% of the addition amount of the dry material of the hydrophilic self-cleaning glaze; the calcination curve of the hydrophilic frit is: after heating from room temperature to 1530°C at a heating rate of 8-10°C / min, keep warm for 45 minutes;

[0096] D. applying a hydrophilic self-cleaning glaze to the surface of the bottom glaze layer to form a hydrophilic self-cleaning glaze layer; wherein the glazing thickness of the hydrophilic self-cleaning glaze is 0.3 mm;

[0097] E. After drying, calcining at a temperature of 1200-1220°C obtains hydrophilic self-cleaning antique tiles.

[0098] Example 3

[0099] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0100] B. Applying a base glaze on the surface of the body to form a base glaze layer; calculated by mass percentage, the chemical composition of the base glaze includes SiO2 60%, Al2O3 24%, Na2O 3.5%, CaO 0.3%, K2O 6.2% and ZrO 26%;

[0101] C. According to the percentage by mass, 4% boric acid, 5% lithium carbonate, 40% wollastonite, 9% talc, 17% kaolin, 13% quartz and 12% alumina are mixed evenly, and the mixture is calcined and then quenched with water to obtain a hydrophilic frit; according to the percentage by mass, 85% hydrophilic frit, 7% black ball clay and 8% fluorite with a mesh size of 8000 mesh and a CaF2 content of 90% are mixed evenly, and then sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and the mixture is sieved to obtain a hydrophilic self-cleaning glaze with a specific gravity of 1.9; In the invention, according to the mass percentage, the hydrophilic self-cleaning glaze passes through a 325-mesh sieve, and the residue is 0.3%; according to the mass percentage, the addition amount of sodium carboxymethyl cellulose is 0.2% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, the addition amount of sodium tripolyphosphate is 0.3% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, and the addition amount of water is 38% of the addition amount of the dry material of the hydrophilic self-cleaning glaze; the calcination curve of the hydrophilic frit is: after heating from room temperature to 1530°C at a heating rate of 8-10°C / min, keep warm for 40 minutes;

[0102] D. applying a hydrophilic self-cleaning glaze to the surface of the bottom glaze layer to form a hydrophilic self-cleaning glaze layer; wherein the glazing thickness of the hydrophilic self-cleaning glaze is 0.7 mm;

[0103] E. After drying, calcining at a temperature of 1200-1220°C obtains hydrophilic self-cleaning antique tiles.

[0104] Comparative Example 1

[0105] The hydrophilic self-cleaning antique brick in Comparative Example 1 includes an antique brick substrate and a hydrophilic self-cleaning coating distributed from bottom to top; wherein the hydrophilic self-cleaning coating is obtained by curing a super hydrophilic coating of model SM-TM-QS3500 / 3200 produced by Shangmeng Technology Wuxi Co., Ltd.

[0106] Comparative Example 2

[0107] Comparative Example 2 has the same preparation method and raw materials as Example 1, except that potassium feldspar and sodium feldspar are added to the hydrophilic frit formula in Comparative Example 2. That is, in Comparative Example 1, the hydrophilic frit includes 3% boric acid, 8% lithium carbonate, 5% potassium feldspar, 3% sodium feldspar, 30% wollastonite, 12% calcined talc, 12% kaolin, 17% quartz and 10% alumina, calculated by mass percentage.

[0108] Comparative Example 3

[0109] The preparation method and raw materials of Comparative Example 3 are the same as those of Example 1, except that in Comparative Example 3, calculated by mass ratio, the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is 1:2.

[0110] Comparative Example 4

[0111] The preparation method and raw materials of Comparative Example 4 are the same as those of Example 1, except that in Comparative Example 4, the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is 1:9.

[0112] Comparative Example 5

[0113] The preparation method and raw materials of Comparative Example 5 are the same as those of Example 1, except that fluorite is not added to the hydrophilic glaze formula in Comparative Example 5. That is, in Comparative Example 1, the hydrophilic self-cleaning glaze includes 90% of hydrophilic frit and 10% of black ball clay, calculated by mass percentage.

[0114] The performance tests were conducted on the hydrophilic self-cleaning antique tiles prepared by the preparation methods of Examples 1-3 and Comparative Examples 1-5, and the results are shown in Table 1 below:

[0115] Table 1 Performance test results of different hydrophilic self-cleaning antique tiles in the embodiments and comparative examples

[0116]

[0117] It can be seen from the performance test results in Table 1 that the antique brick glaze obtained by the technical solution has no shrinkage holes, the bottom glaze layer is not exposed, the static contact angle before being soaked in boiling water is 8-15°, and the static contact angle after being soaked in boiling water for 30 days is 15-22°. On the premise of ensuring the appearance, it not only has excellent, uniform and lasting self-cleaning performance, but also has good anti-slip properties and hardness, and is both decorative and practical, which is more conducive to meeting the use needs of consumers.

[0118] In Comparative Example 1, a hydrophilic self-cleaning coating is provided on the surface of the antique brick substrate to obtain a hydrophilic self-cleaning antique brick. Although the obtained antique brick has a small static contact angle with water before immersion and has good self-cleaning property, it is affected by the poor aging resistance of the hydrophilic self-cleaning coating and its limited bonding force with the brick surface. As a result, after immersion, the hydrophilic self-cleaning coating of the hydrophilic self-cleaning antique brick in Comparative Example 1 falls off, the self-cleaning durability is poor, and the static contact angle after immersion cannot be measured.

[0119] In Comparative Example 2, since potassium feldspar and sodium feldspar are added to the hydrophilic frit formula, not only does it make phase separation difficult, but the surface tension of the hydrophilic self-cleaning glaze layer obtained by calcining the hydrophilic self-cleaning glaze is reduced, the static contact angle of the antique tile is increased, and its self-cleaning property is reduced.

[0120] In Comparative Example 3, since the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is too large, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination is too large, and the fluxing effect is too strong, which easily melts the fluorite that is difficult to melt in the early stage and the solid phase raw materials in the hydrophilic melt, resulting in difficulty in phase separation, which increases the static contact angle of the antique tile and reduces its self-cleaning performance.

[0121] In Comparative Example 4, since the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is too small, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination is too small. On the one hand, it makes it difficult for fluorite and the second gradient fluxing system and high-temperature raw materials in the hydrophilic melt to sink, resulting in difficulty in phase separation; on the other hand, it makes the liquid phase in the upper layer of the phase separation too thin, affecting the surface tension of the glaze and thus affecting its self-cleaning performance.

[0122] In Comparative Example 5, since fluorite was not added, shrinkage holes appeared on the glaze surface and the bottom glaze layer was partially exposed, which not only affected the appearance of the product, but also resulted in poor self-cleaning properties at the exposed part of the bottom glaze layer, affecting the self-cleaning uniformity of the product.

[0123] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A method for preparing hydrophilic self-cleaning antique tiles based on phase separation self-cleaning, characterized in that: The following steps are involved: A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying; B. Applying base glaze on the surface of the body to form a base glaze layer; Calculated by mass percentage, the chemical composition of the base glaze includes SiO257-63%, Al2O3 23-25%, Na2O2.5-3.5%, CaO 0.2-0.8%, K2O 6-7% and ZrO2 5.5-6.5%; C. Prepare hydrophilic self-cleaning glaze; Calculated by mass percentage, the raw materials of the hydrophilic self-cleaning glaze are 80-90% hydrophilic frit, 5-10% black ball clay and 5-10% fluorite; Calculated by mass percentage, the raw materials of the hydrophilic frit are 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% calcined talc, 10-20% kaolin, 13-22% quartz and 8-12% alumina, and the calcination curve of the hydrophilic frit is: from room temperature to 1530°C at a heating rate of 8-10°C / min, and then kept warm for 35-45min; D. applying a hydrophilic self-cleaning glaze material to the surface of the base glaze layer to form a hydrophilic self-cleaning glaze layer; E. After drying, calcining at a temperature of 1200-1220°C obtains hydrophilic self-cleaning antique tiles.

2. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step C, the mesh size of the fluorite is 6000-8000 mesh.

3. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step C, calculated by mass percentage, the content of CaF2 in the fluorite is ≥90%.

4. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step C, the ratio of the sum of the mass percentages of the boric acid and the lithium carbonate to the sum of the mass percentages of the wollastonite and the calcined talc is 1:(4-7).

5. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step C, the hydrophilic self-cleaning glaze is passed through a 325-mesh sieve, and the residue is 0.2-0.4% by mass.

6. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step C, the specific gravity of the hydrophilic self-cleaning glaze is 1.82-1.

9.

7. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step C, the raw materials of the hydrophilic self-cleaning glaze are 80% hydrophilic frit, 10% black ball clay and 10% fluorite, calculated by mass percentage; Calculated by mass percentage, the raw materials of the hydrophilic frit are 3% boric acid, 8% lithium carbonate, 35% wollastonite, 12% calcined talc, 15% kaolin, 17% quartz and 10% alumina.

8. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step D, the glazing thickness of the hydrophilic self-cleaning glaze is 0.3-0.7 mm.

9. The method for preparing a hydrophilic self-cleaning antique tile based on phase separation self-cleaning according to claim 1, characterized in that: In step C, the preparation steps of the hydrophilic self-cleaning glaze are: The raw materials of the hydrophilic frit are uniformly mixed according to the proportion, and the hydrophilic frit is obtained by water quenching after calcination; After the raw materials of the hydrophilic self-cleaning glaze are uniformly mixed according to the proportion, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and the hydrophilic self-cleaning glaze is obtained by sieving.

10. A hydrophilic self-cleaning antique tile based on phase separation self-cleaning, characterized in that: The hydrophilic self-cleaning antique brick is prepared by the preparation method of the hydrophilic self-cleaning antique brick based on phase separation self-cleaning according to any one of claims 1 to 9. The static contact angle of the hydrophilic self-cleaning antique brick before being soaked in boiling water is 8 to 15°, and the static contact angle after being soaked in boiling water for 30 days is 15 to 22°.